Resin composition and molded article

By using a composition containing the first thermoplastic resin and glass fibers and the second thermoplastic resin, the problems of low mechanical properties and MDTD anisotropy of the molded body of the thermoplastic resin composition are solved, and higher impact strength and machinery are achieved Strength and reduce the intensity difference in the MDTD direction.

CN114206997BActive Publication Date: 2024-11-08SUMITOMO CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080055563.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-08-09
Filing Date
2020-04-16
Publication Date
2024-11-08
Estimated Expiration
2040-04-16

AI Technical Summary

Technical Problem

The conventional thermoplastic resin composition has problems with low mechanical properties and MDTD anisotropy in the molded body. Especially in parts such as automobile frame-based components or suspension-based components, it is difficult to realize a molded body that is both lightweight and high-strength.

Method used

A composition containing the first thermoplastic resin and glass fiber and a second thermoplastic resin is adopted, wherein the flow start temperature of the second thermoplastic resin is lower than that of the resin particles, and the fiberglass fiber has a fineness of 500 g/1000 m or more and 3400 g/1000 m or less. Moreover, the content of glass fiber is between 35-65 parts by mass, which is used to reduce the MDTD anisotropy of the molded body.

Benefits of technology

Through the resin composition, the impact strength and mechanical strength of the molded body are significantly improved, the strength difference in the MDTD direction is reduced, and the overall strength and heat resistance of the molded body are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003493662360000331
    Figure BDA0003493662360000331
  • Figure BDA0003493662360000361
    Figure BDA0003493662360000361
  • Figure BDA0003493662360000371
    Figure BDA0003493662360000371
Patent Text Reader

Abstract

The resin composition of the present invention contains resin pellets containing a first thermoplastic resin and glass fibers and a second thermoplastic resin, wherein the flow start temperature of the second thermoplastic resin is lower than that of the resin pellets, and the fineness of the glass fibers is 500 g / 1000 m or more and 3400 g / 1000 m or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a resin composition and a molded body produced using the resin composition.

[0002] This application claims priority based on Japanese Patent Application No. 2019-148160 filed in Japan on August 9, 2019, and the contents are incorporated herein by reference. Background Art

[0003] In recent years, in the field of transportation equipment including automobiles and airplanes, the purpose of improving fuel efficiency is to reduce the weight of parts. In order to reduce the weight of parts, research is being conducted to replace the existing metal materials with resin materials in the materials of various parts. For example, by using thermoplastic resin as a molding material for frame components, suspension components, impact absorbing components, etc. for automobiles, it is possible to obtain automobiles that are lighter than existing products.

[0004] However, there is a problem that molded articles obtained from the above-mentioned thermoplastic resins have lower mechanical properties than molded articles obtained from metal materials.

[0005] Conventionally, in order to improve the strength of molding materials such as thermoplastic resin compositions, a method of mixing fibers as fillers with thermoplastic resins has been proposed (for example, see Patent Document 1).

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent document 1: Japanese Patent Application Laid-Open No. 10-77350. Summary of the invention

[0009] Problems to be solved by the invention

[0010] In the case of molded bodies that account for a large proportion of the weight of the vehicle body, such as frame members, suspension members, and impact absorbing members for automobiles, further weight reduction is required. However, with further weight reduction of the molded bodies, ensuring the strength of the molded bodies becomes a problem.

[0011] With regard to such a problem, the conventional method of simply mixing fibers as fillers with thermoplastic resins cannot obtain the required molded product strength.

[0012] In addition, the injection molded product obtained from the thermoplastic resin composition, usually, when a fibrous filler is used as a filler, the ratio of the filler orientation along the MD direction (flow direction) is increased due to the shear force during injection molding, so there is also a problem of MDTD anisotropy of mechanical strength, that is, the mechanical strength in the MD direction is high, but the mechanical strength in the TD direction (direction orthogonal to the flow) is low.

[0013] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a resin composition having MDTD anisotropy capable of reducing the strength of a molded product, and a molded product produced using the resin composition.

[0014] Technical solutions to solve problems

[0015] In order to solve the above-mentioned problems, the present invention adopts the following configuration.

[0016] [1] A resin composition comprising resin pellets containing a first thermoplastic resin and glass fibers and a second thermoplastic resin, wherein the second thermoplastic resin has a flow start temperature lower than that of the resin pellets, and the glass fibers in the resin pellets have a fineness of 500 g / 1000 m or more and 3400 g / 1000 m or less.

[0017] [2] The resin composition according to [1], wherein the content of the glass fiber is more than 35 parts by mass and less than 65 parts by mass based on 100 parts by mass of the total amount of the resin particles and the second thermoplastic resin.

[0018] [3] The resin composition according to [1] or [2], wherein the content of the second thermoplastic resin is 10 to 45 parts by mass based on 100 parts by mass of the total amount of the resin particles and the second thermoplastic resin.

[0019] [4] The resin composition according to any one of [1] to [3], wherein the first thermoplastic resin and the second thermoplastic resin are both liquid crystal polyester resins.

[0020] [5] The resin composition according to any one of [1] to [4], wherein the length-weighted average fiber length of the glass fibers is 5 to 20 mm.

[0021] [6] The resin composition according to any one of [1] to [5], wherein the number average fiber diameter of the glass fiber is 10 to 20 μm.

[0022] [7] A resin composition comprising resin particles containing a first thermoplastic resin and glass fibers and a second thermoplastic resin, wherein when a notched Charpy impact strength test is performed on a molded body having a size of 10 mm in width, 80 mm in length, and 4 mm in thickness produced using the resin composition, the impact strength in the MD direction (MD i ) and TD direction impact strength (TD i ) ratio (TD i / MD i ) is greater than 0.5.

[0023] [8] A molded product produced using the resin composition according to any one of [1] to [7].

[0024] Effects of the Invention

[0025] According to the present invention, the MDTD anisotropy of the strength of a molded body can be reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a schematic diagram which shows an example of the manufacturing apparatus of a resin pellet. DETAILED DESCRIPTION

[0027] (Resin composition)

[0028] The resin composition of the present embodiment contains resin pellets containing a first thermoplastic resin and glass fibers, and a second thermoplastic resin.

[0029] Here, the form of the resin composition is not particularly limited, and it can be any mixture of resin particles containing a first thermoplastic resin and glass fibers and a powdered or granular second thermoplastic resin; granular materials in which the resin particles are coated with the second thermoplastic resin; injection-molded products formed by injection molding the mixture or the granular materials, etc.

[0030] <Resin pellets containing a first thermoplastic resin and glass fibers>

[0031] The resin particles containing the first thermoplastic resin and glass fibers in this embodiment (hereinafter also referred to as "resin particles") are, for example, a substance obtained by impregnating glass fibers with a molten product obtained by melt-kneading the first thermoplastic resin and other components as required and granulating the molten product, and are resin particles in which the glass fibers are fixed by the first thermoplastic resin.

[0032] The flow start temperature of the resin particles in the present embodiment is preferably 250° C. or higher, more preferably 260° C. or higher.

[0033] In addition, the flow start temperature of the resin particles in the present embodiment is preferably 400° C. or lower, and more preferably 380° C. or lower.

[0034] For example, the flow start temperature of the resin particles in the present embodiment is preferably 250°C to 400°C, more preferably 260°C to 400°C, and further preferably 260°C to 380°C.

[0035] There is a tendency that the higher the flow start temperature of the resin particles is, the higher the heat resistance and strength of a molded body produced using a resin composition containing the resin particles is.

[0036] On the other hand, when the flow start temperature of the resin particles exceeds 400° C., the melting temperature or melt viscosity of the resin particles tends to increase. Therefore, the temperature required for molding a resin composition containing the resin particles tends to increase.

[0037] In this specification, the flow start temperature (the flow start temperature of resin particles or liquid crystal polyester resin) is also called the viscosity flow temperature or flow temperature, which is an estimated temperature of the molecular weight of the thermoplastic resin (thermoplastic resin contained in the resin particles) (refer to Naoyuki Oide, "Liquid Crystal Polymer - Synthesis, Molding, and Application -", CMC Co., Ltd. (CMC Co., Ltd.), June 5, 1987, p. 95).

[0038] As a method for measuring the flow start temperature, specifically, a capillary rheometer is used to measure the resin pellets or thermoplastic resin at 9.8 MPa (100 kg / cm 2 ) under a load of 4°C / min while melting and showing a viscosity of 4800 Pa·s (48000 poise) when extruded from a nozzle with an inner diameter of 1 mm and a length of 10 mm.

[0039] The resin pellets were freeze-pulverized using a ball mill freeze pulverizer (manufactured by Japan Analytical Industry Co., Ltd., JFC-1500) under the following conditions before the measurement, and the flow start temperature was measured.

[0040] Granule dosage: 5g.

[0041] Pre-freezing time: 10min.

[0042] Freezing crushing time: 10min.

[0043] 《The first thermoplastic resin》

[0044] Examples of the first thermoplastic resin contained in the resin particles in the present embodiment include polyolefin resins such as polyethylene, polypropylene, polybutadiene, and polymethylpentene; ethylene resins such as vinyl chloride, vinylidene chloride acetate, and polyvinyl alcohol; polystyrene resins such as polystyrene, acrylonitrile-styrene resin (AS resin), and acrylonitrile-butadiene-styrene resin (ABS resin); polyamide 6 (nylon 6), polyamide 66 (nylon 66), polyamide 11 (nylon 11), polyamide 12 (nylon 12), polyamide 46 (nylon 46), polyamide 610 (nylon 610), polytetramethylene terephthalamide (nylon 4T), and polyhexamethylene terephthalamide. Polyamide resins such as polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, and polytrimethylene terephthalate; polysulfone resins such as modified polysulfone, polyethersulfone, polysulfone, and polyphenylsulfone; polyphenylene sulfide such as linear polyphenylene sulfide, cross-linked polyphenylene sulfide, and semi-cross-linked polyphenylene sulfide, polyetherketone, polyetheretherketone, and polyetherketoneketone; polycarbonate; polyphenylene ether; polyimide resins such as thermoplastic polyimide, polyamideimide, and polyetherimide, etc.

