A control method for preparing TiN coating based on reaction hysteresis curve

Through the fitting of the reaction gas flow-discharge voltage and parameter regulation, the deposition rate reduction caused by target poisoning in high-power pulse magnetron sputtering is solved, and the high-speed stable preparation of high-purity TiN coating is achieved, which improves coating layer performance and application prospects.

CN114107936BActive Publication Date: 2024-12-06NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202111448309.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-30
Publication Date
2024-12-06
Estimated Expiration
2041-11-30

AI Technical Summary

Technical Problem

In high-power pulse magnetron sputtering technology, the addition of reaction gas leads to target poisoning, resulting in nonlinear hysteresis characteristics of discharge voltage, reducing the deposition rate of the coating, and the deposition rate is lower than 20% of traditional DC magnetron sputtering -70%, it is difficult to achieve high-speed stable preparation of compound coatings.

Method used

Through the least squares regression fitting of the reaction gas flow-discharge voltage, the reaction hysteresis curve is drawn, the gas flow in the transition area is selected to control the deposition rate and stoichiometric ratio, and high-power pulse magnetron sputtering technology is used, and the power supply power is 1.3-1.6kW, pulse frequency is 300-600Hz, pulse duty cycle is 3%-6%, nitrogen flow is 4-5sccm, argon flow is 40-60sccm, substrate bias is -80--350V, deposition cavity The chamber air pressure is kept constant at 0.4-1Pa. A pure Ti transition layer is first deposited to achieve high-speed and stable preparation of TiN coating.

Benefits of technology

High-rate stable preparation of high-purity TiN coatings is achieved, with a deposition rate of 35-45nm/min, and the stability of the stoichiometric ratio is maintained at a lower nitrogen partial pressure, which improves the performance and application prospects of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114107936B_ABST
    Figure CN114107936B_ABST
Patent Text Reader

Abstract

The invention discloses a control method for preparing a TiN coating based on a reaction hysteresis curve, comprising adopting a high-power pulse magnetron sputtering technology, using a Ti metal single target as a metal target, and a N 2 As the reaction gas, the discharge voltage of the metal target is measured based on the reaction gas flow rate first increasing and then decreasing, and the least squares regression fitting of the reaction gas flow rate is completed. The horizontal axis is the reaction gas flow rate at the detection point, and the vertical axis is the discharge voltage at the detection point. The "reaction gas flow rate-discharge target voltage" reaction hysteresis curve is fitted; in the process of the reaction gas flow rate rising and falling, the area where the difference of the discharge voltage corresponding to the same gas flow rate reaches the voltage difference threshold is used as the transition area of ​​the reaction hysteresis curve. The reaction gas flow rate is selected in the transition area to realize the control of the stoichiometric ratio and preparation rate of the TiN coating deposited on the substrate surface. This method can simply and efficiently select the preparation parameters and stably prepare the TiN coating at a high rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of surface coating modification, and in particular relates to a control method for preparing a TiN coating based on a reaction hysteresis curve. Background Art

[0002] Nitride coatings have excellent properties such as high hardness, high chemical stability, corrosion resistance, and wear resistance. Transition metal elements with smaller electronegativity than nitrogen are usually selected to form transition metal nitrides. MM (metal-metal) interactions dominate transition metal nitrides, which are generally conductive, so they are also called conductive ceramics or metal nitrides. The main transition metal nitrides currently studied include IVB, VB, and VIB transition group element nitrides. Applied to the field of surface engineering protection technology, transition metal nitride coatings, as a protective coating, have broad application prospects in harsh service environments such as high chloride ion content, high temperature and humidity, gravel impact, and neutron irradiation.

[0003] Reactive magnetron sputtering technology is one of the important methods for preparing transition metal compound coating materials. Reactive sputtering refers to the inert gas ions (Ar + , Kr + ) is a technology that sputters the surface of a metal or alloy target, and the sputtered metal atoms react with the reaction gas to form compounds on the surface of the substrate. This technology can be used to prepare high-purity coatings with controllable stoichiometric ratios. In recent years, a high-power pulsed magnetron sputtering (HiPIMS) technology has been developed. As an emerging physical vapor deposition (PVD) technology, it can prepare high-density and excellent nitride coatings. Compared with traditional DC magnetron sputtering technology and cathode arc ion plating, it has unique advantages in coating preparation. It can achieve high ionization of sputtered metal materials and produce high-density deposited ion beams without defects such as macroscopic large particles. The dense plasma in front of the target has the dual functions of maintaining discharge and providing plasma assistance for coating growth, thereby affecting the microstructure of the growing coating. At the same time, high-power pulsed magnetron sputtering technology has good plating properties, so that the prepared coating has both high density and uniformity.

