Aluminum alloy processing technology

By optimizing the composition and parameters of the electrochemical polishing solution, the problems of high energy consumption and poor polishing effect caused by the large resistance of the electrolytic polishing mucosal are solved, and the surface treatment of aluminum alloy with low roughness and high mirror effect is achieved, reducing energy consumption and improving Polishing efficiency.

CN114108065BActive Publication Date: 2024-12-03SICHUAN XINHEXIN ALUMINUM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111650133.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-30
Publication Date
2024-12-03
Estimated Expiration
2041-12-30

AI Technical Summary

Technical Problem

In the existing electrochemical polishing technology, the resistance of the electrolytic polishing mucosa is too large, resulting in an increase in the voltage-current density CD period, difficulty in gas release, high energy consumption, and poor polishing effect.

Method used

Using an aluminum alloy processing technology, including surface pretreatment, electrochemical polishing and post-treatment, using perchloric acid, maleic acid, jordine, sulfosalicylic acid, butyl glycol, triethanolamine and styrene trinitronitrogen Electrochemical polishing solution of azoles and other components optimizes the voltage and current density through curve fitting, reduces the mucosal resistivity of the anode dissolution process, improves the diffusion speed of metal ions, reduces energy consumption, and improves polishing efficiency.

Benefits of technology

It effectively reduces the mucosal resistivity of the anode dissolution process, improves the low roughness and high mirror effect of the aluminum alloy surface, saves energy consumption, improves the polishing efficiency, avoids the smooth section during the polishing process, and significantly improves the polishing effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114108065B_ABST
    Figure CN114108065B_ABST
Patent Text Reader

Abstract

The present invention provides an aluminum alloy processing technology, which includes surface pretreatment-electrochemical polishing-surface post-treatment. The aluminum alloy is configured with an electrochemical polishing solution in the processing solution, so that the resistivity of the mucous film formed in the anodic dissolution process can be effectively reduced, the diffusion rate of the dissolved metal can be increased, and the surface roughness of the aluminum alloy is low and the mirror effect is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an aluminum alloy processing technology, in particular to an aluminum alloy electrochemical polishing technology. Background Art

[0002] Electrochemical polishing is a common titanium surface treatment technology that has been developed and matured after mechanical polishing and chemical polishing. This technology can not only significantly reduce the microscopic roughness of the surface of titanium and titanium alloy materials and improve their surface brightness, but also has no cutting force, heat and burrs during the polishing process, and will not produce residual strain layer and phase change layer.

[0003] The basic polishing principle of electrochemical polishing is that after a certain polishing voltage and current density are passed through the electrochemical polishing system, a sticky film with high resistivity will be produced on the surface of the anode workpiece. The thickness of the film at different locations on the workpiece surface is not the same: the film layer is thinner at the microscopic convex parts of the surface, the resistance is smaller and the current density is larger, and the dissolution rate of the anode workpiece is faster; on the contrary, the film distribution is thicker at the microscopic concave parts of the surface, the resistance is larger, and the dissolution rate of the anode workpiece is lower than that of the convex parts of the surface. It is precisely because of the inconsistency in the thickness of this sticky film and the current density that the dissolution rate of the microscopic convex parts of the workpiece surface is greater than that of the concave parts, and as the working time increases, the roughness of the metal surface decreases and the brightness increases, and polishing is achieved.

[0004] In the process of polishing, the combined effect of many factors has a certain effect on the polishing effect.

[0005] Due to the different material properties of metal workpieces, electropolishing fluid formula and process parameters, there may be some problems on the surface of metal workpieces.

[0006] Describe the process of one or more chemical reactions:

[0007] (1) The anode metal dissolves under the combined effect of electrical parameters and polishing liquid Me=Me 2+ +2e - ;

[0008] (2) Passivation film Me+2OH is formed on the surface of the anode metal - =MeO+H2O+2e - ;

[0009] (3) Evolution of gaseous oxygen 4OH - =O2+2H2O+4e - ;

[0010] (4) Oxidation of the active ingredients of electrochemical polishing fluid on the surface of metal workpieces

[0011] Therefore, the surface quality of the metal workpiece after electrochemical polishing is determined by the coordinated progress of these four reaction processes.

