A positive electrode sheet, an electrochemical device and an electronic device containing the positive electrode sheet

By using the synergistic effect of the first positive electrode active material and the second positive electrode active material in the lithium-ion secondary battery, combined with the appropriate compaction density and single-sided density design, the energy density and cycling performance of the lithium-ion secondary battery are solved. Problem, higher energy density and cyclic stability are achieved.

CN114144919BActive Publication Date: 2024-11-01NINGDE AMPEREX TECHNOLOGY LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180004387.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-03-26
Publication Date
2024-11-01
Estimated Expiration
2041-03-26

AI Technical Summary

Technical Problem

During the first charging and discharging process of lithium-ion secondary batteries, it produces solid electrolyte interface masks, resulting in irreversible capacity loss and reducing energy density. The existing lithium supplementation methods such as the use of metal lithium powder are dangerous and have strict production environment requirements, which is difficult to meet the market's energy requirements. Improved density, cyclic performance and kinetic performance.

Method used

Using a positive electrode sheet including the first positive electrode active material Li1+xAaFeyMnzTivPO4-wSw and the second positive electrode active material Li2+rNasM1+qO2+t, the high specific capacity and low first-term capacity of the second positive electrode active material during the first charging through synergistic effect. The cycling stability and rate performance of lithium ion secondary batteries are improved by controlling the compaction density and single-sided density of the positive electrode sheet.

Benefits of technology

It effectively improves the energy density and cycling performance of lithium-ion secondary batteries, improves the rate performance, reduces the capacity loss and impedance increase caused by the structural damage of the positive electrode active material, and improves the overall performance of the electrochemical device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114144919B_ABST
    Figure CN114144919B_ABST
Patent Text Reader

Abstract

The present application provides a positive electrode sheet, an electrochemical device and an electronic device comprising the positive electrode sheet, wherein the positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector; wherein the positive electrode active material layer comprises a first positive electrode active material represented by chemical formula (1) and a second positive electrode active material represented by chemical formula (2): Li 1+ x A a Fe y Mn z Ti v PO 4‑w S w (1) Li 2+r Na s M 1+q O 2+t (2) The positive electrode sheet satisfies: 5.2≤R / Q≤13.5. The positive electrode sheet can give full play to the synergistic effect between the first positive electrode active material and the second positive electrode active material, thereby improving the energy density of the electrochemical device. Furthermore, by limiting the relationship between the compaction density R and the single-surface surface density Q of the positive electrode sheet, the cycle stability and rate performance of the electrochemical device are effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of electrochemistry, and in particular to a positive electrode sheet, an electrochemical device and an electronic device comprising the positive electrode sheet. Background Art

[0002] Lithium-ion secondary batteries have the advantages of high energy storage density, high open circuit voltage, low self-discharge rate, long cycle life, and good safety. They are widely used in various fields such as power storage, mobile electronic devices, electric vehicles, and aerospace equipment. As mobile electronic devices and electric vehicles enter a stage of rapid development, the market has put forward higher and higher requirements on the energy density, cycle performance, and kinetic performance of lithium-ion secondary batteries.

[0003] During the first charge and discharge process of lithium-ion secondary batteries, a large amount of solid electrolyte interphase (SEI) will be produced on the negative electrode surface, which consumes the limited lithium ions and electrolyte in the lithium-ion battery, causing irreversible capacity loss and reducing the energy density of the lithium-ion secondary battery. In batteries using graphite negative electrodes, the first cycle will consume about 10% of the active lithium source; when using negative electrode materials with high specific capacity, such as alloys (silicon, tin, etc.), oxides (silicon oxide, tin oxide, etc.) and amorphous carbon negative electrodes, the consumption of active lithium sources will be further aggravated. Therefore, a suitable lithium supplementation method is particularly important for improving the energy density of lithium-ion secondary batteries.

[0004] At present, a method of replenishing negative electrode lithium has been proposed to solve the above problems, which is usually solved by adding metal lithium powder or stabilized metal lithium powder to the negative electrode slurry. However, metal lithium powder / stabilized metal lithium powder has high reactivity and is easy to react with moisture in the air, which has a high risk factor and puts forward stringent requirements on the production environment and manufacturing process, making negative electrode lithium replenishment face huge challenges. Summary of the invention

[0005] The purpose of the present application is to provide a positive electrode sheet, an electrochemical device and an electronic device comprising the positive electrode sheet, so as to improve the energy density, cycle stability and rate performance of the electrochemical device.

[0006] It should be noted that, in the content of the present application, a lithium ion secondary battery is used as an example of an electrochemical device to explain the present application, but the electrochemical device of the present application is not limited to a lithium ion secondary battery.

[0007] The specific technical solutions are as follows:

[0008] The first aspect of the present application provides a positive electrode plate, which includes a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector; wherein, the positive electrode active material layer includes a first positive electrode active material represented by chemical formula (1) and a second positive electrode active material represented by chemical formula (2): Li 1+x A a Fe y Mn z Ti v PO 4-w S w (1), in chemical formula (1), -0.1 < x < 0.1, 0 < a < 0.01, 0 ≤ y ≤ 1, 0 ≤ z ≤ 1, 0.001 < v < 0.005, 0 ≤ w < 0.05, A includes at least one of Na or K; Li 2+r Na s M 1+q O 2+t (2), in chemical formula (2), -0.2 < r < 0.2, 0 < s < 0.05, -0.1 < q < 0.1, 0 ≤ t < 0.05, M includes at least one of Ni, Cu, Mn, Fe or Co; the tap density of the positive electrode plate is R g / cm 3 , that is, the unit of the tap density R is g / cm 3 , the single-sided areal density of the positive electrode plate is Q g / 1540.25mm 2 , that is, the unit of the single-sided areal density Q is g / 1540.25mm 2 , where 5.2 ≤ R / Q ≤ 13.5.