[0004] However, with the addition of reactive gas, the compound layer is generated not only on the substrate surface, but also on the grounded cavity inner wall and the metal target surface. The situation of compound generation on the metal target surface is often called "target poisoning". The degree of target poisoning depends on the competition between the target surface sputtering rate and the target surface compound generation rate, which causes nonlinear hysteresis characteristics of parameters such as discharge voltage or reactive gas partial pressure in the reactive sputtering process, which is called hysteresis effect. And because the chemical bond strength of the compound is usually much stronger than the metallic bond between metal atoms, when the target surface is poisoned, the sputtering yield will be greatly reduced, and the lower sputtering yield will lead to a lower deposition rate. In addition, high-power pulsed magnetron sputtering can produce more metal ions, and metal ion resorption effect is prone to occur under higher negative target voltage, resulting in a further reduction in deposition rate. Its deposition rate is generally 20%-70% of that of traditional DC magnetron sputtering.

[0005] Therefore, studying how to achieve high-rate and stable preparation of compound coatings is crucial for developing binary and multinary nitride coatings with stable component structures and excellent performance. This not only helps to deeply understand the basic physical process of reactive sputtering, guide equipment design and the construction of coating component structures, but also provides a theoretical basis and experimental foundation for the development of high-performance coatings under harsh working conditions, which has broad and far-reaching significance. Summary of the invention

[0006] The invention provides a control method for preparing a TiN coating based on a reaction hysteresis curve. The method can be used to simply and efficiently select preparation parameters and stably prepare the TiN coating at a high rate.

[0007] A control method for preparing a TiN coating based on a reaction hysteresis curve comprises:

[0008] High power pulse magnetron sputtering technology is used, with Ti metal single target as the metal target, N 2 As the reaction gas, the discharge voltage of the metal target is measured based on the reaction gas flow rate first increasing and then decreasing, and the least squares regression fitting of the reaction gas flow rate is completed. The horizontal axis is the reaction gas flow rate at the detection point, and the vertical axis is the discharge voltage at the detection point. The reaction hysteresis curve of the reaction gas flow rate-discharge target voltage is fitted;

[0009] During the process of increasing and decreasing the reaction gas flow rate, the area where the difference in discharge voltage corresponding to the same gas flow rate reaches the voltage difference threshold is used as the transition area of ​​the reaction hysteresis curve. The flow rate of the reaction gas is selected in the transition area to achieve the control of the stoichiometric ratio and preparation rate of the TiN coating deposited on the substrate surface.

[0010] Analyzing the reactive magnetron sputtering process, due to the introduction of reactive gas, a compound layer is generated on the target surface, which is called target poisoning. The degree of target poisoning depends on the competition between the sputtering rate and the reaction rate on the target surface. Therefore, when the reactive gas flow rate is continuously increased and then reduced, the inconsistent discharge voltage occurs due to the inconsistent poisoning state on the target surface, which makes it present a nonlinear hysteresis characteristic. According to the amount of reactive gas introduced, reactive sputtering is divided into three modes, namely, the initial curve overlap stage is called the metal mode, the intermediate curve non-overlap stage, that is, the area that meets the voltage difference threshold is called the transition mode, and the second curve overlap stage is called the compound mode. When the reactive gas flow rate is low, the target surface sputtering rate is approximately equal to the target surface compound generation rate, and there is no poisoning on the target surface, so the initial curve overlaps, which is called the metal mode. As the reaction gas flow rate increases, the rate of compound generation on the target surface also gradually increases. When it increases to a certain critical value, the state of the target surface undergoes a sudden change, that is, target poisoning begins to occur, which is manifested by a sudden increase in target voltage. In the subsequent process of gradually reducing the reaction gas, the target poisoning degree is different under the same reaction gas flow rate, and a certain hysteresis behavior occurs, which is manifested by the non-overlap of the two curves. This stage is called the transition mode. As the reaction gas flow rate further increases, the target surface becomes completely poisoned, and the target surface sputtering rate and the target surface compound generation rate reach a balance again, which is manifested by the overlap of the two curves again, which is called the compound mode.