[0012] Usually, the conventional theoretical anode current-potential curve can be found in "Aluminum Alloy Anodizing and Surface Treatment Technology Second Edition" edited by Zhu Zufang, page 51. The usual electrochemical polishing process is divided into AB section, BC section, CD section, and DE section.

[0013] In the AB segment, the anode current density increases rapidly with the increase of potential. At this time, the anode metal surface is in an active dissolution state, and the metal cations diffuse into the polishing liquid to form hydrated ions, which basically conforms to the Tafel law, that is, Me=Me 2+ +2e - .

[0014] In this stage: the current is concentrated at the micro-convex part of the anode metal surface, the current density is relatively large, the micro-convex part dissolves first, the metal atoms on the surface of the anode workpiece lose electrons to generate metal cations, the speed of their diffusion into the polishing liquid is slightly faster than the speed of the substrate dissolution, and the viscous film is not completely formed. In this process, because the viscous film is not completely formed, the electrochemical polishing is only in the active dissolution stage of the anode metal substrate surface, and there is no polishing effect.

[0015] In the BC section, the anode potential increases significantly, but the anode current density decreases with the increase of the anode potential. This is because a large number of hydrated ions are generated in the AB stage and gather near the anode surface. The speed of their diffusion into the electrochemical polishing solution is slower than the speed of metal dissolution on the anode substrate surface, forming anode concentration polarization. In addition, oxides are generated on the substrate surface, and their resistance is large, which is another reason for the decrease in current density in this stage. That is, the main occurrence of Me+2OH - =MeO+H2O+2e - .

[0016] In the BC section, the anode substrate continues to dissolve, but the current density is not high enough and is unstable, the anode oxygen evolution reaction is difficult and the mucous film is still in the formation stage, and there is no polishing effect.

[0017] In the CD section, the anode current density is basically stable, which theoretically belongs to a good electrochemical polishing stage and a current density stable zone. In this process, almost all the oxides on the anode surface are generated, and the dissolution of the metal substrate, the generation and destruction of the oxide film are in a dynamic equilibrium state to maintain a relatively stable current density. In this stage, the metal surface gradually becomes flat, and the difference between the micro-concave and micro-convex parts is not large, showing a certain metallic luster. However, due to the weak oxygen evolution phenomenon, a small amount of oxygen bubbles will adhere to the surface of the substrate, and the bubbles will prevent the smooth progress of electrochemical polishing. Therefore, there are often small spots and other defects on the anode surface. Although there is a certain metallic luster, the brightness is not high.

[0018] In the DE stage, the voltage continues to increase and has reached the oxygen evolution potential. The anode current density increases rapidly with the increase of the anode potential, mainly used for the evolution of oxygen. At this time, a large number of bubbles are generated on the surface of the anode workpiece, but the oxygen still adheres to the surface of the workpiece due to insufficient pressure, preventing the smooth progress of electrochemical polishing. Therefore, there are often large spots and other defects on the anode surface.

[0019] It can be clearly seen that when the voltage is in the CDE segment, a polishing effect is achieved and oxygen is released in the DE segment, which can improve the polishing effect. Therefore, the prior art usually performs electrochemical polishing at a voltage after point D. However, the following technical problems still exist: the resistance of the electrolytic polishing film is too large, the time of the voltage-current density CD segment is increased, gas release is difficult, energy consumption is high, and the polishing effect is poor. Summary of the invention

[0020] Based on the technical problems existing in the above-mentioned electrolytic polishing process: the present invention provides an electrochemical polishing solution for aluminum alloy processing, which can effectively improve the electrochemical polishing efficiency, and there is almost no anode current density plateau during the electrolytic polishing process. Through curve fitting, the optimal electrochemical polishing voltage can be effectively obtained, and the diffusion rate of metal ions can be increased during the polishing process, thereby effectively obtaining aluminum alloy materials with low roughness and high mirror effect.

[0021] An aluminum alloy processing process comprises the following steps:

[0022] (1) Surface pretreatment: cleaning - mechanical grinding - degreasing - cleaning - drying;

[0023] (2) Electrochemical polishing: Prepare the processing solution and place it in the electrochemical polishing tank. Use the surface pretreated aluminum alloy as the anode and the stainless steel as the cathode. Connect them to a DC power supply. The electrolysis temperature is 27°C, the voltage is less than 81V, and the current density is less than 1.9A. . cm -2 , electrode spacing 17mm;

[0024] (3) Surface post-treatment,

[0025] For aluminum alloy in the processing solution, the fitting function relationship between voltage and current density is as follows:

[0026] A1= 0.0105V1 + 0.0082, 0<V1<46;

[0027] A2 = 0.09e 0.0369V2 , 46<V2<81.