[0009] In the present application, the positive electrode current collector includes two opposite first surfaces and second surfaces in the thickness direction, and the positive electrode active material layer is disposed on at least one surface of the positive electrode current collector. Those skilled in the art should understand that the positive electrode active material layer can be disposed on the first surface, or on the second surface, or on both the first surface and the second surface at the same time. Those skilled in the art can make a choice according to actual needs. It should be noted that the above "surface" can be the entire area of the first surface and / or the second surface, or a partial area of the first surface and / or the second surface. There is no special limitation in the present application, as long as the purpose of the present application can be achieved.

[0010] The positive electrode active material layer of the present application includes the first positive electrode active material represented by chemical formula Li 1+x A a Fe y Mn z Ti v PO 4-w S w (1) and the chemical formula Li 2+r Nas M 1+q O 2+t (2) The second positive electrode active material shown in. Among them, in Chemical Formula (1), -0.1 < x < 0.1, 0 < a < 0.01, 0 ≤ y ≤ 1, 0 ≤ z ≤ 1, 0.001 < v < 0.005, 0 ≤ w < 0.05, A includes at least one of Na or K; Li 2+r Na s M 1+q O 2+t (2). In Chemical Formula (2), -0.2 < r < 0.2, 0 < s < 0.05, -0.1 < q < 0.1, 0 ≤ t < 0.05, M includes at least one of Ni, Cu, Mn, Fe or Co. In this application, by using the first positive electrode active material and the second positive electrode active material together to produce a synergistic effect, during the first charge, taking advantage of the characteristics of the second positive electrode active material having a high first charge specific capacity and a low first efficiency, the loss of active lithium caused by the formation of SEI is effectively compensated. During the first discharge, there are sufficient lithium ions intercalated back into the first positive electrode active material, effectively improving the discharge specific capacity of the lithium-ion secondary battery, and further improving the energy density of the lithium-ion secondary battery. On the other hand, the structure of the first positive electrode active material is stable and the cycling performance is good.

[0011] In this application, the tap density of the positive electrode sheet is R g / cm 3 , and the single-sided areal density of the positive electrode sheet is Q g / 1540.25 mm 2, where 5.2 ≤ R / Q ≤ 13.5. For example, the lower limit value of R / Q may include the following values: 5.2, 5.48, 5.6, 6.73, 7.43, 7.47, 7.72, 7.93, 8.00, 8.07, or 8.36; the upper limit value of R / Q may include the following values: 8.54, 11, 11.58, 12, 13.1, or 13.5. Without being limited to any theory, when R / Q is too small (e.g., less than 5.2), the compaction density of the positive electrode sheet is too small, which will deteriorate the rate performance and cycling performance of the lithium-ion secondary battery; when the single-sided surface density of the positive electrode sheet is too large, the cycle life of the lithium-ion secondary battery is reduced, and it will also affect the rate performance of the lithium-ion secondary battery, especially reducing the discharge capacity of the lithium-ion secondary battery at high rates. When R / Q is too large (e.g., greater than 13.5), the compaction density of the positive electrode sheet is too large, which will deteriorate the rate performance and cycling performance of the lithium-ion secondary battery; when the single-sided surface density of the positive electrode sheet is too small, it means that under the same lithium-ion secondary battery capacity, the length of the current collector and the separator is increased, which will increase the internal resistance of the lithium-ion secondary battery. By comprehensively designing the compaction density and single-sided surface density of the positive electrode sheet, the cycling performance and rate performance of the lithium-ion secondary battery can be improved. Preferably, 5.6 ≤ R / Q ≤ 12.0. For example, the lower limit value of R / Q may include the following values: 5.6, 6.73, 7.43, 7.47, 7.72, 7.93, 8.00, 8.07, or 8.36; the upper limit value of R / Q may include the following values: 8.54, 11, 11.58, or 12. By controlling the value of R / Q within this preferred range, the cycling performance and kinetic performance of the lithium-ion secondary battery can be further improved.

[0012] In summary, the positive electrode sheet of the present application can fully exert the synergistic effect between the first positive active material and the second positive material. On the one hand, through the first positive active material, the energy density of the lithium-ion secondary battery is increased; on the other hand, through the second positive active material, the cycling performance of the lithium-ion secondary battery is improved. At the same time, by comprehensively designing the compaction density and single-sided surface density of the positive electrode sheet, the cycling performance and rate performance of the lithium-ion secondary battery are further improved.

[0013] In one embodiment of the present application, the compaction density R of the positive electrode sheet satisfies: 1.8 < R < 2.5. For example, the lower limit value of the compaction density R of the positive electrode sheet may include the following values: 1.81 or 1.84; the upper limit value of the compaction density R of the positive electrode sheet may include the following values: 2.2, 2.22, 2.23, 2.24, 2.26, 2.4, or 2.49. Controlling the compaction density R of the positive electrode sheet within the above range is beneficial to the migration of electrons and ions in the positive electrode sheet, thereby improving the rate performance and cycling performance of the lithium-ion secondary battery.

[0014] In an embodiment of the present application, the single-sided surface density Q of the positive electrode sheet satisfies: 0.18 < Q < 0.34. For example, the lower limit value of the single-sided surface density Q of the positive electrode sheet may include the following values: 0.19, 0.20, 0.22, or 0.26; the upper limit value of the single-sided surface density Q of the positive electrode sheet may include the following values: 0.28, 0.29, 0.30, 0.32, or 0.33. Controlling the single-sided surface density Q of the positive electrode sheet within the above range can improve the rate performance and cycle performance of the lithium-ion secondary battery while ensuring the charge-discharge capacity.