[0011] The inventors have found through a large number of experimental explorations that when preparing TiN coatings by high-power pulsed magnetron sputtering, when the reaction gas flow rate is in the metal mode, the coating deposition rate is high, but a substoichiometric compound is obtained; while in the compound mode, although a stoichiometric compound can be obtained, the deposition rate is greatly reduced. Therefore, the present invention selects the gas flow rate in the transition zone to prepare the coating, so as to obtain a relatively high deposition rate and high-purity TiN coating.

[0012] The voltage difference threshold is 5-8V.

[0013] The reaction gas N is selected in the transition region 2 The inlet flow rate is 4-5sccm.

[0014] It also includes a sputtering gas, wherein the sputtering gas is an inert gas, and further, the sputtering gas is argon.

[0015] The inlet flow rate of the sputtering gas is 40-60 sccm, the substrate bias voltage is -80--350 V, and the gas pressure in the deposition chamber is kept constant at 0.4-1 Pa.

[0016] The parameters of the high-power pulse magnetron sputtering technology are: power supply power is 1.3-1.6KW, pulse frequency is 300-600Hz, and pulse duty ratio is 3%-6%.

[0017] The pure Ti transition layer is first deposited before the TiN coating is deposited on the substrate surface, and the specific steps are as follows:

[0018] A Ti coating is deposited on the surface of a substrate, wherein the substrate bias voltage is -80-120V, the sputtering gas flow rate is controlled at 40-60sccm, the deposition chamber pressure is kept constant at 0.4-0.6Pa, and the thickness of the Ti coating is 0.1-0.3μm.

[0019] The method of using high-power pulsed magnetron sputtering technology to control the stoichiometric ratio and preparation rate of depositing a TiN coating on a substrate surface includes:

[0020] The power supply power is kept constant at 1.3-1.6kW, the pulse frequency is 300-600Hz, the pulse duty cycle is 3%-6%, the substrate bias is -80--120V, the sputtering gas flow rate is controlled at 40-60sccm, the nitrogen flow rate is controlled at 4-5sccm, the deposition chamber pressure is kept constant at 0.4-0.6Pa, and the thickness of the TiN coating is 1.3-1.6μm.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] (1) The present invention selects a reasonable reaction gas flow rate by studying the reactive sputtering discharge voltage hysteresis curve, combines the regulation of sputtering power supply parameters, and utilizes reactive high-power magnetron sputtering technology to achieve high-rate and stable preparation of high-purity TiN coatings. The deposition rate of the TiN coating is 35-45nm / min.

[0023] (2) The present invention optimizes and controls the reaction gas flow rate to achieve stable and controllable preparation of a TiN coating that meets the stoichiometric ratio at a low nitrogen-argon ratio (nitrogen flow rate: 4-5 sccm, argon flow rate: 40-60 sccm), that is, at a relatively low nitrogen partial pressure. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 A discharge voltage reaction hysteresis curve diagram of a TiN coating prepared based on a HiPIMS reaction hysteresis curve provided in Example 1;

[0025] Figure 2 is a graph showing the variation of the element mole fraction of the TiN nitride coating obtained in Example 1 with the coating thickness;

[0026] Figure 3is a cross-sectional scanning electron morphology image of the TiN nitride coating prepared in Example 1;

[0027] Figure 4 is a cross-sectional scanning electron morphology image of the TiN nitride coating prepared in Comparative Example 1;

[0028] Figure 5 is a cross-sectional scanning electron morphology image of the TiN nitride coating prepared in Comparative Example 2;

[0029] Figure 6 The X-ray diffraction patterns of the TiN nitride coatings prepared in Example 3, Comparative Example 1 and Comparative Example 2 are shown. DETAILED DESCRIPTION

[0030] The embodiment of the present invention uses a Ti metal single-substance target as a sputtering target, and argon and nitrogen gases as a sputtering gas and a reaction gas, respectively. By reasonably regulating power supply parameters and working parameters, high-speed and stable preparation of a high-purity TiN coating by reactive high-power pulsed magnetron sputtering is achieved.

[0031] The technical solution of the present invention is further described in detail below in conjunction with the preferred embodiments and the accompanying drawings. This embodiment is implemented on the premise of the technical solution of the invention, and a detailed implementation method and specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments.