[0028] Furthermore, the polishing voltage is preferably 46±0.3V, and the polishing time is preferably 120s.

[0029] Furthermore, the cleaning is deionized cleaning, and the mechanical grinding is performed by mechanical grinding with 400# and 800# water sandpaper on a pre-grinding machine to remove the oxide layer.

[0030] Furthermore, the degreasing agent is composed of an aqueous solution of 15 g / L sodium silicate, 10 g / L sodium hydroxide and 20 g / L sodium phosphate, and the degreasing temperature is 55 o C, the degreasing method is stirring and immersing for 3 minutes; the drying is carried out at 30°C with nitrogen purge drying.

[0031] Furthermore, the processing solution includes a composite acid, a corrosion inhibitor, a brightener, a viscosity regulator, and an additive, wherein the composite acid is a mixture of perchloric acid, maleic acid, and oxalic acid, the corrosion inhibitor is rhodamine, the brightener is sulfosalicylic acid, the viscosity regulator is butylene glycol, the additives are triethanolamine and benzotriazole, and the solvent is ethanol and water.

[0032] Furthermore, the ratio of each component of the processing solution is:

[0033] The volume ratio of perchloric acid, maleic acid and oxalic acid is 1:11:4, 135ml / L

[0034] Said rhodamine: 3g / L;

[0035] Sulfosalicylic acid: 2 g / L;

[0036] Butanediol: 190 ml / L;

[0037] The triethanolamine: 1 g / L;

[0038] The benzotriazole: 1 g / L;

[0039] The ethanol: 570 ml / L;

[0040] The balance is deionized water.

[0041] Furthermore, the post-treatment is: cleaning-drying-coating a resin protective layer, wherein the resin protective layer is a UV protective resin such as unsaturated polyester, epoxy acrylate, polyurethane acrylate, or polyether acrylate, and the thickness of the resin is less than 1 mm.

[0042] Furthermore, the post-treatment is: anodizing treatment-sealing treatment, and the thickness of the oxide film layer obtained by the anodizing and sealing treatment is less than 10 μm.

[0043] Furthermore, the sealing treatment is steam sealing, and the water vapor temperature is 105°C.

[0044] Pretreatment: washing - mechanical grinding - degreasing - cleaning - drying. There are oxide scale, rust, welding slag, oil, water, dust and old weak coating on the metal surface, which will affect the contact effect between the electrochemical polishing liquid and the metal substrate surface, and then affect the polishing voltage and current density. The purpose of surface pretreatment is to remove these pollutants and improve the polishing effect.

[0045] Electrochemical polishing: Generally speaking, the electrochemical polishing solution mainly includes oxidizing acid and regulator, among which the oxidizing acid mainly participates in the dissolution of the anode workpiece, forms soluble salts with the main elements of the polished metal sample, and produces an oxide film on the surface of the polished sample. Secondly, the regulator component is an indispensable component of the electrochemical polishing solution, but it does not directly participate in the electrochemical reaction and is used to adjust the polishing effect, such as the brightener to adjust the brightness of the polishing.

[0046] The oxidizing acid of the invention is a composite acid, which is a mixture of perchloric acid, maleic acid and oxalic acid; the regulator is a corrosion inhibitor, a viscosity regulator, an additive and a solution.

[0047] Perchloric acid is a strong oxidant and is the main component of electrolytic polishing. It is easy to obtain better polishing effects and is a common component.

[0048] Maleic acid and oxalic acid are mainly used to dissolve soluble salts generated during the electrochemical polishing process. Both are diacidic acid dissolving agents, which can effectively complex the metal ions dissolved from the anode, increase the diffusion rate of metal ions, reduce the viscosity of the solution, and thus reduce the mucosal resistance of the solution on the anode surface, effectively improving the polishing effect. In addition, the carboxyl groups on maleic acid and oxalic acid not only have the effect of complexing dissolved metals, but also have the effect of corrosion inhibitors.