[0015] In an embodiment of the present application, the mass ratio of the first positive electrode active material to the second positive electrode active material is 4:1 to 100:1. For example, the lower limit value of the mass ratio may include the following values: 4:1, 4.9:1, 7.5:1, 9:1, 11.4:1, 18.3:1, or 33.4:1; the upper limit value of the mass ratio may include the following values: 98:1, 99:1, or 100:1. When the mass ratio of the first positive electrode active material to the second positive electrode active material is controlled within the above range, a synergistic effect can be generated between the first positive electrode active material and the second positive electrode active material, improving the cycle performance of the lithium-ion secondary battery while enhancing the lithium-ion secondary battery. Preferably, the mass ratio of the first positive electrode active material to the second positive electrode active material is 9:1 to 99:1. For example, the lower limit value of the mass ratio may include the following values: 9:1, 11.4:1, 18.3:1, or 33.4:1; the upper limit value of the mass ratio may include the following values: 98:1 or 99:1. When the mass ratio of the first positive electrode active material to the second positive electrode active material is controlled within the above preferred range, the vast majority of the positive electrode active layer is the first positive electrode active material, which has higher structural stability and can reduce the capacity loss and impedance increase caused by the structural damage of the positive electrode active material, thereby maintaining the cycle stability and kinetic performance of the lithium-ion secondary battery.

[0016] In one embodiment of the present application, the content of the first positive electrode active material in the positive electrode active material layer is 80wt% to 98wt%. For example, the lower limit of the content of the first positive electrode active material may include the following values: 80wt%, 85wt% or 88.6wt%; the upper limit of the content of the first positive electrode active material may include the following values: 91.4wt%, 93.6wt% or 98wt%. By controlling the content of the first positive electrode active material in the positive electrode active material layer within the above range, the positive electrode active material layer has good structural stability, which can reduce the capacity loss and impedance increase caused by the structural destruction of the positive electrode active material. Preferably, the content of the first positive electrode active material in the positive electrode active material layer is 85wt% to 98wt%. For example, the lower limit of the content of the first positive electrode active material may include the following values: 85wt% or 88.6wt%; the upper limit of the content of the first positive electrode active material may include the following values: 91.4wt%, 93.6wt% or 98wt%. The preferred range is higher than the aforementioned range in that the content of the first positive electrode active material in the positive electrode active material layer is higher. Therefore, the positive electrode active material layer can have better structural stability and can also minimize the capacity loss and impedance increase caused by structural damage of the positive electrode active material.

[0017] In one embodiment of the present application, the average particle size Dv50 of the first positive active material is 0.5 μm to 3 μm, and the particle size distribution Dv90 of the first positive active material is 4 μm to 10 μm. For example, the lower limit of the average particle size Dv50 of the first positive active material may include the following values: 0.5 μm, 0.8 μm, 1.1 μm, 1.4 μm or 1.7 μm; the upper limit of the average particle size Dv50 of the first positive active material may include the following values: 2 μm, 2.5 μm or 3 μm. The lower limit of the particle size distribution Dv90 of the first positive active material may include the following values: 4 μm, 5 μm, 6 μm or 7 μm; the upper limit of the particle size distribution Dv90 of the first positive active material may include the following values: 8 μm, 9 μm or 10 μm. The average particle size Dv50 of the second positive electrode active material is 6μm to 18μm, and the particle size distribution Dv90 of the second positive electrode active material is 15μm to 32μm. For example, the lower limit of the average particle size Dv50 of the second positive electrode active material may include the following values: 6μm, 8μm, 10μm or 12μm; the upper limit of the average particle size Dv50 of the second positive electrode active material may include the following values: 14μm, 16μm or 18μm. The lower limit of the particle size distribution Dv90 of the second positive electrode active material may include the following values: 15μm, 17μm, 18μm, 19μm, 21μm or 23μm; the upper limit of the particle size distribution Dv90 of the second positive electrode active material may include the following values: 25μm, 27μm, 29μm, 30μm or 32μm. The use of the first positive electrode active material and the second positive electrode active material having the above-mentioned particle size distribution range further improves the electron and ion transport performance of the positive electrode sheet, thereby improving the cycle performance and kinetic performance of the lithium-ion secondary battery. Preferably, the average particle size Dv50 of the first positive electrode active material is 0.8μm to 2μm, and the particle size distribution Dv90 of the first positive electrode active material is 5μm to 8μm. Preferably, the average particle size Dv50 of the second positive electrode active material is 10μm to 16μm, and the particle size distribution Dv90 of the second positive electrode active material is 18μm to 30μm. The use of the first positive electrode active material and the second positive electrode active material having the above-mentioned preferred particle size distribution range has a better effect on improving the electron and ion transport performance of the positive electrode sheet. Among them, Dv50 represents the particle size distribution of the particle in the volume basis, from the small particle size side, to the volume accumulation of 50%. Dv90 represents the particle size distribution of the particle in the volume basis, from the small particle size side, to the volume accumulation of 90%.

[0018] In one embodiment of the present application, the second positive electrode active material satisfies: X ≥ 300mAh / g, Y / X ≤ 40%; wherein X is the first charge specific capacity of the second positive electrode active material, and Y is the first discharge specific capacity of the second positive electrode active material. This indicates that the second positive electrode active material has a high specific capacity, and a large amount of lithium ions can be released during the first charge to compensate for the loss of active lithium caused by the formation of SEI. During the first discharge, sufficient lithium ions are embedded back into the first active material, which effectively improves the discharge specific capacity of the battery, thereby improving the energy density of the lithium-ion secondary battery.

[0019] In one embodiment of the present application, the positive electrode active material layer includes a first positive electrode active material layer and a second positive electrode active material layer, wherein the first positive electrode active material layer includes a first positive electrode active material, and the second positive electrode active material layer includes a second positive electrode active material. In the present application, the first positive electrode active material and the second positive electrode active material can be separately slurried, and then sequentially coated on the first surface and the second surface of the positive current collector, that is, the first positive electrode active material layer and the second positive electrode active material layer are formed. In some embodiments of the present application, the first surface and / or the second surface of the positive current collector are sequentially provided with the first positive electrode active material layer and the second positive electrode active material layer. In some embodiments of the present application, the first surface and / or the second surface of the positive current collector are sequentially provided with the second positive electrode active material layer and the first positive electrode active material layer. In some embodiments of the present application, the first surface / second surface of the positive current collector is sequentially provided with the second positive electrode active material layer and the second positive electrode active material layer, and the second surface / first surface of the positive current collector is sequentially provided with the first positive electrode active material layer and the second positive electrode active material layer.

[0020] It should be noted that the second positive electrode active material in any of the above embodiments can be used as a positive electrode lithium supplement material in a positive electrode sheet.