[0045] As the first thermoplastic resin in the present embodiment, polypropylene or a liquid crystal polyester resin (hereinafter also referred to as a "first liquid crystal polyester resin") is preferred from the viewpoint of impact strength of a molded body made using a resin composition containing the resin particles, and a liquid crystal polyester resin is more preferred from the viewpoint of fluidity, heat resistance and dimensional accuracy.

[0046] (First Liquid Crystalline Polyester Resin)

[0047] The first liquid crystal polyester resin is not particularly limited as long as it is a polyester resin showing liquid crystal properties in a molten state, but is preferably melted at a temperature below 400° C. It should be noted that the first liquid crystal polyester resin in the present embodiment may be a liquid crystal polyester amide, a liquid crystal polyester ether, a liquid crystal polyester carbonate, a liquid crystal polyester imide, or the like.

[0048] The first liquid crystal polyester resin in the present embodiment is preferably a wholly aromatic liquid crystal polyester produced using only aromatic compounds as raw material monomers.

[0049] Typical examples of the first liquid crystal polyester resin in the present embodiment include liquid crystal polyesters formed by polymerizing (condensing) aromatic hydroxycarboxylic acids, aromatic dicarboxylic acids and at least one compound selected from the group consisting of aromatic diols, aromatic hydroxylamines and aromatic diamines; liquid crystal polyesters formed by polymerizing a plurality of aromatic hydroxycarboxylic acids; liquid crystal polyesters formed by polymerizing aromatic dicarboxylic acids and at least one compound selected from the group consisting of aromatic diols, aromatic hydroxylamines and aromatic diamines; and liquid crystal polyesters formed by polymerizing polyesters such as polyethylene terephthalate and aromatic hydroxycarboxylic acids.

[0050] Here, the aromatic hydroxycarboxylic acid, aromatic dicarboxylic acid, aromatic diol, aromatic hydroxyamine and aromatic diamine may be replaced with a part or all of them, respectively, by polymerizable derivatives thereof.

[0051] Examples of polymerizable derivatives of compounds having a carboxyl group, such as aromatic hydroxycarboxylic acids and aromatic dicarboxylic acids, include substances obtained by converting a carboxyl group into an alkoxycarbonyl group or an aryloxycarbonyl group (esters); substances obtained by converting a carboxyl group into a haloformyl group (acyl halides); substances obtained by converting a carboxyl group into an acyloxycarbonyl group (anhydrides), and the like.

[0052] Examples of polymerizable derivatives of compounds having a hydroxyl group, such as aromatic hydroxycarboxylic acids, aromatic diols, and aromatic hydroxyamines, include those in which the hydroxyl group is acylated and converted into an acyloxy group (acylate).

[0053] Examples of polymerizable derivatives of compounds having an amino group such as aromatic hydroxyamine and aromatic diamine include those obtained by acylation of the amino group and conversion into an acylamino group (acylate).

[0054] The first liquid crystal polyester resin in this embodiment preferably has a repeating unit represented by the following formula (1) (hereinafter, also referred to as "repeating unit (1)"), and more preferably has a repeating unit (1), a repeating unit represented by the following formula (2) (hereinafter, also referred to as "repeating unit (2)") and a repeating unit represented by the following formula (3) (hereinafter, also referred to as "repeating unit (3)").

[0055] -O-Ar 1 -CO- (1)

[0056] -CO-Ar 2 -CO- (2)

[0057] -X-Ar 3 -Y- (3)

[0058] [Wherein, Ar 1 Ar represents phenylene, naphthylene or biphenylene. 2and Ar 3 Each independently represents a phenylene group, a naphthylene group, a biphenylene group or a group represented by the following formula (4). X and Y each independently represent an oxygen atom or an imino group (-NH-). 1 ,Ar 2 or Ar 3 The hydrogen atoms in the groups represented by may be independently substituted by halogen atoms, alkyl groups or aryl groups.]

[0059] -Ar 4 -Z-Ar 5 -(4)

[0060] [where Ar 4 and Ar 5 Each independently represents a phenylene group or a naphthylene group. Z represents an oxygen atom, a sulfur atom, a carbonyl group, a sulfonyl group or an alkylene group.]

[0061] As can replace Ar 1 ,Ar 2 or Ar 3 Examples of the halogen atom having one or more hydrogen atoms in the group represented by include a fluorine atom, a chlorine atom, a bromine atom and an iodine atom.

[0062] As can replace by Ar 1 ,Ar 2 or Ar 3 The alkyl group having one or more hydrogen atoms in the group represented by alkyl includes methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-hexyl, 2-ethylhexyl, n-octyl, n-decyl and the like, and the number of carbon atoms thereof is preferably 1 to 10.

[0063] As can replace by Ar 1 ,Ar 2 or Ar 3 Examples of the aryl group having one or more hydrogen atoms in the group represented by include phenyl, o-tolyl, m-tolyl, p-tolyl, 1-naphthyl, 2-naphthyl and the like, and the number of carbon atoms thereof is preferably 6 to 20.

[0064] In the 1 ,Ar 2 or Ar 3 When a hydrogen atom in the group represented by is substituted with the above-mentioned group, the number of substitution is preferably 1 or 2, and more preferably 1.

[0065] Examples of the alkylene group in Z in formula (4) include methylene, ethylene, isopropylene, n-butylene, and 2-ethylhexylene, and the number of carbon atoms thereof is preferably 1 to 10.

[0066] The repeating unit (1) is a repeating unit derived from a predetermined aromatic hydroxycarboxylic acid. As the repeating unit (1), Ar 1 is a repeating unit of 1,4-phenylene (a repeating unit derived from p-hydroxybenzoic acid) and Ar 1 It is a repeating unit of 2,6-naphthylene (a repeating unit derived from 6-hydroxy-2-naphthoic acid).

[0067] It should be noted that the term “derived from” in the present specification means that in order to polymerize the raw material monomers, the chemical structure of the functional group that contributes to the polymerization is changed, and no other structural changes occur.

[0068] The repeating unit (2) is a repeating unit derived from a predetermined aromatic dicarboxylic acid. As the repeating unit (2), Ar 2 is a repeating unit of 1,4-phenylene (a repeating unit derived from terephthalic acid), Ar 2 is a repeating unit of 1,3-phenylene (a repeating unit derived from isophthalic acid), Ar 2 is a repeating unit of 2,6-naphthylene (derived from a repeating unit of 2,6-naphthalenedicarboxylic acid) and Ar 2 It is a repeating unit of diphenyl ether-4,4'-diyl (a repeating unit derived from diphenyl ether-4,4'-dicarboxylic acid).

[0069] The repeating unit (3) is a repeating unit derived from a predetermined aromatic diol, aromatic hydroxyamine or aromatic diamine. As the repeating unit (3), Ar 3 is a repeating unit of 1,4-phenylene (a repeating unit derived from hydroquinone, p-aminophenol or p-phenylenediamine) and Ar 3 It is a repeating unit of 4,4'-biphenylene (a repeating unit derived from 4,4'-dihydroxybiphenyl, 4-amino-4'-hydroxybiphenyl or 4,4'-diaminobiphenyl).

[0070] The content of the repeating unit (1) is preferably 30 mol% or more, more preferably 30 mol% or more and 80 mol% or less, further preferably 40 mol% or more and 70 mol% or less, and particularly preferably 45 mol% or more and 65 mol% or less, relative to the total amount of all repeating units (the value obtained by dividing the mass of each repeating unit constituting the liquid crystalline polyester resin by the formula weight of each repeating unit to obtain the material equivalent (molar) of each repeating unit, and adding these values ​​together).

[0071] The content of repeating unit (2) is preferably 35 mol% or less, more preferably 10 mol% or more and 35 mol% or less, further preferably 15 mol% or more and 30 mol% or less, and particularly preferably 17.5 mol% or more and 27.5 mol% or less, relative to the total amount of all repeating units.

[0072] The content of repeating unit (3) is preferably 35 mol% or less, more preferably 10 mol% or more and 35 mol% or less, further preferably 15 mol% or more and 30 mol% or less, and particularly preferably 17.5 mol% or more and 27.5 mol% or less, relative to the total amount of all repeating units.

[0073] When the first liquid crystal polyester resin in the present embodiment is composed of the above-mentioned repeating units (1) to (3), the sum of the content of the repeating unit (1) of the above-mentioned liquid crystal polyester, the content of the repeating unit (2) of the liquid crystal polyester and the content of the repeating unit (3) of the liquid crystal polyester does not exceed 100 mol%.

[0074] As the content of the repeating unit (1) increases, the melt fluidity, heat resistance, strength and rigidity tend to be improved. However, when the content is too large, the melt temperature or melt viscosity tends to increase, and the temperature required for molding tends to increase.

[0075] The ratio of the content of repeating unit (2) to the content of repeating unit (3), represented by [content of repeating unit (2)] / [content of repeating unit (3)] (mol / mol), is preferably 0.9 / 1 to 1 / 0.9, more preferably 0.95 / 1 to 1 / 0.95, and further preferably 0.98 / 1 to 1 / 0.98.

[0076] It should be noted that the first liquid crystal polyester resin in this embodiment may independently have two or more repeating units (1) to (3). In addition, the first liquid crystal polyester resin may have repeating units other than repeating units (1) to (3), but the content thereof is preferably 10 mol% or less, more preferably 5 mol% or less relative to the total amount of all repeating units.

[0077] The first liquid crystal polyester resin in the present embodiment has, as a repeating unit (3), a repeating unit in which X and Y are respectively oxygen atoms, that is, a repeating unit derived from a prescribed aromatic diol, which can easily reduce the melt viscosity. Therefore, it is preferred that, as a repeating unit (3), it is more preferred that only a repeating unit in which X and Y are respectively oxygen atoms be present.