[0032] High-power pulsed magnetron sputtering technology is used, and its parameters are: power supply power is 1.3-1.6KW, pulse frequency is 300-600Hz, pulse duty cycle is 3%-6%, Ti metal single target is used as metal target, N 2 As the reaction gas, the discharge voltage of the metal target is measured based on the reaction gas flow rate first increasing and then decreasing, and the least squares regression fitting of the reaction gas flow rate is completed. The horizontal axis is the reaction gas flow rate at the detection point, and the vertical axis is the discharge voltage at the detection point. The reaction hysteresis curve of the reaction gas flow rate-discharge target voltage is fitted. Figure 1 It is the hysteresis curve of the discharge voltage reaction of high-power pulsed magnetron sputtering under the parameters of the technical solution of the present invention. It can be seen from the figure that the reaction gas N in the transition zone 2 The flow rate is 4-5 sccm, which satisfies the voltage difference threshold of 5-8V. Therefore, the reaction gas flow rate selected in the embodiment of the present invention is 4-5 sccm.

[0033] Embodiment 1:

[0034] In this embodiment, the base material is a 431 stainless steel disc with a diameter of 17 mm and a thickness of 3 mm. The surface of the base sample is polished with 400#-1200# sandpaper in sequence, and then mirror-polished with diamond grinding paste. Thereafter, it is ultrasonically cleaned in acetone and ethanol for 10 minutes each, and then dried with cold air for standby use.

[0035] The specific preparation steps of TiN coating are as follows:

[0036] Step 1: The pre-treated sample is attached to the sample holder with high temperature conductive adhesive and placed in the sputtering deposition equipment. The vacuum degree of the deposition chamber is less than 2×10 -3 Pa, introduce 50 sccm of high-purity argon gas, control the chamber pressure to be constant at 1 Pa, the pulse bias voltage to be -350 V, the pulse bias frequency to be 240 kHz, perform glow plasma etching on the substrate surface, and the etching time is 30 min.

[0037] Step 2: Use reactive high-power pulsed magnetron sputtering (HiPIMS) technology, keep the power constant at 1.3kW, the pulse frequency at 500Hz, and the pulse duty cycle at 5%. Pass 50sccm of high-purity argon gas to sputter and clean the metal target for 15 minutes. It should be noted that when cleaning the target, a baffle is placed in front of the target to prevent contaminants on the target surface from being sputtered and deposited onto the substrate. This step does not control the chamber pressure to sputter and clean the metal target surface to remove oxidized contaminants on the target surface. During cleaning, adjust the baffle to a few centimeters in front of the target to prevent sputtered particles from being deposited on the substrate. Subsequently, remove the baffle and deposit a transition layer on the substrate surface. The purpose of depositing the transition layer is to reduce the interface mismatch and enhance the film-base bonding strength.

[0038] Step 3: When depositing the Ti transition layer, a Ti metal single target is used as the sputtering target. The power supply parameters and working gas flow rate are consistent with those described in step 2. The difference from step 2 is that the substrate bias voltage is -100V, and the chamber pressure is controlled at 0.6Pa at this time.

[0039] Step 4: After the Ti transition layer is deposited for 10 minutes, a Ti metal target is used as a sputtering target, argon is used as a sputtering working gas, nitrogen is used as a reaction gas, the argon flow rate is maintained at 50 sccm, and the nitrogen flow valve is opened at the same time to prepare a TiN layer, and the flow rate is set to 4 sccm. During the entire sputtering deposition process, the sputtering power is kept constant at 1.3 kW, the chamber pressure is kept constant at 0.6 Pa, and the substrate bias is set to -100 V. The deposition time is 35 minutes, and the deposited coating thickness is ~1.55 μm.

[0040] Figure 2 This is a graph showing the variation of the molar fraction of elements with the coating thickness of the TiN nitride coating prepared in Example 1 of the present invention, obtained by characterization with a glow discharge emission spectrometer. It can be intuitively seen that the component elements of the TiN layer do not change significantly with the coating thickness, that is, with the deposition time, indicating that stable preparation can be achieved under the deposition conditions.

[0041] Figure 3This is a cross-sectional scanning electron morphology image of the TiN nitride coating prepared in Example 1 of the present invention. It can be seen from the image that the thickness of TiN is ˜1.55 μm.

[0042] Embodiment 2:

[0043] In this embodiment, the base material is a 431 stainless steel disc with a diameter of 17 mm and a thickness of 3 mm. The surface of the base sample is polished with 400# to 1200# sandpaper in sequence, and then mirror-polished with diamond grinding paste. Thereafter, it is ultrasonically cleaned in acetone and ethanol for 10 minutes each, and then dried with cold air for standby use.