[0021] In the positive electrode sheet of the present application, the positive electrode collector is not particularly limited, and can be a positive electrode collector known in the art, such as aluminum foil, aluminum alloy foil or composite current collector. In the present application, there is no particular restriction on the thickness of the positive electrode collector and the positive electrode active material layer, and there is no particular restriction on the thickness of the first positive electrode active material layer and the second positive electrode active material layer, as long as the purpose of the present application can be achieved. For example, the thickness of the positive electrode collector is 5μm to 20μm, preferably 6μm to 18μm, and more preferably 8μm to 16μm. The thickness of the positive electrode active material layer is 30μm to 120μm. Optionally, the positive electrode sheet may also include a conductive layer, which is located between the positive electrode collector and the positive electrode active material layer. The composition of the conductive layer is not particularly limited, and it can be a conductive layer commonly used in the art. The conductive layer includes a conductive agent and a binder.

[0022] The negative electrode sheet of the present application may be a metal lithium sheet, or may include a negative current collector and a negative active material layer disposed on at least one surface of the negative current collector. The present application has no particular restrictions on the negative current collector, as long as the purpose of the present application can be achieved. For example, it may include copper foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, foam nickel, foam copper or a composite current collector. The negative active material layer in the present application includes a negative active material, a conductive agent and a thickener. The negative active material of the present application may include natural graphite, artificial graphite, mesophase microcarbon beads (MCMB), hard carbon, soft carbon, silicon, silicon-carbon composites, SiO, Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, spinel structured lithium titanate Li4Ti5O 12 , at least one of Li-Al alloy and metallic lithium. In the present application, there is no particular restriction on the thickness of the negative electrode current collector and the negative electrode active material layer, as long as the purpose of the present application can be achieved. For example, the thickness of the negative electrode current collector is 6μm to 10μm, and the thickness of the negative electrode active material layer is 30μm to 120μm. In the present application, there is no particular restriction on the thickness of the negative electrode pole piece, as long as the purpose of the present application can be achieved. For example, the thickness of the negative electrode pole piece is 50μm to 150μm. Optionally, the negative electrode pole piece may also include a conductive layer, which is located between the negative electrode current collector and the negative electrode material layer. The composition of the conductive layer is not particularly limited, and it may be a conductive layer commonly used in the art. The conductive layer includes a conductive agent and a binder.

[0023] The above-mentioned conductive agent is not particularly limited, as long as the purpose of the present application can be achieved. For example, the conductive agent can include at least one of conductive carbon black (Super P), carbon nanotubes (CNTs), carbon nanofibers, flake graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes or graphene, etc. The above-mentioned binder is not particularly limited, and any binder known in the art can be used, as long as the purpose of the present application can be achieved. For example, the binder can include at least one of polypropylene alcohol, sodium polyacrylate, potassium polyacrylate, lithium polyacrylate, polyimide, polyimide, polyamide-imide, styrene-butadiene rubber (SBR), polyvinyl alcohol (PVA), polyvinylidene fluoride, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl butyral (PVB), water-based acrylic resin, carboxymethyl cellulose (CMC) or sodium carboxymethyl cellulose (CMC-Na), etc.

[0024] The isolation membrane in the present application is not particularly limited, as long as the purpose of the present application can be achieved. For example, polyethylene (PE), polypropylene (PP)-based polyolefin (PO)-based membranes, polyester films (such as polyethylene terephthalate (PET) films), cellulose films, polyimide films (PI), polyamide films (PA), spandex or aramid films, woven films, non-woven films (non-woven fabrics), microporous films, composite films, diaphragm paper, rolled films, spinning films, etc. At least one. For example, the isolation membrane may include a substrate layer and a surface treatment layer. The substrate layer may be a non-woven fabric, a film or a composite film with a porous structure, and the material of the substrate layer may include at least one of polyethylene, polypropylene, polyethylene terephthalate and polyimide. Optionally, a polypropylene porous membrane, a polyethylene porous membrane, a polypropylene non-woven fabric, a polyethylene non-woven fabric or a polypropylene-polyethylene-polypropylene porous composite membrane may be used. Optionally, a surface treatment layer is provided on at least one surface of the substrate layer, and the surface treatment layer may be a polymer layer or an inorganic layer, or a layer formed by a mixed polymer and an inorganic substance. For example, the inorganic layer includes inorganic particles and a binder, and the inorganic particles are not particularly limited, for example, they can be selected from at least one of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide and barium sulfate. The binder is not particularly limited, for example, it can be selected from one or more combinations of polyvinylidene fluoride, copolymer of vinylidene fluoride-hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylic acid salt, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene and polyhexafluoropropylene. The polymer layer contains a polymer, and the material of the polymer includes at least one of polyamide, polyacrylonitrile, acrylate polymer, polyacrylic acid, polyacrylic acid salt, polyvinylpyrrolidone, polyvinyl ether, polyvinylidene fluoride or poly (vinylidene fluoride-hexafluoropropylene) etc.

[0025] The lithium ion battery of the present application also includes an electrolyte, which may be one or more of a gel electrolyte, a solid electrolyte, and an electrolyte, wherein the electrolyte includes a lithium salt and a non-aqueous solvent. In some embodiments of the present application, the lithium salt may include at least one of LiPF6, LiBF4, LiAsF6, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3, LiSiF6, LiBOB or lithium difluoroborate. For example, the lithium salt may be selected from LiPF6 because it can provide high ionic conductivity and improve cycle characteristics. The non-aqueous solvent may be a carbonate compound, a carboxylate compound, an ether compound, other organic solvents, or a combination thereof. The above-mentioned carbonate compound may be a chain carbonate compound, a cyclic carbonate compound, a fluorinated carbonate compound, or a combination thereof. Examples of the above-mentioned linear carbonate compounds are dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC) and combinations thereof. Examples of cyclic carbonate compounds are ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinyl ethylene carbonate (VEC) and combinations thereof. Examples of fluorocarbonate compounds are fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, trifluoromethylethylene carbonate and combinations thereof. Examples of the above-mentioned carboxylic acid ester compounds are methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decanolactone, valerolactone, mevalonolactone, caprolactone and combinations thereof. Examples of the above-mentioned ether compounds are dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, ethoxymethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran and combinations thereof. Examples of the above-mentioned other organic solvents are dimethyl sulfoxide, 1,2-dioxolane, cyclopentane, methylcyclopentane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, formamide, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate, trioctyl phosphate and phosphates and combinations thereof.