[0049] Corrosion inhibitor: Rhodin is a mixture, mainly including di-o-toluene thiourea, starch, salt and Pingpingjia. Specifically, the main active ingredient is di-o-toluene thiourea, which is used in an amount of 26%; the amount of starch is 17wt.% as a brightener, the amount of salt is 52%, which is used to improve the conductivity and current efficiency, and the amount of Pingpingjia is 5%, which is a surfactant and can improve the release rate of oxygen gas in the polishing liquid. Rhodin is a commercial ingredient, which is relatively stable and easy to purchase, reducing the difficulty of configuring the electrochemical polishing solution.

[0050] Brightener: Sulfosalicylic acid, mainly used to improve the brightness of the workpiece and reduce the surface roughness value.

[0051] Viscosity regulator: Butanediol contains multiple hydroxyl groups and has a high viscosity. It can play a role in viscosity regulation and improve polishing quality. During the electrochemical polishing process, butanediol will produce an adsorption effect at the anode to form an adsorption film attached to the surface of the workpiece to assist in electrochemical polishing. Due to the uneven surface of the workpiece, the adsorption film is distributed differently on the surface, so that the current is concentrated at the micro-convex parts of the workpiece surface, and the current density is relatively large. The dissolution rate of the metal substrate at the micro-convex parts is greater than that of the metal substrate at the micro-concave parts. As the electrochemical reaction continues, the micro-convex parts continue to dissolve, and the microscopic surface of the specimen gradually becomes flat and bright.

[0052] Ethanol: The hydroxyl group -OH contained in it adjusts the pH value of the polishing liquid and can act as a corrosion inhibitor, thereby improving the polishing quality.

[0053] Triethanolamine and benzotriazole are auxiliary complexing agents, which are mainly used to improve the complexing effect of maleic acid, oxalic acid and anodic oxidation dissolved metals, and effectively increase the diffusion rate of metal ions in the polishing liquid.

[0054] Electrochemical polishing parameters:

[0055] (1) Temperature: During the polishing process, the temperature directly affects the viscosity of the electrochemical polishing solution. The viscosity of the solution at a low temperature is large, the dispersion ability of the solution is small, and the dissolution of the anode workpiece is too slow. Within a certain temperature range, the higher the polishing temperature, the smaller the solution viscosity, the faster the movement speed of the reactants and products, and the dissolution speed of the anode metal workpiece will also be correspondingly accelerated, and a better electrochemical polishing effect can be obtained at this time. However, when the temperature of the electrochemical polishing solution is too high, the activity of the perchlorate ion is greatly enhanced, which will cause excessive corrosion and even burning of the metal to be polished. The temperature used in the present invention is 27 o C, effectively balances the electropolishing effect while taking into account viscosity.

[0056] (2) Electrode spacing: When the electrode spacing is too small, the energy consumption is small, but it is not conducive to the diffusion of ions in the solution, and it is easy to cause the solution temperature in the polishing area to rise suddenly, seriously affecting the electrochemical polishing effect; when the spacing is too large, the required voltage increases, and the energy consumption also increases accordingly.

[0057] (3) As mentioned above, if the voltage is too low, the metal will not be electropolished, but only the aluminum will be anodized. If the voltage is too low, the gas will be released very quickly during the electropolishing process, and the current density will increase, causing the temperature of the surrounding solution to rise. The strong oxidizing property of perchloric acid will increase rapidly with the increase in temperature, resulting in corrosion or even burning.

[0058] (4) The polishing time of the present invention is 120 seconds. If the polishing time is less than 120 seconds, the sticky film is not completely removed, resulting in the inability to carry out the polishing process. When the time exceeds 120 seconds, the oxidation corrosion on the surface of the sample is aggravated and even pits appear, which seriously affects the surface quality and reduces the polishing effect.

[0059] By effectively matching the components of the electrolytic polishing solution and adjusting the electrolytic parameters, the stable stage of the electrochemical polishing process can be effectively avoided and the energy consumption can be effectively reduced. The applied voltage is divided into two stages, V1 and V2, by linear fitting of voltage and current density. In the 0~V1 stage, the voltage and current density are linearly related, and the function is: A1=0.0105V1 + 0.0082, 0<V1<46. In the latter part of this function, partial polishing will occur, but there will be no gas release. In the V1-V2 section, oxygen will be released, and the function of this section is A2 = 0.09e 0.0369V2 , 46<V2<81, as shown in the attached Figure 1 , attached Figure 2 , and attached Figure 3 As shown, when the electrochemical polishing DC voltage is 46±0.3V, the polishing effect is most suitable. While effectively polishing the substrate, no burning or uneven polishing will occur to the substrate.