[0078] The first thermoplastic resin in this embodiment is preferably produced by melt-polymerizing raw material monomers corresponding to the repeating units constituting the thermoplastic resin and solid-phase polymerizing the obtained polymer, thereby making it possible to produce a high molecular weight thermoplastic resin having high heat resistance or strength / rigidity with good operability.

[0079] Melt polymerization can be carried out in the presence of a catalyst. Examples of the catalyst include metal compounds such as magnesium acetate, stannous acetate, tetrabutyl titanate, lead acetate, sodium acetate, potassium acetate, antimony trioxide, and nitrogen-containing heterocyclic compounds such as 4-(dimethylamino)pyridine and 1-methylimidazole. Preferably, nitrogen-containing heterocyclic compounds are used.

[0080] The first thermoplastic resin in the present embodiment may be used alone or in combination of two or more.

[0081] The content of the first thermoplastic resin in the present embodiment is preferably 10 parts by mass or more, more preferably 20 parts by mass or more, and even more preferably 25 parts by mass or more, relative to the total amount (100 parts by mass) of the resin particles.

[0082] The content of the first thermoplastic resin in the present embodiment is preferably 80 parts by mass or less, more preferably 60 parts by mass or less, and even more preferably 45 parts by mass or less, based on the total amount (100 parts by mass) of the resin particles.

[0083] For example, the content of the first thermoplastic resin in the present embodiment is preferably 10 to 80 parts by mass, more preferably 20 to 60 parts by mass, and even more preferably 25 to 45 parts by mass, relative to the total amount (100 parts by mass) of the resin particles.

[0084] The content of the first thermoplastic resin in the present embodiment is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more, based on the total amount (100 parts by mass) of the resin composition in the present embodiment.

[0085] The content of the first thermoplastic resin in the present embodiment is preferably 60 parts by mass or less, more preferably 50 parts by mass or less, and even more preferably 40 parts by mass or less, based on the total amount (100 parts by mass) of the resin composition in the present embodiment.

[0086] For example, the content of the first thermoplastic resin in the present embodiment is preferably 5 to 60 parts by mass, more preferably 10 to 50 parts by mass, and even more preferably 15 to 40 parts by mass, based on the total amount (100 parts by mass) of the resin composition in the present embodiment.

[0087] Fiberglass

[0088] The type of glass fiber in this embodiment is not particularly limited, and known glass fibers can be used, for example, E glass (i.e., alkali-free glass), C glass (i.e., glass for acid-resistant purposes), AR glass (i.e., glass for alkali-resistant purposes), S glass or T glass, etc.

[0089] Among them, the glass fiber is preferably E glass.

[0090] Untreated glass fibers may be used, as well as treated glass fibers.

[0091] The treatment of the glass fiber can be performed using a convergent, a silane coupling agent, a boron compound, etc. Examples of the convergent include aromatic urethane convergents, aliphatic urethane convergents, and acrylic convergents.

[0092] The fineness of the glass fiber in the resin pellet in the present embodiment is 500 g / 1000 m or more, preferably 800 g / 1000 m or more.

[0093] The fineness of the glass fiber in the resin pellet in the present embodiment is 3400 g / 1000 m or less, preferably 2500 g / 1000 m or less, and more preferably 1500 g / 1000 m or less.

[0094] For example, the fineness of the glass fiber in the resin pellet in the present embodiment is preferably 800 g / 1000 m or more and 2500 g / 1000 m or less, and more preferably 800 g / 1000 m or more and 1500 g / 1000 m or less.

[0095] In this specification, "fineness" refers to the thickness of a bundle when glass fibers are aligned in one direction (the thickness of a fiber bundle).

[0096] Generally, the fiber orientation of injection molded products is layered, and they mainly have a three-layer structure: the center of the molded product (core layer), the layers located on both sides thereof (shell layers), and the surface layer of the molded product (skin layer).

[0097] When a plate-shaped molded product is injection molded using a film gate or the like provided on one side of the plate-shaped molded product, the fibers are oriented in the MD direction in the shell layer due to shear flow in the thickness direction, and are randomly or oriented in the TD direction in the core layer.

[0098] When the fineness of the glass fiber in the resin pellet is high, during the molding process, the glass fiber remains in the molded product as a fiber bundle in the resin pellet. Therefore, as the fineness in the resin pellet is higher, thicker fiber bundles remain in the molded product.

[0099] On the other hand, in the molding process, the glass fibers maintained in the fiber bundle state in the resin particles are oriented in the MD direction due to the shear flow in the thickness direction of the shell layer. Therefore, when the fineness of the glass fibers in the resin particles is too high, that is, when the fiber bundle of the glass fibers is too thick, the proportion of the shell layer of the glass fibers oriented in the MD direction increases, and the space for the core layer and the skin layer in which the glass fibers are randomly or oriented in the TD direction disappears. Therefore, the fiber orientation of the glass fibers in the MD direction is enhanced and the MDTD anisotropy of the strength of the molded body becomes larger.

[0100] That is, when the fineness range of the glass fiber in the resin particles is above the above-mentioned lower limit, during the molding process, since the glass fiber is still present in the molded body while maintaining the state of fiber bundles in the resin particles, the glass fiber remains in the molded body in the state of thicker fiber bundles, thereby further improving the mechanical strength (especially impact strength) of the molded body.

[0101] When the fineness of the glass fiber is below the upper limit, during the molding process, the orientation of the glass fiber in the MD direction is suppressed, and a core layer in which the glass fiber is randomly or oriented in the TD direction can be formed, thereby reducing the MDTD anisotropy of the mechanical strength of the molded body.

[0102] The fineness of the glass fibers in the resin pellets can be determined by taking out only the glass fibers in the resin pellets, measuring the weight and the number average fiber length, and calculating after the weight per number average fiber length of the glass fibers in the resin pellets is known.

[0103] Specifically, the calculation is performed according to the following steps.

[0104] Step (a): The weight of the resin particles per 100 resin particles was measured to 0.1 mg unit using a precision balance. Thereafter, the resin particles were heated at 600° C. for 4 hours using a muffle furnace to remove the resin portion (first thermoplastic resin).

[0105] Step (b): remove the resin part from the resin particles, take out the material that is only glass fiber, and measure the total weight A of glass fiber to 0.1 mg unit with a precision balance. Thereafter, the glass fiber having measured the total weight is dispersed in 1000 mL of an aqueous solution to which 0.05 volume % surfactant (Micro90, made by International Products Corporation) is added to prepare a glass fiber dispersion.

[0106] Step (c): 100 mL was taken out from the dispersion and diluted 5 to 20 times with pure water. 50 mL was taken out from the diluted dispersion and dispersed in a culture dish. Then, the glass fibers dispersed in the culture dish were observed using a microscope (VH-Z25, manufactured by KEYENCE, with a magnification of 10 to 20 times), and 10 pieces were photographed in a manner that the photographed areas did not overlap.

[0107] Step (d): Use the measuring tool of the microscope to measure the length of all glass fibers present in one of the captured images. It should be noted that the bent glass fibers are measured by multi-point measurement, and the fibers in contact with the edge of the image are not measured. The same operation is performed in the 10 captured images in sequence until the total number of glass fibers measured exceeds 500 to determine the fiber length of the glass fibers. When the total number of glass fibers in the 10 captured images does not exceed 500, return to step (c), retake the image and measure the fiber length again based on the appropriately adjusted dilution ratio with pure water.

[0108] Step (e): From the fiber length of the glass fiber measured in step (d), calculate the number average fiber length Lm = (ΣLi×ni) / Σni, (Σni>500).

[0109] Li: Fiber length of glass fiber.

[0110] ni: The number of glass fibers with fiber length Li.

[0111] Step (f): The fineness can be calculated based on 100 resin pellets used to measure the total weight A of the glass fibers obtained in step (b) and the number average fiber length Lm of the glass fibers obtained in step (e).

[0112] Fineness (unit: g / 1000m) = 1000 × 1000 (unit: m) / Lm (unit: mm) × A (unit: g) / 100

[0113] The length-weighted average fiber length of the glass fibers in the resin particles in the present embodiment is preferably 4 mm or more, more preferably 4.5 mm or more, further preferably 5 mm or more, particularly preferably 6 mm or more, and most preferably 7 mm or more.

[0114] On the other hand, the length-weighted average fiber length of the glass fiber is preferably less than 50 mm, more preferably 40 mm or less, further preferably 20 mm or less, and particularly preferably 15 mm or less.

[0115] For example, the length-weighted average fiber length of the glass fiber is preferably 4 mm or more and less than 50 mm, more preferably 4.5 mm or more and 40 mm or less, further preferably 5 mm or more and 20 mm or less, further preferably 5.5 mm or more and 15 mm or less, and particularly preferably 6 mm or more and 15 mm or less.

[0116] When the length-weighted average fiber length of the glass fibers is at least the lower limit of the preferred range, the strength of the molded product is further improved. On the other hand, when it is at most the upper limit of the preferred range, molding is easier.

[0117] In this embodiment, the fiber length and the length-weighted average fiber length of the glass fibers are measured in the following steps.

[0118] Step (1): 2 g of the resin pellets were heated at 600° C. for 4 hours in a muffle furnace to remove the resin portion (first thermoplastic resin).

[0119] Step (2): The resin portion is removed from the resin particles, and the glass fiber-only substance is dispersed in 1000 mL of an aqueous solution to which 0.05% by volume of a surfactant (Micro90, manufactured by INTERNATIONAL PRODUCTS CORPORATION) is added to prepare a glass fiber dispersion.

[0120] Step (3): Take 100 mL of the dispersion and dilute it 5 to 20 times with pure water. Take 50 mL of the diluted dispersion and disperse it in a culture dish. Then, observe the glass fibers dispersed in the culture dish using a microscope (VH-Z25, manufactured by KEYENCE, magnification 10 to 20 times), and take 10 images of each sample in a manner that the shooting areas do not overlap.