[0026] In the present application, when preparing the positive electrode active material layer, there is no particular restriction on the order of adding the first positive electrode active material and the second positive electrode active material. For example, the first positive electrode active material and the second positive electrode active material can be directly mixed evenly during slurry preparation, and the mixed slurry can be applied to the first surface and / or the second surface of the positive electrode current collector; the first positive electrode active material and the second positive electrode active material can also be slurried separately, and then the above two slurries are sequentially applied to the first surface and / or the second surface of the positive electrode current collector to form the first positive electrode active material layer and the second positive electrode active material layer.

[0027] The present application also provides an electrochemical device, comprising the positive electrode sheet described in any of the above embodiments, and the electrochemical device has high energy density, good cycle performance and rate performance.

[0028] The electrochemical device of the present application is not particularly limited, and may include any device that undergoes an electrochemical reaction. In some embodiments, the electrochemical device may include, but is not limited to: a lithium metal secondary battery, a lithium ion secondary battery (lithium ion battery), a lithium polymer secondary battery, or a lithium ion polymer secondary battery, etc.

[0029] The present application also provides an electronic device, comprising the electrochemical device described in the embodiments of the present application, wherein the electronic device has high energy density, good cycle performance and rate performance.

[0030] The electronic device of the present application is not particularly limited, and it can be any electronic device known in the prior art. In some embodiments, the electronic device may include, but is not limited to, a laptop computer, a pen-input computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, an LCD TV, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery and a lithium-ion capacitor, etc.

[0031] The preparation process of the electrochemical device is well known to those skilled in the art and is not particularly limited in this application. For example, the electrochemical device can be manufactured by the following process: the positive electrode sheet and the negative electrode sheet are overlapped via a separator, and are wound, folded, etc. as required and placed in a housing, and the electrolyte is injected into the housing and sealed, wherein the separator used is the above-mentioned separator provided in this application. In addition, overcurrent protection elements, guide plates, etc. can also be placed in the housing as required to prevent pressure rise and overcharge and discharge inside the electrochemical device.

[0032] The present application provides a positive electrode sheet, an electrochemical device and an electronic device comprising the positive electrode sheet, wherein the positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector; wherein the positive electrode active material layer comprises a first positive electrode active material represented by chemical formula (1) and a second positive electrode active material represented by chemical formula (2): Li 1+x A a Fe y Mn z Ti v PO 4-w S w (1) Li 2+r Na s M 1+q O 2+t (2); The positive electrode sheet satisfies: 5.2≤R / Q≤13.5. The positive electrode sheet can give full play to the synergistic effect between the first positive electrode active material and the second positive electrode active material, effectively improve the discharge specific capacity of the electrochemical device, and thus improve the energy density of the electrochemical device. In addition, by limiting the relationship between the compaction density R and the single-surface surface density Q of the positive electrode sheet, the cycle stability and rate performance of the electrochemical device are effectively improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the technical solutions of the present application and the prior art, the following briefly introduces the drawings required for use in the embodiments and the prior art. Obviously, the drawings described below are only some embodiments of the present application.

[0034] Figure 1 A schematic diagram of the structure of a positive electrode sheet according to an embodiment of the present application (front view);

[0035] Figure 2 A schematic diagram of the positive electrode structure of another embodiment of the present application (front view);

[0036] Figure 3 A schematic diagram of the structure of a positive electrode sheet according to another embodiment of the present application (top view);

[0037] Figure 4 This is a schematic diagram of the positive electrode structure of another embodiment of the present application (front view);

[0038] Figure 5 This is a schematic diagram of the positive electrode plate structure (front view) of another implementation scheme of the present application.

[0039] Reference numerals: 10. positive electrode current collector, 20. positive electrode active material layer, 21. first positive electrode active material layer, 22. second positive electrode active material layer, 31. first surface, 32. second surface. DETAILED DESCRIPTION

[0040] In order to make the purpose, technical scheme, and advantages of the present application more clearly understood, the present application is further described in detail with reference to the accompanying drawings and embodiments. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all the embodiments. All other embodiments obtained by ordinary technicians in this field based on the present application belong to the scope of protection of the present application.

[0041] It should be noted that in the specific embodiments of the present application, a lithium ion secondary battery is used as an example of an electrochemical device to explain the present application, but the electrochemical device of the present application is not limited to a lithium ion secondary battery.

[0042] Figure 1 A schematic diagram of the positive electrode structure of an embodiment of the present application (front view) is shown, as Figure 1 As shown, the positive electrode current collector 10 is coated with the positive electrode active material layer 20 on the first surface 31 and the second surface 32 in the thickness direction, wherein the first positive electrode active material and the second positive electrode active material in the positive electrode active material layer 20 are directly mixed evenly during slurry preparation, and the mixed slurry is coated on the first surface 31 and the second surface 32 of the positive electrode current collector 10. Of course, it is also possible to coat only one side of the first surface 31 or the second surface 32, such as Figure 2 As shown, Figure 2 A schematic diagram (front view) of the positive electrode sheet structure of another embodiment of the present application is shown, in which the positive electrode active material layer 20 is only coated on the first surface 31 of the positive electrode collector 10, and is not coated on the second surface 32.

[0043] Figure 3 A schematic diagram (top view) of the positive electrode structure of another embodiment of the present application is shown. Figure 3 As shown, the positive electrode active material layer 20 is coated on a partial area of ​​the surface of the positive electrode current collector 10. Of course, the positive electrode active material layer 20 can also be coated on the entire area of ​​the surface of the positive electrode current collector 10.