[0060] Post-processing: The main purpose of post-processing is to form a protective film to protect the metal substrate, or to provide a flat surface for other subsequent treatments. Specifically, if the polished mirror effect of aluminum is required, it is only necessary to coat a simple protective resin on its surface. The resin can be a UV resin or other photosensitive resin. The resin protective layer is a UV protective resin such as unsaturated polyester or epoxy acrylate or polyurethane acrylate or polyether acrylate. The thickness of the resin is less than 1mm. When it is needed, it can be directly peeled off manually, or a paint stripper can be used to automatically peel it off within seconds to obtain a complete mirror aluminum alloy material.

[0061] If the low-roughness aluminum alloy mirror substrate is used for other treatments, the treatments are usually to obtain the desired product and to improve the bonding strength between the passivation layer and the substrate, such as anodizing to obtain a regular anodized channel array, or dyeing treatment, or phosphating treatment. The low-roughness aluminum alloy mirror substrate can be used as a post-treatment substrate, and there are no other clear restrictions on post-treatment.

[0062] Beneficial technical effects:

[0063] (1) The present invention can effectively reduce the resistivity of the mucous membrane formed during the anodic dissolution process and increase the diffusion rate of the dissolved metal by configuring an electrolytic polishing liquid containing perchloric acid, maleic acid and oxalic acid, rhodamine, sulfosalicylic acid, butylene glycol, triethanolamine, benzotriazole, ethanol and water, that is, effectively avoid the CD segment during the electrolytic polishing process, thereby reducing the voltage requirement for polishing, and effectively improving the polishing efficiency while reducing energy consumption while evolving oxygen at a low pressure.

[0064] (2) The surface roughness of the obtained aluminum alloy is low and the mirror effect is good. BRIEF DESCRIPTION OF THE DRAWINGS

[0065] Attached Figure 1 The voltage-current density curve of Example 1 of the present invention.

[0066] Attached Figure 2 4 is a voltage-current density curve in the voltage range of 0<V1<46 in Example 1 of the present invention.

[0067] Attached Figure 3 This is a voltage-current density curve diagram for a voltage range of 46<V2<81 in Example 1 of the present invention.

[0068] Attached Figure 4 This is the SEM image of the polished aluminum alloy in Example 1 of the present invention.

[0069] Attached Figure 5 This is a SEM image of the aluminum alloy of the present invention.

[0070] Attached Figure 6 This is the SEM image of the polished aluminum alloy of Comparative Example 1 of the present invention.

[0071] Attached Figure 7 This is the SEM image of the polished aluminum alloy of Comparative Example 2 of the present invention.

[0072] Attached Figure 8 This is the SEM image of the polished aluminum alloy of Comparative Example 3 of the present invention.

[0073] Attached Fig. 9 This is the SEM image of the polished aluminum alloy of Comparative Example 4 of the present invention. DETAILED DESCRIPTION

[0074] The treatment methods of all aluminum alloys of the present invention include electrochemical polishing pre-treatment, electrochemical polishing treatment and electrochemical polishing post-treatment, wherein the configuration of the electrochemical polishing solution is:

[0075] (1) adding water to a reaction vessel, and sequentially adding oxalic acid, perchloric acid and maleic acid thereto;

[0076] (2) adding part of ethanol, rhodamine, sulfosalicylic acid, triethanolamine and benzotriazole to the mixed solution in step (1) in sequence, and mixing by magnetic stirring;

[0077] (3) The remaining amount of ethanol is supplemented, and butylene glycol is added thereto, and the mixture is mixed evenly by magnetic stirring to obtain an aluminum alloy processing solution for electrolytic polishing.

[0078] For the comparative example, if one of the components is reduced, ethanol is used to make up for it.

[0079] The pre-treatment: surface pre-treatment: cleaning - mechanical grinding - degreasing - cleaning - drying;

[0080] The cleaning is deionized cleaning, and the mechanical grinding is: 400#, 800# water sandpaper is used for mechanical grinding on a pre-grinding machine to remove the oxide layer.

[0081] The degreasing agent is composed of an aqueous solution of 15 g / L sodium silicate, 10 g / L sodium hydroxide and 20 g / L sodium phosphate, and the degreasing temperature is 55 o C. The degreasing method is stirring and soaking for 3 minutes.