[0121] Step (4): Use the microscope's measuring tool to measure the length of all glass fibers present in one of the captured images. It should be noted that the bent glass fibers are measured by multi-point measurement, and the fibers that are in contact with the edge of the image are not measured. The same operation is performed in the 10 captured images in sequence until the total number of measured glass fibers exceeds 500 to measure the fiber length. If the total number of measured glass fibers in the 10 captured images does not exceed 500, return to step (3), retake the image and measure the fiber length again based on appropriately adjusting the dilution ratio with pure water.

[0122] Step (5): From the fiber length of the glass fiber measured in step (4), calculate the length-weighted average fiber length lm = (Σli 2 ×ni) / (Σli×ni), (Σni>500).

[0123] li: fiber length of glass fiber.

[0124] ni: The number of glass fibers with fiber length li.

[0125] The number average fiber diameter of the glass fibers in the resin particles is preferably 5 μm or more, more preferably 10 μm or more.

[0126] The number average fiber diameter of the glass fibers in the resin pellets is preferably 35 μm or less, more preferably 25 μm or less, and even more preferably 20 μm or less.

[0127] For example, the number average fiber diameter of the glass fibers in the resin particles is preferably 5 to 35 μm, more preferably 10 to 25 μm, and further preferably 10 to 20 μm.

[0128] When the number average fiber diameter of the glass fibers in the resin particles is equal to or larger than the lower limit of the above preferred range, the glass fibers are easily dispersed in the resin particles.

[0129] On the other hand, when the content is below the upper limit of the preferred range, the glass fibers can efficiently reinforce the molded body, thereby further improving the strength of the molded body.

[0130] The number average fiber diameter of the glass fibers in the resin particles can be determined, for example, by removing the resin portion by the same method as in step (1) for determining the fiber length and length-weighted average fiber length of the glass fibers, observing the obtained glass fibers with a scanning electron microscope (1000 times), and measuring the number average value of the fiber diameters of 500 randomly selected glass fibers.

[0131] The resin pellets in the present embodiment preferably have 100 parts by mass of the first thermoplastic resin impregnated in 80 parts by mass or more of the glass fibers, more preferably 100 parts by mass or more of the glass fibers, and even more preferably 120 parts by mass or more of the glass fibers.

[0132] In the resin pellets of the present embodiment, preferably 100 parts by mass of the first thermoplastic resin is impregnated in 260 parts by mass or less of the glass fiber, more preferably 250 parts by mass or less of the glass fiber, and even more preferably 240 parts by mass or less of the glass fiber.

[0133] For example, the resin pellets in the present embodiment preferably contain 100 parts by mass of the first thermoplastic resin impregnated in 80 to 260 parts by mass of glass fibers, more preferably 100 to 250 parts by mass of glass fibers, and even more preferably 120 to 240 parts by mass of glass fibers.

[0134] When the mass ratio of the first thermoplastic resin to the glass fiber is above the lower limit of the preferred range, the strength of the molded product is further improved. On the other hand, when it is below the upper limit of the preferred range, the fiber bundle is easily opened and the glass fiber is impregnated with the first thermoplastic resin.

[0135] In the resin composition of this embodiment, the content of the glass fiber is preferably more than 35 parts by mass, more preferably 40 parts by mass or more, and further preferably 45 parts by mass or more, relative to the total amount (100 parts by mass) of the resin particles and the second thermoplastic resin.

[0136] In addition, in the resin composition of this embodiment, the content of the above-mentioned glass fiber is preferably less than 65 parts by mass, more preferably 60 parts by mass or less, and further preferably 55 parts by mass or less, relative to the total amount (100 parts by mass) of the resin particles and the second thermoplastic resin.

[0137] For example, in the resin composition of the present embodiment, the content of the above-mentioned glass fiber is preferably greater than 35 parts by mass and less than 65 parts by mass, more preferably greater than 40 parts by mass and less than 60 parts by mass, and further preferably greater than 45 parts by mass and less than 55 parts by mass, relative to the total amount (100 parts by mass) of the resin particles and the second thermoplastic resin.

[0138] When the content of the glass fiber is equal to or less than the above preferred upper limit, moldability is improved.

[0139] When the content of the glass fiber is equal to or more than the above preferred lower limit, the strength of the molded product can be further improved.

[0140] The content of the glass fiber in the present embodiment is preferably 20 parts by mass or more, more preferably 30 parts by mass or more, and even more preferably 40 parts by mass or more, based on the total amount (100 parts by mass) of the resin composition in the present embodiment.

[0141] The content of the glass fiber in the present embodiment is preferably 70 parts by mass or less, more preferably 65 parts by mass or less, and even more preferably 60 parts by mass or less, based on the total amount (100 parts by mass) of the resin composition in the present embodiment.

[0142] For example, the content of the glass fiber in the present embodiment is preferably 20 to 70 parts by mass, more preferably 30 to 65 parts by mass, and even more preferably 40 to 60 parts by mass, based on the total amount (100 parts by mass) of the resin composition in the present embodiment.

[0143] <Second thermoplastic resin>

[0144] Examples of the second thermoplastic resin in the present embodiment include the same ones as those listed above for the first thermoplastic resin, and the second thermoplastic resin has a flow start temperature lower than that of the resin particles.

[0145] The flow start temperature of the second thermoplastic resin in the present embodiment is preferably 250° C. or higher, more preferably 260° C. or higher.

[0146] In addition, the flow start temperature of the second thermoplastic resin in the present embodiment is preferably 400° C. or lower, and more preferably 380° C. or lower.

[0147] For example, the flow start temperature of the second thermoplastic resin in the present embodiment is preferably 250°C to 400°C, more preferably 260°C to 400°C, and further preferably 260°C to 380°C.

[0148] There is a tendency that the higher the flow start temperature of the second thermoplastic resin is, the higher the heat resistance and strength of a molded body produced using a resin composition containing the second thermoplastic resin are.

[0149] On the other hand, when the flow start temperature of the second thermoplastic resin exceeds 400° C., the melting temperature or melt viscosity of the second thermoplastic resin tends to increase. Therefore, the temperature required for molding the resin composition containing the second thermoplastic resin tends to increase.

[0150] In the resin composition of this embodiment, the difference in flow start temperature between the resin particles and the second thermoplastic resin (flow start temperature of the resin particles - flow start temperature of the second thermoplastic resin) is preferably 10°C or more, more preferably more than 10°C, further preferably 15°C or more, and particularly preferably 25°C or more.

[0151] By making the difference between the flow start temperature of the resin pellets and the second thermoplastic resin equal to or greater than the above-mentioned preferred lower limit, the resin pellets are less likely to melt even at a molding temperature at which the second thermoplastic resin is sufficiently molten during the processing until the molded body is produced. Therefore, the glass fibers contained in the resin pellets can be further maintained in a bundle state and the residual glass fibers can be relatively long, thereby improving the strength of the molded body.

[0152] In addition, the upper limit of the difference between the flow start temperature of the resin pellet and the second thermoplastic resin is not particularly limited, and is, for example, 40°C.

[0153] For example, the difference in flow start temperature between the resin pellets and the second thermoplastic resin is preferably 10°C to 40°C, more preferably more than 10°C to 40°C, further preferably 15°C to 40°C, further more preferably 20°C to 40°C, particularly preferably 25°C to 40°C, and most preferably 28°C to 40°C.

[0154] As the second thermoplastic resin in the present embodiment, among those listed above for the first thermoplastic resin, a liquid crystal polyester resin (hereinafter, also referred to as a "second liquid crystal polyester resin") is preferable.

[0155] That is, in the resin composition of this embodiment, it is preferred that both the first thermoplastic resin and the second thermoplastic resin are liquid crystal polyester resins. It should be noted that the flow start temperature of the second liquid crystal polyester resin is lower than that of the first liquid crystal polyester resin (resin particles containing the first liquid crystal polyester resin).

[0156] For example, it is preferred that the flow start temperature of the resin particles in the present embodiment is 300° C. to 400° C., and the flow start temperature of the second thermoplastic resin is 250° C. to less than 290° C., it is more preferred that the flow start temperature of the resin particles in the present embodiment is 300° C. to 380° C., and the flow start temperature of the second thermoplastic resin is 260° C. to less than 290° C., it is further preferred that the flow start temperature of the resin particles in the present embodiment is 300° C. to 325° C., and the flow start temperature of the second thermoplastic resin is 270° C. to less than 290° C.

[0157] Specific examples of the second liquid crystal polyester resin include liquid crystal polyester resins having the same repeating unit (1) as the first liquid crystal polyester resin.

[0158] By appropriately selecting the types of raw material monomers or the contents of the respective repeating units described above for the first liquid crystal polyester resin and adjusting the molecular weight, it is possible to produce a second liquid crystal polyester resin having a flow start temperature lower than that of the resin particles.

[0159] The second liquid crystal polyester resin in the present embodiment may be used alone or in combination of two or more.

[0160] The content of the second thermoplastic resin in the present embodiment is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more, based on the total amount (100 parts by mass) of the resin particles and the second thermoplastic resin.

[0161] The content of the second thermoplastic resin in the present embodiment is preferably 50 parts by mass or less, more preferably 45 parts by mass or less, and even more preferably 40 parts by mass or less, based on the total amount (100 parts by mass) of the resin particles and the second thermoplastic resin.

[0162] For example, the content of the second thermoplastic resin in the present embodiment is preferably 5 to 50 parts by mass, more preferably 10 to 45 parts by mass, and even more preferably 15 to 40 parts by mass, based on the total amount (100 parts by mass) of the resin particles and the second thermoplastic resin.

[0163] When the content of the second thermoplastic resin is equal to or less than the above preferred upper limit, the strength of the molded product can be further improved.

[0164] When the content of the second thermoplastic resin is equal to or more than the above preferred lower limit, moldability is improved.

[0165] The content of the second thermoplastic resin in the present embodiment is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more, based on the total amount (100 parts by mass) of the resin composition in the present embodiment.