[0044] Figure 4 and Figure 5 The schematic diagrams (front views) of the structures of the positive electrode sheets of two further embodiments of the present application are shown respectively, as shown in FIG. Figure 4 and Figure 5 As shown, the first positive electrode active material and the second positive electrode active material in the positive electrode active material layer 20 are slurried separately and sequentially coated on the first surface 31 and the second surface 32 of the positive electrode current collector 10. In these two embodiments, the positive electrode active material layer 20 includes the first positive electrode active material layer 21 and the second positive electrode active material layer 22. Figure 4As shown, the first surface 31 / the second surface 32 is coated with the first positive electrode active material layer 21 and the second positive electrode active material layer 22 in sequence along the direction in which the first surface 31 / the second surface 32 extends outward. Figure 5 As shown, the first positive electrode active material layer 21 and the second positive electrode active material layer 22 are sequentially coated on the first surface 31 along the direction in which the first surface 31 extends outward, and the second positive electrode active material layer 22 and the first positive electrode active material layer 21 are sequentially coated on the second surface 32 along the direction in which the second surface 32 extends outward.

[0045] Example

[0046] The following examples and comparative examples are given to more specifically describe the embodiments of the present application. Various tests and evaluations were performed according to the following methods. In addition, unless otherwise specified, "parts" and "%" are based on mass.

[0047] Test methods and equipment:

[0048] Compacted density R of positive electrode:

[0049] The compaction density R of the positive electrode sheet is calculated by the formula: R = m / v. In the formula, m is the mass of the positive electrode active material layer, unit: g; v is the volume of the positive electrode active material layer, unit: cm 3 , where the volume v is the product of the area Ar of the positive electrode active material layer and the thickness of the positive electrode active material layer.

[0050] Single-sided surface density Q of the positive electrode:

[0051] The single-surface density Q of the positive electrode sheet is calculated by the formula: Q = 1540.25m / Ar. In the formula, m is the mass of the positive electrode active material layer, unit: g; Ar is the area of ​​the positive electrode active material layer, unit: mm 2 .

[0052] Cathode active material Dv50 and Dv90 test:

[0053] The Dv50 and Dv90 of the first positive electrode active material and the second positive electrode active material were measured using a laser particle size analyzer.

[0054] High temperature cycle performance test:

[0055] At 60°C, charge the lithium-ion secondary battery to 3.6V at a constant current of 1C, then charge at a constant voltage until the current is less than or equal to 0.05C, and then discharge at a constant current of 1C to 2.5V. This is a charge and discharge cycle, and record the discharge capacity of the first cycle of the lithium-ion secondary battery. Perform charge and discharge cycles of the lithium-ion secondary battery 1000 times according to the above method, record the 1000th discharge capacity, and the capacity retention rate = 1000th discharge capacity / first discharge capacity, and record the capacity retention rate.

[0056] Rate performance test:

[0057] At 25°C, the lithium-ion secondary battery was charged at a constant current of 0.2C to 3.6V, then charged at a constant voltage to a current less than or equal to 0.05C, then left to stand for 30 minutes, and then discharged at a constant current of 0.2C to 2.5V. The 0.2C rate discharge capacity of the lithium-ion secondary battery was obtained by testing.

[0058] At 25°C, the lithium-ion secondary battery was charged at a constant current of 0.2C to 3.6V, then charged at a constant voltage to a current less than or equal to 0.05C, then left to stand for 30 minutes, and then discharged at a constant current of 1C to 2.5V. The 1C rate discharge capacity of the lithium-ion secondary battery was obtained by testing.

[0059] 1C rate discharge capacity retention rate of lithium ion secondary battery (%)=1C rate discharge capacity / 0.2C rate discharge capacity×100%.

[0060] Energy density test:

[0061] At 25°C, charge the lithium-ion secondary battery to 3.6V at a constant current of 0.2C, then charge at a constant voltage until the current is less than or equal to 0.05C, let it stand for 30 minutes, and then discharge it to 2.5V at a constant current of 0.2C. Record the discharge capacity D0 (Ah) and discharge platform V0 (V) of the lithium-ion secondary battery at 0.2C. Weigh the mass of the lithium-ion battery, recorded as m0 (kg).

[0062] The energy density of the lithium-ion secondary battery is calculated according to the following formula: Energy density = D0×V0 / m0.

[0063] Charge and discharge specific capacity test:

[0064] <Preparation of button cell>

[0065] The second positive electrode active material, conductive carbon black and binder polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 90:5:5, N-methylpyrrolidone (NMP) was added as a solvent, and a slurry with a solid content of 40% was prepared by stirring. A coating with a thickness of 100 μm was applied on the current collector aluminum foil using a scraper, and after drying in a vacuum drying oven at 130°C for 12 hours, a punch was used to cut into discs with a diameter of 1 cm in a dry environment, and a metal lithium sheet was used as a counter electrode in a glove box, and a ceglard composite membrane was selected as an isolation membrane, and an electrolyte was added to assemble a button cell. The electrolyte was an organic solution obtained by mixing ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) in a mass ratio of 30:50:20, and the concentration of lithium salt in the electrolyte was 1.15 mol / L.

[0066] <Charge specific capacity test>

[0067] This application uses the Wuhan Blue Electric CT2001A system to perform a charge capacity test. The button battery to be tested containing the second positive electrode active material is placed in an environment of 25±3°C for 30 minutes, and is charged at a constant current rate of 0.1C (theoretical gram capacity is 400mAh / g) to a voltage of 4.4V, and then charged at a constant voltage to a current of 0.025C, and the charging capacity is recorded.

[0068] The charging specific capacity of the button cell containing the second positive electrode active material=charging capacity / mass of the second positive electrode active material.

[0069] <Test of discharge specific capacity>

[0070] This application uses the Wuhan Blue Electric CT2001A system to perform a discharge specific capacity test. The button battery to be tested containing the second positive electrode active material is placed in an environment of 25±3°C for 30 minutes, and is charged at a constant current rate of 0.1C (theoretical gram capacity is 400mAh / g) to a voltage of 4.4V. Subsequently, it is charged at a constant voltage to a current of 0.025C and placed for 5 minutes. The button battery is then discharged at a constant current of 0.1C to a termination voltage of 2.5V, and the first discharge capacity is recorded.