[0044] The specific preparation steps of TiN coating are as follows:

[0045] Step 1: The pre-treated sample is attached to the sample holder with high temperature conductive adhesive and placed in the sputtering deposition equipment. The vacuum degree of the deposition chamber is less than 2×10 -3 Pa, 50 sccm of high-purity argon is introduced, argon is used as the sputtering working gas, the chamber pressure is controlled to be constant at 1 Pa, the pulse bias is -350 V, the pulse bias frequency is 240 kHz, and the substrate surface is subjected to glow plasma etching for 30 min.

[0046] Step 2: Reactive high power pulsed magnetron sputtering (HiPIMS) technology was used, with the power supply kept constant at 1.6 kW, the pulse frequency at 300 Hz, and the pulse duty cycle at 3%. 60 sccm of high purity argon was introduced to sputter clean the metal target for 15 min. It should be noted that a baffle was placed in front of the target to prevent contaminants on the target surface from being sputtered and deposited on the substrate when cleaning the target, and the chamber pressure was not controlled in this step.

[0047] Step 3: When the Ti transition layer is deposited, a Ti metal target is used as a sputtering target, and the power supply parameters and working gas flow rate are consistent with those described in step 2. The difference from step 2 is that the substrate bias voltage is set to -120V, and the chamber pressure is controlled at 0.5Pa.

[0048] Step 4: After the Ti transition layer is deposited for 10 minutes, a Ti metal target is used as a sputtering target, argon is used as a sputtering working gas, and nitrogen is used as a reaction gas to deposit and prepare a TiN coating. The argon flow rate is maintained at 60 sccm. At the same time, the nitrogen flow valve is opened to prepare a TiN layer. The flow rate is set to 4.5 sccm. During the entire sputtering deposition process, the sputtering power is kept constant at 1.6 kW, the chamber pressure is kept constant at 0.5 Pa, and the substrate bias is set to -120 V. The deposition time is 38 minutes, and the thickness of the deposited coating is 1.54 μm.

[0049] Embodiment 3:

[0050] In this embodiment, the base material is a 431 stainless steel disc with a diameter of 17 mm and a thickness of 3 mm. The surface of the base sample is polished with 400# to 1200# sandpaper in sequence, and then mirror-polished with diamond grinding paste. Thereafter, it is ultrasonically cleaned in acetone and ethanol for 10 minutes each, and then dried with cold air for standby use.

[0051] The specific preparation steps of TiN coating are as follows:

[0052] Step 1: The pre-treated sample is attached to the sample holder with high temperature conductive adhesive and placed in the sputtering deposition equipment. The vacuum degree of the deposition chamber is less than 2×10 -3 Pa, introduce 50 sccm of high-purity argon gas, control the chamber pressure to be constant at 1 Pa, the pulse bias voltage to be -350 V, the pulse bias frequency to be 240 kHz, perform glow plasma etching on the substrate surface, and the etching time is 30 min.

[0053] Step 2: Reactive high power pulsed magnetron sputtering (HiPIMS) technology was used, with the power supply kept constant at 1.5 kW, the pulse frequency at 600 Hz, and the pulse duty cycle at 6%. 40 sccm of high purity argon was introduced to sputter clean the metal target for 15 minutes. It should be noted that when cleaning the target, a baffle was placed in front of the target to prevent contaminants on the target surface from being sputtered and deposited on the substrate, and the chamber pressure was not controlled in this step.

[0054] Step 3: When depositing the Ti transition layer, a Ti metal target is used as the sputtering target. The power supply parameters and working gas flow rate are consistent with those described in step 2. The difference from step 1 is that the substrate bias voltage is set to -80V, and the chamber pressure is controlled at 0.4Pa.

[0055] Step 4: After the Ti transition layer is deposited for 10 minutes, a Ti metal target is used as a sputtering target, argon is used as a sputtering working gas, nitrogen is used as a reaction gas, the argon flow rate is maintained at 40 sccm, and the nitrogen flow valve is opened at the same time to prepare a TiN layer with a flow rate of 5 sccm. During the entire sputtering deposition process, the sputtering power is kept constant at 1.5 kW, the chamber pressure is kept constant at 0.4 Pa, and the substrate bias is set to -80 V. The deposition time is 40 minutes, and the deposited coating thickness is 1.50 μm.