[0166] The content of the second thermoplastic resin in the present embodiment is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, and even more preferably 30 parts by mass or less, based on the total amount (100 parts by mass) of the resin composition in the present embodiment.

[0167] For example, the content of the second thermoplastic resin in the present embodiment is preferably 5 to 50 parts by mass, more preferably 10 to 40 parts by mass, and even more preferably 15 to 30 parts by mass, based on the total amount (100 parts by mass) of the resin composition in the present embodiment.

[0168] <Other ingredients>

[0169] The resin composition of the present embodiment may contain, in addition to the above-mentioned resin particles and the second thermoplastic resin, one or more higher fatty acid metal salts, other fillers, additives, and the like as necessary.

[0170] Specific examples of the higher fatty acid metal salt include lithium laurate, calcium laurate, barium laurate, lithium stearate, barium stearate, sodium stearate, potassium stearate, calcium stearate, aluminum stearate, magnesium behenate, calcium behenate, and barium behenate.

[0171] Among them, calcium behenate, magnesium behenate, and calcium stearate are preferred, and magnesium behenate is more preferred, because they have relatively low melting points and can be molded at lower temperatures.

[0172] The content of the higher fatty acid metal salt in the present embodiment is preferably 0.01 parts by mass or more, and more preferably 0.02 parts by mass or more, based on the total amount (100 parts by mass) of the resin particles and the second thermoplastic resin.

[0173] The content of the higher fatty acid metal salt in the present embodiment is preferably 0.15 parts by mass or less, and more preferably 0.08 parts by mass or less, based on the total amount (100 parts by mass) of the resin particles and the second thermoplastic resin.

[0174] For example, the content of the higher fatty acid metal salt in the present embodiment is preferably 0.01 to 0.15 parts by mass, and more preferably 0.02 to 0.08 parts by mass, based on the total amount (100 parts by mass) of the resin particles and the second thermoplastic resin.

[0175] When the content of the higher fatty acid metal salt is equal to or greater than the above preferred lower limit, the strength of the molded product (particularly the impact strength) is further improved. In addition, the moldability is further improved.

[0176] When the content of the higher fatty acid metal salt is below the above preferred upper limit, the strength of the molded product (especially bending strength and tensile strength) is suppressed from decreasing. In addition, there is a tendency that contamination of the mold used or foaming of the molded product is less likely to occur.

[0177] The content of the higher fatty acid metal salt in the present embodiment is preferably 0.02 parts by mass or more relative to the total amount (100 parts by mass) of the resin composition in the present embodiment.

[0178] The content of the higher fatty acid metal salt in the present embodiment is preferably 0.15 parts by mass or less, more preferably 0.12 parts by mass or less, and even more preferably 0.08 parts by mass or less, based on the total amount (100 parts by mass) of the resin composition in the present embodiment.

[0179] For example, the content of the higher fatty acid metal salt in the present embodiment is preferably 0.02 to 0.15 parts by mass, more preferably 0.02 to 0.12 parts by mass, and even more preferably 0.02 to 0.08 parts by mass, based on the total amount (100 parts by mass) of the resin composition in the present embodiment.

[0180] As other fillers, plate-like fillers, spherical fillers or other granular fillers may be used. Other fillers may be inorganic fillers or organic fillers.

[0181] Examples of the plate-like inorganic filler include talc, mica, graphite, wollastonite, glass flakes, barium sulfate, and calcium carbonate. The mica may be muscovite, phlogopite, fluorophlogopite, or tetrasilicon mica.

[0182] Examples of the particulate inorganic filler include silica, alumina, titanium oxide, glass beads, glass balloons, boron nitride, silicon carbide, and calcium carbonate.

[0183] Examples of additives include flame retardants, conductivity imparting agents, crystal nuclei, ultraviolet absorbers, antioxidants, vibration damping agents, antibacterial agents, insect repellents, deodorants, anti-coloring agents, heat stabilizers, mold release agents, antistatic agents, plasticizers, lubricants, colorants, pigments, dyes, foaming agents, foam suppressants, viscosity modifiers, and surfactants.

[0184] The resin composition of the present embodiment reduces the MDTD anisotropy of the strength of the molded body by the above-mentioned constitution. Therefore, for the resin composition of the present embodiment, when a Charpy impact strength test (with a notch) is performed on a molded body having a width of 10 mm×a length of 80 mm×a thickness of 4 mm produced by injection molding using the above-mentioned resin composition, the impact strength in the MD direction (MD i ) and TD direction impact strength (TD i ) ratio (TD i / MD i ) is preferably greater than 0.5, more preferably greater than 0.7, and even more preferably greater than 0.8.

[0185] That is, a resin composition according to one embodiment of the present embodiment is a resin composition comprising resin pellets containing a first thermoplastic resin and glass fibers and a second thermoplastic resin, wherein when a Charpy impact strength test (with a notch) is performed on a molded body having a size of 10 mm in width × 80 mm in length × 4 mm in thickness produced by injection molding using the resin composition, the impact strength in the MD direction (MD i ) and TD direction impact strength (TD i ) ratio (TD i / MD i ) is greater than 0.5.

[0186] The resin composition of the present embodiment contains resin pellets and a second thermoplastic resin, the second thermoplastic resin has a flow start temperature lower than that of the resin pellets, and the fineness of the glass fiber in the resin pellets is 500 g / 1000 m or more and 3400 g / 1000 m or less.

[0187] Among them, in the resin composition of this embodiment, the difference between the flow start temperature of the resin particles and the second thermoplastic resin (flow start temperature of the resin particles-flow start temperature of the second thermoplastic resin) is greater than 10°C, and the fineness of the glass fiber in the resin particles is preferably greater than 800g / 1000m and less than 2500g / 1000m.

[0188] In addition, in the resin composition of the present embodiment, the difference in flow start temperature between the resin particles and the second thermoplastic resin (flow start temperature of the resin particles - flow start temperature of the second thermoplastic resin) exceeds 10°C, and the fineness of the glass fiber in the resin particles is more preferably greater than 800 g / 1000 m and less than 1500 g / 1000 m.

[0189] In addition, in the resin composition of the present embodiment, the difference between the flow start temperature of the resin particles and the second thermoplastic resin (flow start temperature of the resin particles - flow start temperature of the second thermoplastic resin) is greater than 15°C, and the fineness of the glass fiber in the resin particles is further preferably greater than 800 g / 1000 m and less than 1500 g / 1000 m.

[0190] In addition, in the resin composition of the present embodiment, the difference between the flow start temperature of the resin particles and the second thermoplastic resin (flow start temperature of the resin particles - flow start temperature of the second thermoplastic resin) is greater than 25°C, and the fineness of the glass fiber in the resin particles is particularly preferably greater than 800 g / 1000 m and less than 1500 g / 1000 m.

[0191] In addition, for example, in the resin composition of the present embodiment, the difference between the flow start temperature of the resin particles and the second thermoplastic resin (flow start temperature of the resin particles - flow start temperature of the second thermoplastic resin) is greater than 27°C, and the fineness of the glass fiber in the resin particles can be greater than 1180g / 1000m and less than 2300g / 1000m.

[0192] As described above, the resin composition of the present embodiment contains resin particles and a second thermoplastic resin. In addition, the fineness of the glass fiber contained in the resin particles is 500g / 1000m or more and 3400g / 1000m or less. That is, it is speculated that in the present embodiment, by making the fineness of the glass fiber contained in the resin particles within a specific range, the resin particles and the second thermoplastic resin with different flow start temperatures are used in parallel to reduce the breakage of the glass fiber contained in the resin particles during molding and suppress the orientation of the glass fiber along the MD direction, thereby reducing the MDTD anisotropy of the strength of the molded body.

[0193] The present invention has the following aspects.

[0194] [1] A resin composition comprising: resin pellets containing a first thermoplastic resin and glass fibers; and a second thermoplastic resin, wherein the fineness of the glass fibers in the resin pellets is greater than or equal to 500 g / 1000 m and less than or equal to 3400 g / 1000 m, the flow start temperatures of the resin pellets and the second thermoplastic resin are both greater than or equal to 250° C. and less than or equal to 400° C., and the difference in flow start temperature between the resin pellets and the second thermoplastic resin (flow start temperature of the resin pellets minus flow start temperature of the second thermoplastic resin) is greater than or equal to 10° C. and less than or equal to 40° C.

[0195] [2] The resin composition according to [1], wherein the resin pellets are preferably prepared by impregnating 80 to 260 parts by mass of glass fibers with 100 parts by mass of the first thermoplastic resin, more preferably 100 to 250 parts by mass of glass fibers, and even more preferably 120 to 240 parts by mass of glass fibers; the content of the glass fibers is preferably more than 35 parts by mass and less than 65 parts by mass, more preferably 40 parts by mass to 60 parts by mass, and even more preferably 45 parts by mass to 55 parts by mass, relative to the total amount (100 parts by mass) of the resin pellets and the second thermoplastic resin; and the content of the second thermoplastic resin is preferably 5 to 50 parts by mass, more preferably 10 to 45 parts by mass, and even more preferably 15 to 40 parts by mass, relative to the total amount (100 parts by mass) of the resin pellets and the second thermoplastic resin.

[0196] [3] The resin composition as described in [1] or [2], wherein the length-weighted average fiber length of the glass fiber is preferably 4 mm or more and less than 50 mm, more preferably 4.5 mm or more and 40 mm or less, further preferably 5 mm or more and 20 mm or less, further preferably 5.5 mm or more and 15 mm or less, and particularly preferably 6 mm or more and 15 mm or less.

[0197] [4] The resin composition according to any one of [1] to [3], wherein the number average fiber diameter of the glass fiber is preferably 5 to 35 μm, more preferably 10 to 25 μm, and even more preferably 10 to 20 μm.