[0071] The discharge specific capacity of the button cell containing the second positive electrode active material=discharge capacity / mass of the second positive electrode active material.

[0072] Example 1

[0073] <Preparation of positive electrode sheet>

[0074] The first positive electrode active material Li 0.998 Na 0.002 Fe 0.996 Ti 0.002 PO4, the second positive electrode active material Li 1.995Na 0.005 NiO2, binder PVDF and conductive agent conductive carbon black are mixed, among which Li 0.998 Na 0.002 Fe 0.996 Ti 0.002 PO4、Li 1.995 Na 0.005 The mass ratio of NiO2, PVDF and conductive carbon black is 93.6:2.8:2.1:1.5, and then the solvent NMP is added, and stirred under vacuum stirring until a uniform transparent system is obtained to obtain a positive electrode slurry with a solid content of 75%. The positive electrode slurry is evenly coated on a positive electrode current collector aluminum foil with a thickness of 10μm, and dried at 130°C to obtain a positive electrode sheet with a coating thickness of 110μm. After the above steps are completed, the single-sided coating of the positive electrode sheet is completed. After that, the above steps are repeated on the other surface of the positive electrode sheet to obtain a positive electrode sheet with double-sided coating of positive electrode active materials. After the coating is completed, the positive electrode sheet is cut into a specification of 74mm×867mm after cold pressing and welded to the pole ear for standby use.

[0075] <Preparation of negative electrode sheet>

[0076] The negative electrode active material graphite, nano-conductive carbon black, styrene-butadiene rubber and sodium carboxymethyl cellulose are mixed in a mass ratio of 95:2:1.5:1.5, deionized water is added as a solvent, and a slurry with a solid content of 70% is prepared and stirred evenly. The slurry is evenly coated on the current collector copper foil, dried at 110°C, and cold pressed to obtain a negative electrode sheet with a single-sided coating of active material layer with a thickness of 150μm. After the above steps are completed, the same method is used to complete these steps on the back of the negative electrode sheet, that is, a negative electrode sheet with double-sided coating is obtained. After the coating is completed, the negative electrode sheet is cut into a specification of 76mm×851mm and the pole ears are welded for standby use.

[0077] <Preparation of Electrolyte>

[0078] In a dry argon atmosphere, organic solvents ethylene carbonate, ethyl methyl carbonate and diethyl carbonate were mixed in a mass ratio of EC:EMC:DEC=30:50:20 to obtain an organic solution, and then lithium salt lithium hexafluorophosphate was added to the organic solvent to dissolve and mix evenly to obtain an electrolyte with a lithium salt concentration of 1.15 mol / L.

[0079] <Preparation of Separator Film>

[0080] A polypropylene (PP) film with a thickness of 14 μm (provided by Celgard Company) was used.

[0081] <Preparation of lithium-ion batteries>

[0082] The positive electrode, separator and negative electrode prepared above are stacked in order, with the separator placed between the positive and negative electrodes to play a role of isolation, and then wound to obtain an electrode assembly. The electrode assembly is placed in an aluminum-plastic film packaging bag, and the moisture is removed at 80°C, and the prepared electrolyte is injected. After vacuum packaging, standing, forming, shaping and other processes, a lithium-ion battery is obtained.

[0083] In Example 2, Example 3, Example 4, Example 5, Example 6, Example 7, Example 8, Example 9, Example 10, Example 11, Example 12, Example 13, Example 14, Example 15, Example 16, Example 17, Example 18 and Example 19, the preparation steps of <Preparation of positive electrode sheet>, <Preparation of negative electrode sheet>, <Preparation of electrolyte>, <Preparation of separator> and <Preparation of lithium ion battery> are the same as those in Example 1, and the changes of relevant preparation parameters are shown in Table 1:

[0084] Table 1

[0085]

[0086] In Comparative Example 1, Comparative Example 2, Comparative Example 3, Comparative Example 4 and Comparative Example 5, the preparation steps of <Preparation of Positive Electrode Plate>, <Preparation of Negative Electrode Plate>, <Preparation of Electrolyte>, <Preparation of Separator> and <Preparation of Lithium Ion Battery> are the same as those in Example 1, and the changes in relevant preparation parameters are shown in Table 2:

[0087] Table 2

[0088]

[0089] Note: “ / ” in Table 2 indicates that the corresponding preparation parameter does not exist.

[0090] Comparative Example 6

[0091] <Preparation of Second Positive Electrode Active Material>

[0092] Weigh an appropriate amount of citric acid and add it to Li2NiO2 (the mass ratio of citric acid to Li2NiO2 is 1:50), use ethanol as solvent for mechanical stirring and mixing, ultrasonic dispersion for 1 hour, and after obtaining a mixed solution, stir in a water bath to evaporate the solvent, and after obtaining a dry product, perform the first sintering in a nitrogen atmosphere at a sintering temperature of 350°C for 4 hours; after cooling, grind the above product and acetylene black (the mass ratio of the above product to acetylene black is 97:3), and then perform a second sintering in an inert atmosphere at a sintering temperature of 600°C for 8 hours to obtain the second positive electrode active material of carbon-coated Li2NiO2.

[0093] <Preparation of positive electrode sheet>, <Preparation of negative electrode sheet>, <Preparation of electrolyte>, <Preparation of separator> and <Preparation of lithium-ion battery> are the same as those in Example 1.