[0082] The drying is carried out at 30°C with nitrogen purge.

[0083] Post-treatment only includes cleaning and drying, without coating, anodizing and sealing.

[0084] Example 1

[0085] An aluminum alloy processing solution, the composition of the solution is as follows:

[0086] The volume ratio of perchloric acid, maleic acid and oxalic acid is 1:11:4, 135ml / L;

[0087] Rutin: 3g / L;

[0088] Sulfosalicylic acid: 2 g / L;

[0089] Butanediol: 190ml / L;

[0090] Triethanolamine: 1 g / L;

[0091] Benzotriazole: 1 g / L;

[0092] Ethanol: 570 ml / L;

[0093] The balance is deionized water.

[0094] The aluminum alloy workpiece was used as the anode connected to the positive electrode of the DC power supply, and the stainless steel was used as the cathode connected to the negative electrode of the DC power supply. The electrolysis temperature was 27 °C, the electrode spacing was 17 mm, the electrochemical polishing DC voltage was 46 V, and the polishing time was 120 s.

[0095] Comparative Example 1

[0096] An aluminum alloy processing solution, the composition of the solution is as follows:

[0097] The volume ratio of perchloric acid, maleic acid and oxalic acid is 1,8.43ml / L;

[0098] Rutin: 3g / L;

[0099] Sulfosalicylic acid: 2 g / L;

[0100] Butanediol: 190ml / L;

[0101] Triethanolamine: 1 g / L;

[0102] Benzotriazole: 1 g / L;

[0103] Ethanol: 570+126.56 ml / L;

[0104] The balance is deionized water.

[0105] The aluminum alloy workpiece was used as the anode connected to the positive electrode of the DC power supply, and the stainless steel was used as the cathode connected to the negative electrode of the DC power supply. The electrolysis temperature was 27 °C, the electrode spacing was 17 mm, the electrochemical polishing DC voltage was 46 V, and the polishing time was 120 s.

[0106] Comparative Example 2

[0107] An aluminum alloy processing solution, the composition of the solution is as follows:

[0108] The volume ratio of perchloric acid, maleic acid and oxalic acid is 1:11:4, 135ml / L;

[0109] Sulfosalicylic acid: 2 g / L;

[0110] Butanediol: 190ml / L;

[0111] Triethanolamine: 1 g / L;

[0112] Benzotriazole: 1 g / L;

[0113] Ethanol: 570 ml / L+3g;

[0114] The balance is deionized water.

[0115] The aluminum alloy workpiece was used as the anode connected to the positive electrode of the DC power supply, and the stainless steel was used as the cathode connected to the negative electrode of the DC power supply. The electrolysis temperature was 27 °C, the electrode spacing was 17 mm, the electrochemical polishing DC voltage was 46 V, and the polishing time was 120 s.

[0116] Comparative Example 3

[0117] An aluminum alloy processing solution, the composition of the solution is as follows:

[0118] The volume ratio of perchloric acid, maleic acid and oxalic acid is 1:11:4, 135ml / L;

[0119] Rutin: 3g / L;

[0120] Butanediol: 190ml / L;

[0121] Triethanolamine: 1 g / L;

[0122] Benzotriazole: 1 g / L;

[0123] Ethanol: 570 ml / L+2g;

[0124] The balance is deionized water.

[0125] The aluminum alloy workpiece was used as the anode connected to the positive electrode of the DC power supply, and the stainless steel was used as the cathode connected to the negative electrode of the DC power supply. The electrolysis temperature was 27 °C, the electrode spacing was 17 mm, the electrochemical polishing DC voltage was 46 V, and the polishing time was 120 s.

[0126] Comparative Example 4

[0127] An aluminum alloy processing solution, the composition of the solution is as follows:

[0128] The volume ratio of perchloric acid, maleic acid and oxalic acid is 1:11:4, 135ml / L;

[0129] Rutin: 3g / L;

[0130] Sulfosalicylic acid: 2 g / L;

[0131] Butanediol: 190ml / L;

[0132] Triethanolamine: 1 g / L;

[0133] Benzotriazole: 1 g / L;

[0134] Ethanol: 570+190ml / L;

[0135] The balance is deionized water.