[0198] [5] The resin composition as described in [1], wherein when a Charpy impact strength test (with notch) is performed on a molded body having a width of 10 mm × a length of 80 mm × a thickness of 4 mm produced by injection molding using the resin composition, the ratio (TDi / MDi) of the impact strength in the MD direction (MDi) to the impact strength in the TD direction (TDi) is preferably 0.5 or more, more preferably 0.7 or more, and even more preferably 0.8 or more.

[0199] (Method for producing resin composition)

[0200] The resin composition of the present embodiment can be produced by mixing the above-mentioned resin pellets, the second thermoplastic resin, and other components as necessary.

[0201] [Method for producing resin pellets]

[0202] The method for producing the resin pellets in the present embodiment includes, for example, melt-kneading the first thermoplastic resin and other components as required, impregnating the obtained melt into glass fibers, and pelletizing to obtain the resin pellets.

[0203] Figure 1 One embodiment of a resin pellet production apparatus is shown.

[0204] exist Figure 1 In the present embodiment shown, a case where the resin pellets 15 are obtained by using the fiber roving 10 in which the fiber bundle 11 formed by a plurality of glass fibers being converged by a convergent is wound into a roll shape is described.

[0205] like Figure 1 As shown, the manufacturing apparatus 100 includes a preheating unit 121 , an impregnation unit 123 , a cooling unit 125 , a pulling unit 127 , a cutting unit 129 , and conveying rollers 101 to 109 . Figure 1 In the manufacturing apparatus 100 shown, the impregnation unit 123 is connected to the extruder 120 .

[0206] exist Figure 1 , a state where the fiber bundle 11 is continuously fed out from the fiber roving 10 is shown. In the present embodiment, the resin pellets 15 are produced while the fiber bundle 11 fed out from the fiber roving 10 is fed in the longitudinal direction by the feed rollers 101 to 109.

[0207] The fineness of the fiber roving 10 used for producing the resin pellets of the present embodiment is 500 g / 1000 m to 3400 g / 1000 m, preferably 800 g / 1000 m to 3200 g / 1000 m, and more preferably 800 g / 1000 m to 2400 g / 1000 m.

[0208] When the fineness of the fiber roving 10 is equal to or larger than the lower limit of the preferred range, the fiber roving 10 can be easily handled in the method for producing the resin pellet.

[0209] When the fineness of the fiber roving 10 is equal to or smaller than the upper limit of the preferred range, the fiber can be easily dispersed in the first thermoplastic resin and can be easily handled when producing the resin pellet.

[0210] The number average fiber diameter of the fiber roving 10 is preferably 5 to 35 μm, more preferably 10 to 25 μm, and even more preferably 10 to 20 μm.

[0211] The number average fiber diameter of the fiber roving 10 is a number average value obtained by observing the glass fibers using a scanning electron microscope (1000 times) and measuring the fiber diameters of 500 randomly selected glass fibers.

[0212] When the number average fiber diameter of the fiber roving 10 is above the lower limit of the preferred range, the glass fiber is easily dispersed in the resin pellets. In addition, the glass fiber is easy to handle when the resin pellets are manufactured. On the other hand, when it is below the upper limit of the preferred range, the glass fiber efficiently reinforces the molded body. Therefore, the strength of the molded body can be improved.

[0213] In the present embodiment, the fiber roving 10 treated with a convergent (sizing agent) is used. Glass fibers that have been appropriately sizing-treated have better productivity and quality stability during pellet production and can reduce variations in physical properties of molded products.

[0214] The astringent (sizing agent) is not particularly limited, and for example, nylon polymers, polyether polymers, epoxy polymers, ester polymers, urethane polymers, mixed polymers thereof, or modified polymers thereof can be cited. In addition, known coupling agents such as so-called silane coupling agents such as aminosilane and epoxysilane, and titanium coupling agents can also be used.

[0215] In the glass fiber used in the resin pellet of this embodiment, the single fibers do not necessarily need to be arranged in one direction. From the viewpoint of productivity in the process of manufacturing the molding material, it is preferred that the single fibers are arranged in one direction and the fiber bundles are continuous in the longitudinal direction of the fibers.

[0216] The number of filaments in the fiber roving 10 is preferably 1000 to 10000, more preferably 1000 to 8000, and even more preferably 1500 to 6000, from the viewpoint of improving economic efficiency and impregnation properties.

[0217] The fiber bundle 11 fed from the fiber roving 10 is heated and dried in the preheating section 121. The heating temperature is not particularly limited, and is, for example, 50 to 250° C. The heating time in the preheating section 121 is not particularly limited, and is, for example, 3 to 30 seconds.

[0218] In the impregnation section 123 , the fiber bundle 11 is impregnated with the molding material M (the first thermoplastic resin and other components blended as needed) other than the fiber bundle 11 .

[0219] As described later, the first thermoplastic resin is appropriately selected in consideration of the type, melt viscosity, flow start temperature, and the like of the second thermoplastic resin.

[0220] The first thermoplastic resin may be used alone or in combination of two or more.

[0221] The fiber bundle 11 may be impregnated with a melt obtained by feeding the molding material M from the supply port 123 a and heating it in the impregnation section 123 , or the molding material M melt-kneaded by the extruder 120 may be fed from the supply port 123 a and impregnated with the fiber bundle 11 .

[0222] In addition, Figure 1 In the illustrated embodiment, the resin structure 13 in which the fiber bundle 11 is impregnated with and coated with the melt is obtained.

[0223] The heating temperature in the impregnation part 123 is appropriately determined according to the type of the first thermoplastic resin, and is preferably set to a temperature 10 to 80° C. higher than the flow start temperature of the first thermoplastic resin used, for example, 300 to 400° C.

[0224] In the impregnation portion 123, depending on the properties required for the molded body, etc., it is preferred that 100 parts by mass of the first thermoplastic resin be impregnated into 80 to 260 parts by mass of glass fibers (fiber bundles 11), more preferably into 100 to 250 parts by mass of glass fibers, and even more preferably into 120 to 240 parts by mass of glass fibers.

[0225] When the amount of glass fiber blended is above the lower limit of the preferred range, the strength of the molded product is further improved. On the other hand, when it is below the upper limit of the preferred range, the fiber bundle is easily opened and the first thermoplastic resin is impregnated into the fiber bundle.

[0226] By changing the nozzle diameter of the die at the outlet of the impregnation section 123 according to the diameter of the fiber bundle 11 , the blending ratio of the first thermoplastic resin and the glass fiber in the resin structure 13 can be adjusted.

[0227] In the cooling section 125 , the resin structure 13 heated in the impregnation section 123 (the resin structure 13 in which the fiber bundle is impregnated with the melt) is cooled, for example, to 50 to 150° C. The cooling time is not particularly limited, and is, for example, 3 to 30 seconds.

[0228] In the pulling section 127 , the resin structure 13 cooled in the cooling section 125 is continuously pulled and sent to the subsequent cutting section 129 .

[0229] In the cutting unit 129, the cooled resin structure 13 is cut into desired lengths to produce resin pellets 15. The cutting unit 129 includes, for example, a rotary blade or the like.

[0230] Using the above-described production apparatus 100 , as the resin pellets of the present embodiment, pellets in which glass fibers are fixed by the first thermoplastic resin are produced, for example, as follows.

[0231] A step of obtaining a resin structure.

[0232] While a fiber bundle 11 in which a plurality of single fibers are converged by a convergent is continuously fed out from the fiber roving 10 , the fiber bundle 11 is first heated and dried by the preheating unit 121 .

[0233] Next, while the dried fiber bundle 11 is supplied to the impregnation section 123, the molding material M melt-kneaded by the extruder 120 is introduced from the supply port 123a, and the molten molding material M is impregnated into the fiber bundle 11. Thus, the resin structure 13 in which the fiber bundle is impregnated and coated with the melt is obtained. Thereafter, the resin structure 13 in the state heated in the impregnation section 123 is cooled by the cooling section 125.

[0234] In the resin structure 13 obtained here, the fibers are arranged substantially in parallel along the longitudinal direction of the resin structure 13 .

[0235] “The fibers are arranged substantially parallel to the longitudinal direction of the resin structure” means that the angle between the longitudinal direction of the fibers and the longitudinal direction of the resin structure is substantially 0°, specifically, the angle between the longitudinal directions of the fibers and the resin structure is -5° to 5°.

[0236] The process of obtaining particles.

[0237] Next, the cooled resin structure 13 is pulled out into a strand shape by the pulling unit 127 and sent out to the cutting unit 129 .

[0238] Next, in the cutting unit 129 , the strand-shaped resin structure 13 is cut into predetermined lengths along the longitudinal direction thereof to obtain resin pellets 15 .

[0239] The predetermined length of the resin pellet 15 mentioned here is the length of the resin pellet 15 set according to the required performance of the molded body made of the resin pellet 15. In the resin pellet obtained by the manufacturing method of this embodiment, the length of the resin pellet 15 is substantially the same as the length of the fibers arranged in the resin pellet 15.

[0240] “The length of the pellet and the length of the fibers are substantially the same length” means that the length-weighted average fiber length of the fibers arranged in the pellet is 95 to 105% of the length in the longitudinal direction of the pellet.

[0241] As described above, resin pellets (resin pellets 15 ) containing the first thermoplastic resin and glass fibers are produced.

[0242] The resin pellets 15 are pellets in which glass fibers are fixed by a first thermoplastic resin, and the glass fibers are arranged substantially in parallel along the length direction of the pellets. In addition, the length of the glass fibers arranged in the resin pellets 15 is substantially the same as the length of the pellets. The length of the resin pellets 15 manufactured in this embodiment depends on the required performance of the molded body made of the resin pellets 15, and is, for example, 3 to 50 mm.

[0243] In this way, the glass fibers are arranged roughly in parallel along the length direction of the particle, and the length of the glass fibers is substantially the same as the length of the particle. Therefore, when it is used as an injection molded product, for example, the residual glass fibers in the injection molded product can be lengthened, thereby having the effect of improving the strength of the molded product, improving the heat resistance and alleviating the anisotropy.