[0094] The preparation parameters and test results of Example 1, Example 2, Example 3, Example 4, Example 5, Example 6, Example 7, Example 8, Example 9, Example 10, Example 11, Example 12, Example 13, Example 14, Example 15, Example 16, Example 17, Example 18, Example 19, Comparative Example 1, Comparative Example 2, Comparative Example 3, Comparative Example 4, Comparative Example 5, and Comparative Example 6 are shown in Table 3:

[0095]

[0096]

[0097] From Example 1, Example 2, Example 3, Example 4, Example 5, Example 6, Example 7, Example 8, Example 9, Example 10, Example 11, Example 12, Example 13, Example 14, Example 15, Example 16, Example 17, Example 18, Example 19 and Comparative Example 1, Comparative Example 2, Comparative Example 3, Comparative Example 4, Comparative Example 6, it can be seen that the use of the first positive electrode active material and the second positive electrode active material together produces a synergistic effect. On the one hand, during the first charge, the second positive electrode active material has the characteristics of high first charge specific capacity and low first efficiency, which effectively compensates for the loss of active lithium caused by the generation of SEI. During the first discharge, there are enough lithium ions embedded back into the first positive electrode active material, which effectively improves the discharge specific capacity of the lithium ion secondary battery, thereby improving the energy density. On the other hand, the first positive electrode active material has a stable structure and good cycle performance. In addition, by controlling the compaction density R and single-sided surface density Q of the positive electrode sheet within the scope of this application, the lithium ion secondary battery can have good rate performance.

[0098] It can be seen from Example 1, Example 2, Example 3, Example 13, Example 14, Example 15 and Comparative Example 5 that the same first positive electrode active material and the second positive electrode active material are used in the positive electrode plate, and the cycle performance, rate performance and energy density of the lithium-ion secondary battery change with the change of the content of the first positive electrode active material and the second positive electrode active material. When the content of the first positive electrode active material and the second positive electrode active material in the positive electrode active material layer is within the scope of this application, the cycle performance, rate performance and energy density of the lithium-ion secondary battery are significantly improved. The proportional relationship between the compaction density R and the single-sided surface density Q of the positive electrode plate usually also affects the performance of the lithium-ion secondary battery. By controlling the ratio between the compaction density R and the single-sided surface density Q of the positive electrode plate within the scope of this application, the cycle stability and rate performance of the lithium-ion secondary battery are improved.

[0099] It can be seen from Example 8 and Comparative Example 4 that when the same first positive electrode active material is used, the use of the second positive electrode active material of the present application can more effectively exert the synergistic effect of the first positive electrode active material and the second positive electrode active material, so that the cycle performance, rate performance and energy density of the lithium-ion secondary battery are significantly improved.

[0100] From the above analysis, it can be seen that the positive electrode plate provided in the present application, by selecting a suitable first positive electrode active material and a second positive electrode active material, enables the positive electrode plate to give full play to the synergistic effect between the first positive electrode active material and the second positive electrode active material, effectively improve the discharge specific capacity of the electrochemical device, and then improve the energy density, cycle performance and rate performance of the electrochemical device.

[0101] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.

Claims

1. A positive electrode plate, which comprises a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector; wherein, the positive electrode active material layer comprises a first positive electrode active material represented by chemical formula (1) and a second positive electrode active material represented by chemical formula (2): Li 1+x A a Fe y Mn z You v PO 4-w S w (1) In chemical formula (1), -0.1 < x < 0.1, 0 < a < 0.01, 0 ≤ y ≤ 1, 0 ≤ z ≤ 1, 0.001 < v < 0.005, 0 ≤ w < 0.05, and A includes at least one of Na or K; Li 2+r So s M 1+q O 2+t (2), In chemical formula (2), -0.2 < r < 0.2, 0 < s < 0.05, -0.1 < q < 0.1, 0 ≤ t < 0.05, and M includes at least one of Ni, Cu, Mn, Fe, or Co; The compaction density of the positive electrode sheet is R g / cm 3 The single-sided surface density of the positive electrode sheet is Q g / 1540.25 mm 2 , and 5.2≤R / Q≤13.5; the mass ratio of the first positive electrode active material to the second positive electrode active material is 4:1 to 100:1, and the content of the first positive electrode active material in the positive electrode active material layer is 80wt% to 98wt%.

2. The positive electrode sheet according to claim 1, wherein: The tap density R of the positive electrode plate satisfies: 1.8 < R < 2.

5.

3. The positive electrode sheet according to claim 1, wherein: The single-sided surface density Q of the positive electrode plate satisfies: 0.18 < Q < 0.

34.

4. The positive electrode sheet according to claim 1, wherein: The average particle size Dv50 of the first positive electrode active material is 0.5 μm to 3 μm, and the particle size distribution Dv90 of the first positive electrode active material is 4 μm to 10 μm.

5. The positive electrode sheet according to claim 1, wherein: The average particle size Dv50 of the second positive electrode active material is 6 μm to 18 μm, and the particle size distribution Dv90 of the second positive electrode active material is 15 μm to 32 μm.

6. The positive electrode sheet according to claim 1, wherein: The second positive electrode active material satisfies: X ≥ 300 mAh / g, Y / X ≤ 40%; wherein, X is the initial charge specific capacity of the second positive electrode active material, and Y is the initial discharge specific capacity of the second positive electrode active material.

7. The positive electrode sheet according to claim 1, wherein: The positive electrode plate satisfies at least one of the following characteristics: (a) The positive electrode plate satisfies: 5.6 ≤ R / Q ≤ 12.0; (b) The mass ratio of the first positive electrode active material to the second positive electrode active material is 9:1 to 99:1; (c) The content of the first positive electrode active material in the positive electrode active material layer is 85 wt% to 98 wt%; (d) The average particle size Dv50 of the first positive electrode active material is 0.8 μm to 2 μm, and the particle size distribution Dv90 of the first positive electrode active material is 5 μm to 8 μm; (e) The average particle size Dv50 of the second positive electrode active material is 10 μm to 16 μm, and the particle size distribution Dv90 of the second positive electrode active material is 18 μm to 30 μm.

8. The positive electrode sheet according to any one of claims 1 to 7, wherein: The positive electrode active material layer includes a first positive electrode active material layer and a second positive electrode active material layer. The first positive electrode active material layer includes the first positive electrode active material, and the second positive electrode active material layer includes the second positive electrode active material.

9. An electrochemical device, which comprises the positive electrode plate according to any one of claims 1 to 8.

10. An electronic device, which comprises the electrochemical device according to claim 9.