[0056] Comparative Example 1:

[0057] This embodiment is a comparative embodiment with the above-mentioned embodiment 3.

[0058] In this comparative example, the substrate is exactly the same as that in Example 3, and the preparation method of the TiN coating on the substrate surface is basically the same as that in Example 3, except that the flow rate of the reaction gas nitrogen is controlled to 15 sccm in step 4. The deposition time of the TiN coating in this comparative example is kept consistent with the deposition time of the TiN coating in Example 3. Figure 4 , Figure 6 Comparative Example 1 is a cross-sectional scanning electron morphology image (coating thickness 0.39 μm) and an X-ray diffraction pattern of the TiN nitride coating obtained in the comparative example. Under the same deposition time, compared with Example 3, the comparative example can also obtain a high-purity TiN coating, but its deposition rate is greatly reduced, and its deposition rate is only 26% of that of Example 3.

[0059] Comparative Example 2:

[0060] This embodiment is another comparative embodiment with the above-mentioned embodiment 3.

[0061] In this embodiment, the substrate is exactly the same as that in Example 3, and the preparation method of the TiN coating on the surface of the substrate is basically the same as that in Example 3, except that the flow rate of the reaction gas nitrogen is adjusted to 2 sccm in step 4. The deposition time of the TiN coating in this comparative example is kept consistent with the deposition time of the TiN coating in Example 3. Figure 5 The cross-sectional scanning electron morphology image of the TiN nitride coating prepared in this comparative example (coating thickness ~1.58 μm). Figure 6 The X-ray diffraction pattern of Comparative Example 2 shows that the coating is mainly composed of TiN 0.3 The composition belongs to the substoichiometric ratio.

[0062] Figure 6 It is the X-ray diffraction spectrum of the TiN nitride coating prepared in Example 3, Comparative Example 1 and Comparative Example 2 of the present invention.

Claims

1. A control method for preparing a TiN coating based on a reaction hysteresis curve, characterized in that: include: High-power pulsed magnetron sputtering technology was used, with Ti metal single target as the metal target and N2 as the reaction gas. The discharge voltage of the metal target was measured based on the reaction gas flow rate first increasing and then decreasing. The least squares regression fitting of the reaction gas flow rate was completed. The horizontal axis was the reaction gas flow rate at the detection point, and the vertical axis was the discharge voltage at the detection point. The reaction hysteresis curve of the reaction gas flow rate-discharge target voltage was fitted. In the process of increasing and decreasing the reaction gas flow rate, the area where the difference of the discharge voltage corresponding to the same gas flow rate reaches the voltage difference threshold is used as the transition area of ​​the reaction hysteresis curve. The flow rate of the reaction gas is selected in the transition area, and the high-power pulsed magnetron sputtering technology is used to realize the control of the stoichiometric ratio and preparation rate of the TiN coating deposited on the substrate surface; the flow rate of the reaction gas N2 selected in the transition area is 4-5sccm; The method of using high-power pulsed magnetron sputtering technology to control the stoichiometric ratio and preparation rate of depositing a TiN coating on a substrate surface includes: The power supply power is kept constant at 1.3-1.6kW, the pulse frequency is 300-600Hz, the pulse duty cycle is 3%-6%, the substrate bias is -80--120V, the sputtering gas flow rate is controlled at 40-60sccm, the nitrogen flow rate is controlled at 4-5sccm, the deposition chamber pressure is kept constant at 0.4-0.6Pa, and the thickness of the TiN coating is 1.3-1.6μm.

2. The control method for preparing a TiN coating based on a reaction hysteresis curve according to claim 1, characterized in that: The voltage difference threshold is 5-8V.

3. The control method for preparing a TiN coating based on a reaction hysteresis curve according to claim 1, characterized in that: It also includes a sputtering gas, and the sputtering gas is an inert gas.

4. The control method for preparing a TiN coating based on a reaction hysteresis curve according to claim 1, characterized in that: The pure Ti transition layer is first deposited before the TiN coating is deposited on the substrate surface, and the specific steps are as follows: A Ti coating is deposited on the surface of a substrate, wherein the substrate bias voltage is -80-120V, the sputtering gas flow rate is controlled at 40-60sccm, the deposition chamber pressure is kept constant at 0.4-0.6Pa, and the thickness of the Ti coating is 0.1-0.3μm.

Citation Information

Patent Citations

  • TiAlSiN coating layer preparation method based on reactive sputtering hysteresis effect