[0244] The arrangement direction of the glass fibers in the resin pellet can be confirmed by observing a cross section of the resin pellet cut along the length direction with a microscope.

[0245] As the length of the glass fibers in the resin pellets, the length-weighted average fiber length determined by the same procedure as the measurement of the fiber length of the glass fibers in the resin pellets described above is used.

[0246] [Method for producing second resin particles]

[0247] For the second thermoplastic resin, a mixture of the second thermoplastic resin and other components as needed can be pelletized by melt extrusion molding or melt compression molding to produce particles containing the second thermoplastic resin (second resin particles). In addition, the difference in particle length between the second resin particles and the resin particles 15 is preferably 15 mm or less, more preferably 5 mm or less.

[0248] The smaller the difference in particle length between the second resin particles and the resin particles 15 is, the more effective it is in reducing the strength variation and the filling amount variation of the glass fiber of a molded body produced using a resin composition containing the second resin particles and the resin particles 15 .

[0249] In the manufacturing method of this embodiment, all the components may be added before mixing, some of the components may be added sequentially while mixing, or all the components may be added sequentially while mixing. That is, the resin particles and the second thermoplastic resin may be mixed first, and a higher fatty acid metal salt may be added to the mixture of the resin particles and the second thermoplastic resin as required. In addition, a higher fatty acid metal salt may be added to the resin particles coated with the second thermoplastic resin as required.

[0250] (Molding body)

[0251] The molded product of the present embodiment is a molded product produced using the above-mentioned resin composition.

[0252] The molded body of the present embodiment can be obtained by a known molding method using a resin composition. As the molding method of the resin composition of the present embodiment, a melt molding method is preferred, and as an example, extrusion molding methods such as injection molding, T-die method or inflation method, compression molding, blow molding, vacuum molding and press molding can be cited. Among them, injection molding is preferred.

[0253] For example, when the resin composition is used as a molding material and molded by injection molding, the resin composition is melted using a known injection molding machine and the molten resin composition is injected into a mold for molding.

[0254] Here, when the resin composition is fed into the injection molding machine, each component (resin pellets, second thermoplastic resin, etc.) may be fed into the injection molding machine separately, or a part or all of the components may be mixed in advance and fed into the injection molding machine as a mixture.

[0255] Examples of known injection molding machines include TR450EH3 manufactured by Sodick Co., Ltd. and hydraulic horizontal molding machine PS40E5ASE manufactured by Nissei Plastics Industries, Ltd.

[0256] The temperature conditions for injection molding are appropriately determined according to the type of thermoplastic resin, and the cylinder temperature of the injection molding machine is preferably set to a temperature 10 to 80° C. higher than the flow start temperature of the thermoplastic resin used.

[0257] For example, the melt kneading temperature (plasticization part) is preferably higher than the flow start temperature of the second thermoplastic resin and lower than the flow start temperature of the first thermoplastic resin or the resin particles. Specifically, the melt kneading temperature (plasticization part) is preferably 250 to 350°C, more preferably 260 to 340°C, and further preferably 270 to 320°C.

[0258] The temperature of the measuring portion or the plunger portion is preferably 280 to 400°C, more preferably 290 to 380°C, and even more preferably 300 to 370°C.

[0259] The temperature of the mold is preferably set to a range of room temperature (eg, 23° C.) to 180° C. from the viewpoint of the cooling rate of the resin composition and productivity.

[0260] As other injection conditions, the screw speed, back pressure, injection speed, holding pressure, holding time, etc. can be appropriately adjusted.

[0261] The molded article of the present embodiment described above can be used for all applications to which thermoplastic resins are generally applied, and is particularly suitable for applications in the automotive field.

[0262] As for the use in the automobile field, for example, as injection molded bodies for automobile interior materials, there can be mentioned injection molded bodies for ceiling materials, injection molded bodies for wheel covers, injection molded bodies for trunk linings, injection molded bodies for instrument panel surface materials, injection molded bodies for handle covers, injection molded bodies for armrests, injection molded bodies for head pads, injection molded bodies for seat belt covers, injection molded bodies for shift lever covers, injection molded bodies for console boxes, injection molded bodies for horn pads, injection molded bodies for knobs, injection molded bodies for airbag covers, injection molded bodies for various decorative parts, injection molded bodies for various pillars, injection molded bodies for door lock bezels, injection molded bodies for glove boxes, injection molded bodies for defrost nozzles, injection molded bodies for scuff plates, injection molded bodies for steering wheels, injection molded bodies for steering column covers, etc.

[0263] In addition, as applications in the automotive field, for example, as injection-molded articles for automotive exterior materials, there are injection-molded articles for bumpers, injection-molded articles for air flow deflectors, injection-molded articles for fenders, injection-molded articles for side moldings, injection-molded articles for door mirror housings, injection-molded articles for floor guards, and the like.

[0264] Examples of other injection-molded articles for automobile parts include injection-molded articles for automobile headlights, injection-molded articles for glass runners, injection-molded articles for weather strips, injection-molded articles for drain hoses, injection-molded articles for window washer pipes, injection-molded articles for pipes, injection-molded articles for rack and pinion sleeves, injection-molded articles for gaskets, injection-molded articles for bumper beams, injection-molded articles for crash boxes, injection-molded articles for various components, injection-molded articles for suspension systems, injection-molded articles for front-end modules, injection-molded articles for radiator brackets, injection-molded articles for rear door interiors, and the like.

[0265] In addition, the molded body of this embodiment can be applied to sensors, LED lamps, connectors, slots, resistors, relay boxes, switches, coil bobbins, capacitors, variable capacitor boxes, optical pickups, oscillators, various terminal boards, transformers, plugs, printed circuit boards, tuners, speakers, microphones, headphones, small motors, head mounts, energy modules, semiconductors, liquid crystal displays, FDD slides, FDD chassis, motor brush holders, parabolic antennas, computer-related parts, microwave oven parts, audio / sound equipment parts, lighting parts, air conditioning parts, office computer-related parts, telephone / FAX-related parts, and copier-related parts, in addition to the above.

[0266] Since the molded article of the present embodiment described above uses the above resin composition, the mechanical strength is further improved and the MDTD anisotropy of the mechanical strength is reduced.

[0267] [Example]

[0268] Hereinafter, the present invention will be described in further detail based on specific examples. However, the present invention is not limited to the following examples at all.

[0269] [Flow start temperature of thermoplastic resin]

[0270] The flow start temperature of the thermoplastic resin (liquid crystal polyester resin) described below was evaluated using a flow tester (manufactured by Shimadzu Corporation, CFT-500 model). Specifically, about 2 g of the thermoplastic resin (liquid crystal polyester resin) was filled into a capillary rheometer equipped with a die head with an inner diameter of 1 mm and a length of 10 mm. Next, the filled thermoplastic resin (liquid crystal polyester resin) was heated at a rate of 4°C / min at 9.8 MPa (100 kg / cm 2 ) when extruded from the nozzle of the rheometer under a load of , the temperature at which the melt viscosity showed 4800 Pa·s (48000 poise) was recorded as the flow start temperature.

[0271] [Flow start temperature of resin particles]

[0272] The flow starting temperature of the resin pellets described below was evaluated using a flow tester (manufactured by Shimadzu Corporation, CFT-500 model). Specifically, first, the resin pellets were freeze-crushed under specified conditions (resin pellet input amount: 5 g, pre-freezing time: 10 minutes, freeze-crushing time: 10 minutes) using a ball mill freeze-crusher ("JFC-1500" manufactured by Japan Analytical Industry Co., Ltd.).

[0273] Next, the flow starting temperature of the resin particles was measured in the same manner except that the thermoplastic resin (liquid crystal polyester resin) in the above-mentioned [Flow starting temperature of thermoplastic resin] was changed to the frozen pulverized resin particles.

[0274] <Production of pure particles>

[0275] Pure particles (1) to (2) processed from liquid crystal polyester resin are manufactured respectively.

[0276] 《Manufacturing of pure particles (1)》

[0277] Pure particles (1) (LCP1) were produced as follows.

[0278] In a reactor equipped with a stirring device, a torque measuring instrument, a nitrogen inlet pipe, a thermometer and a reflux cooler, p-hydroxybenzoic acid (994.5 g, 7.2 moles), 4,4'-dihydroxybiphenyl (446.9 g, 2.4 moles), terephthalic acid (299.0 g, 1.8 moles), isophthalic acid (99.7 g, 0.6 moles), acetic anhydride (1347.6 g, 13.2 moles) and 1-methylimidazole 0.9 g were added, and the reactor was fully substituted with nitrogen. Thereafter, the temperature was raised from room temperature to 150°C in 30 minutes under a nitrogen stream, and refluxed at 150°C for 1 hour. Next, 1-methylimidazole (0.9 g) was added, and the by-produced acetic acid or unreacted acetic anhydride was distilled off while the temperature was raised from 150°C to 320°C for 2 hours and 50 minutes. The moment when the torque rise was found was regarded as the end of the reaction and the contents were taken out and cooled to room temperature. The obtained solid material was crushed into a particle size of about 0.1 to 1 mm by a crusher, and then heated from room temperature to 250° C. for 1 hour, and from 250° C. to 285° C. for 5 hours, and maintained at 285° C. for 3 hours under a nitrogen environment to perform solid phase polymerization. After solid phase polymerization, the mixture was cooled to obtain a powdery liquid crystal polyester resin.

[0279] The liquid crystal polyester resin obtained here has 60 mol % Ar based on the total amount of all repeating units. 1 The repeating unit (1) is 1,4-phenylene, having 15 mol% Ar 2 The repeating unit (2) is 1,4-phenylene, and has 5 mol% Ar 2 The repeating unit (2) is 1,3-phenylene and has 20 mol% Ar 3 The repeating unit (3) is 4,4'-biphenylene and its flow starting temperature is 327°C.