[0136] The aluminum alloy workpiece was used as the anode connected to the positive electrode of the DC power supply, and the stainless steel was used as the cathode connected to the negative electrode of the DC power supply. The electrolysis temperature was 27 °C, the electrode spacing was 17 mm, the electrochemical polishing DC voltage was 46 V, and the polishing time was 120 s.

[0137] Comparative Example 5

[0138] An aluminum alloy processing solution, the composition of the solution is as follows:

[0139] The volume ratio of perchloric acid, maleic acid and oxalic acid is 1:11:4, 135ml / L;

[0140] Rutin: 3g / L;

[0141] Sulfosalicylic acid: 2 g / L;

[0142] Butanediol: 190ml / L;

[0143] Ethanol: 570 ml / L+2g;

[0144] The balance is deionized water.

[0145] The aluminum alloy workpiece was used as the anode connected to the positive electrode of the DC power supply, and the stainless steel was used as the cathode connected to the negative electrode of the DC power supply. The electrolysis temperature was 27 °C, the electrode spacing was 17 mm, the electrochemical polishing DC voltage was 46 V, and the polishing time was 120 s.

[0146]

[0147] Gloss test: DR60A intelligent gloss meter, reflection angle is 45 o C.

[0148] Roughness test: TMR roughness tester, the average roughness of 5 areas is taken as the roughness result.

[0149] As shown in the table above, when the composite acid maleic acid and oxalic acid are not added to the polishing liquid, and when the viscosity modifier is not added, the polishing effect is very poor. The possible reason is that when the polishing voltage is 46V, the dissolved metal ions are limited, the anode surface mucosal resistance is large, and effective polishing cannot occur. Figure 4 The aluminum alloy treated with the electrolytic polishing liquid configured by the present invention has very few surface irregularities and a good polishing effect, which is far better than that of the attached Figure 5 Aluminum alloy, Figure 6 Comparative Example 1, Figure 7 Comparative Example 2, Figure 8 Comparative Example 3, Fig. 9 Comparative Example 4 shows the effect of the SEM image of the aluminum alloy after polishing.

[0150] The above embodiments are only for illustrating the technical idea of ​​the present invention, and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the present invention; any technology not involved in the present invention can be realized by existing technologies.

Claims

1. A process for processing aluminum alloy, characterized in that The steps include: (1) Surface pretreatment: cleaning - mechanical polishing - degreasing - cleaning - drying; (2) Electrochemical polishing: Prepare the processing solution and place it in the electrochemical polishing tank. Use the surface pretreated aluminum alloy as the anode and the stainless steel as the cathode. Connect them to a DC power supply. The electrolysis temperature is 27 °C, the electrode spacing is 17 mm, the polishing voltage is 46 ± 0.3 V, and the polishing time is 120 s. The processing solution includes a composite acid, a corrosion inhibitor, a brightener, a viscosity regulator, and additives, wherein the composite acid is a mixture of perchloric acid, maleic acid, and oxalic acid, the corrosion inhibitor is rhodine, the brightener is sulfosalicylic acid, the viscosity regulator is butylene glycol, the additives are triethanolamine and benzotriazole, and the solvent is ethanol and water; The ratio of each component of the processing solution is: The volume ratio of perchloric acid, maleic acid and oxalic acid is 1:11:4, 135ml / L Rhodin: 3g / L; Sulfosalicylic acid: 2 g / L; Butylene glycol: 190 ml / L; Triethanolamine: 1 g / L; The benzotriazole: 1 g / L; Ethanol: 570 ml / L; The balance is deionized water; (3) Surface post-treatment: cleaning - drying - coating with a resin protective layer, wherein the resin protective layer is an unsaturated polyester or epoxy acrylate or polyurethane acrylate or polyether acrylate UV protective resin, and the thickness of the resin is less than 1 mm.

2. The aluminum alloy processing process according to claim 1, characterized in that The cleaning is deionized cleaning, and the mechanical polishing is performed by mechanical polishing with 400# and 800# water sandpaper on a pre-grinder to remove the oxide layer.

3. The aluminum alloy processing process according to claim 1, characterized in that The degreasing agent is composed of an aqueous solution of 15 g / L sodium silicate, 10 g / L sodium hydroxide and 20 g / L sodium phosphate, the degreasing temperature is 55° C., the degreasing method is stirring and soaking, and the time is 3 minutes; the drying is carried out at 30° C. and nitrogen purging and drying.