[0280] The obtained powdery liquid crystal polyester resin was pelletized using a twin-screw extruder (PMT47, manufactured by IKG) at a cylinder temperature of 320°C to produce LCP1. The flow start temperature of the obtained LCP1 was 316°C.

[0281] 《Manufacturing of pure particles (2)》

[0282] Pure particles (2) (LCP2) were produced as follows.

[0283] To a reactor equipped with a stirring device, a torque measuring instrument, a nitrogen inlet pipe, a thermometer and a reflux cooler, p-hydroxybenzoic acid (994.5 g, 7.2 moles), 4,4'-dihydroxybiphenyl (446.9 g, 2.4 moles), terephthalic acid (239.2 g, 1.44 moles), isophthalic acid (159.5 g, 0.96 moles) and acetic anhydride (1347.6 g, 13.2 moles) were added, and 1-methylimidazole (0.9 g) was added, and the reactor was fully replaced with nitrogen. Thereafter, the temperature was raised from room temperature to 150°C in 30 minutes under a nitrogen stream, and refluxed at 150°C for 1 hour. Next, 0.9 g of 1-methylimidazole was added, and the by-produced acetic acid or unreacted acetic anhydride was distilled off, while the temperature was raised from 150°C to 320°C for 2 hours and 50 minutes, and the moment when the torque rise was found was regarded as the end of the reaction and the contents were taken out and cooled to room temperature. The obtained solid material was crushed into a particle size of about 0.1 to 1 mm by a crusher, and then heated from room temperature to 220° C. in 1 hour, and from 220° C. to 240° C. in 0.5 hour, and maintained at 240° C. for 10 hours under a nitrogen environment to perform solid phase polymerization. After solid phase polymerization, the mixture was cooled to obtain a powdery liquid crystal polyester resin.

[0284] The liquid crystal polyester resin obtained here has 60 mol % Ar based on the total amount of all repeating units. 1 The repeating unit (1) is 1,4-phenylene, having 12 mol% Ar 2 The repeating unit (2) is 1,4-phenylene, having 8 mol% Ar 2 The repeating unit (2) is 1,3-phenylene and has 20 mol% Ar 3 The repeating unit (3) is 4,4'-biphenylene and its flow starting temperature is 291°C.

[0285] The obtained powdered liquid crystal polyester resin was pelletized using a twin-screw extruder (PMT47, manufactured by IKG) at a cylinder temperature of 290° C. to produce LCP2. The flow start temperature of the obtained LCP2 was 284° C.

[0286] <Manufacturing of resin pellets>

[0287] Resin pellets 1 to 5 in which glass fibers were impregnated with a liquid crystal polyester resin were respectively produced.

[0288] Use with Figure 1 Resin pellets 1 to 5 were produced in the following manner using a production apparatus having the same form as shown.

[0289] The extruder 120 used was a GTS-40 extruder (manufactured by Plastic Engineering Laboratory Co., Ltd.). The belt puller used was an EBD-1500A (manufactured by AIMEX Corporation). The following glass fibers were used as the glass fibers.

[0290] [Fiberglass]

[0291] GF1: glass fiber roving (E glass, fiber diameter 11 μm, fineness 1400 g / 1000 m, manufactured by Nippon Electric Glass Co., Ltd.).

[0292] GF2: glass fiber roving (E glass, fiber diameter 17 μm, fineness 2300 g / 1000 m, manufactured by Nippon Electric Glass Co., Ltd.).

[0293] GF3: glass fiber roving (HME-glass, fiber diameter 17 μm, fineness 1180 g / 1000 m, manufactured by Nitto Bosho Co., Ltd.).

[0294] GF4: glass fiber roving (HME-glass, fiber diameter 17 μm, fineness 3540 g / 1000 m).

[0295] It should be noted that GF4 is a glass fiber roving obtained by bundling three GF3 strands.

[0296] GF5: glass fiber roving (E glass and HME-glass, fiber diameter 17 μm, fineness 3480 g / 1000 m).

[0297] It should be noted that GF5 is a glass fiber roving obtained by bundling GF2 and GF3.

[0298] 《Manufacturing of resin pellets 1》

[0299] As pure particles, the above-mentioned LCP1 and LCP2 were used.

[0300] A resin structure 13 containing 156 parts by mass of GF1: glass fiber roving (E glass, fiber diameter 11 μm, fineness 1400 g / 1000 m, manufactured by Nippon Electric Glass Co., Ltd.) was obtained relative to a total of 100 parts by mass of LCP1 and LCP2 (75 parts by mass of LCP1, 25 parts by mass of LCP2). Specifically, it was manufactured as follows.

[0301] A step of obtaining a resin structure.

[0302] The belt take-up machine (the take-up unit 127 ) is operated to continuously feed the glass fiber bundle 11 from the glass fiber roving 10 at a take-up speed of 10 m / min. First, the glass fiber bundle 11 is heated to 150° C. by the preheating unit 121 and dried.

[0303] Next, while supplying the dried glass fiber bundle 11 to the die (impregnation section 123) installed at the front end of the extruder 120, molten LCP1 and LCP2 are introduced from the supply port 123a of the extruder 120. LCP1 and LCP2 are melted at 380°C and impregnated into the glass fiber bundle 11 in the die (impregnation section 123), and the bundle diameter is adjusted at the die (impregnation section 123) outlet with a die head having a nozzle diameter of 1.3 mm to obtain a resin structure 13 having 156 parts by mass of glass fibers relative to a total of 100 parts by mass of LCP1 and LCP2 (75 parts by mass of LCP1 and 25 parts by mass of LCP2).

[0304] In the resin structure 13 obtained here, the glass fibers are arranged substantially in parallel with the longitudinal direction of the first liquid crystal polyester resin layer.

[0305] Thereafter, the resin structure 13 in a heated state in the mold (impregnation unit 123 ) is cooled to 150° C. or less in the cooling unit 125 .

[0306] The process of obtaining particles.

[0307] Next, the cooled resin structure 13 is pulled into a strand shape by the belt puller (pulling unit 127), sent to a pelletizer (cutting unit 129), and cut into a predetermined length (12 mm) along its longitudinal direction to obtain cylindrical resin pellets 1.

[0308] The flow start temperature of the resin pellet 1 was 311°C.

[0309] [Measurement of the length-weighted average fiber length of glass fibers in resin pellets]

[0310] The resin pellet 1 was cut in the longitudinal direction and the cross section obtained by cutting was observed under a microscope. As a result of this observation, it was confirmed that the arrangement direction of the glass fibers was substantially consistent with the longitudinal direction of the resin pellet 1 and substantially parallel to the longitudinal direction of the resin pellet 1 .

[0311] The length-weighted average fiber length of the glass fibers in the resin pellets 1 is determined in the following manner.

[0312] Step (1): 2 g of the resin pellets were heated at 600° C. for 4 hours in a muffle furnace to remove the resin portion (first thermoplastic resin).

[0313] Step (2): The resin portion is removed from the resin particles, and the glass fiber-only substance is dispersed in 1000 mL of an aqueous solution to which 0.05% by volume of a surfactant (Micro90, manufactured by INTERNATIONAL PRODUCTS CORPORATION) is added to prepare a glass fiber dispersion.

[0314] Step (3): Take 100 mL of the dispersion and dilute it 10 times with pure water. Take 50 mL of the diluted dispersion and disperse it in a culture dish. Then, observe the glass fibers dispersed in the culture dish using a microscope (VH-Z25, manufactured by KEYENCE, magnification 10 times), and take 10 images of each sample in a manner that the shooting areas do not overlap.

[0315] Step (4): Use the measuring tool of the microscope to measure the length of all glass fibers present in one of the captured images. It should be noted that the bent glass fibers are measured by multi-point measurement, and the fibers touching the edge of the image are not measured. The same operation is performed in the 10 captured images in sequence until the total number of glass fibers measured exceeds 500, so as to determine the fiber length of the glass fibers.

[0316] Step (5): From the fiber length of the glass fiber measured in step (4), calculate the length-weighted average fiber length lm = (Σli 2 ×ni) / (Σli×ni), (Σni>500).

[0317] li: fiber length of glass fiber.

[0318] ni: The number of glass fibers with fiber length li.

[0319] As a result, the length-weighted average fiber length of the glass fibers in the resin pellet 1 was the same as the length of the pellet (12 mm).

[0320] [Measurement of the Fineness of Glass Fiber in Resin Pellets]

[0321] In addition, the fineness of the glass fibers in the resin pellets 1 was determined in the following manner.

[0322] Step (a): The weight of the resin particles per 100 resin particles was measured to 0.1 mg unit using a precision balance. Thereafter, the resin particles were heated at 600° C. for 4 hours using a muffle furnace to remove the resin portion (first thermoplastic resin).

[0323] Step (b): remove the resin part from the resin particles, take out the material that is only glass fiber, and measure the total weight A of glass fiber to 0.1 mg unit with a precision balance. Thereafter, the glass fiber having measured the total weight is dispersed in 1000 mL of an aqueous solution to which 0.05 volume % surfactant (Micro90, made by International Products Corporation) is added to prepare a glass fiber dispersion.

[0324] Step (c): 100 mL was taken out from the dispersion and diluted 10 times with pure water. 50 mL was taken out from the diluted dispersion and dispersed in a culture dish. Then, the glass fibers dispersed in the culture dish were observed using a microscope (VH-Z25, manufactured by KEYENCE, magnification 10 times), and 10 pieces were photographed in a manner that the photographed areas did not overlap.

[0325] Step (d): Use the measuring tool of the microscope to measure the length of all glass fibers present in one of the captured images. It should be noted that the bent glass fibers are measured by multi-point measurement, and the fibers touching the edge of the image are not measured. The same operation is performed in the 10 images captured in sequence until the total number of glass fibers measured exceeds 500, so as to measure the fiber length of the glass fibers.

[0326] Step (e): From the fiber length of the glass fiber measured in step (d), calculate the number average fiber length Lm = (ΣLi×ni) / Σni, (Σni>500).

[0327] Li: Fiber length of glass fiber.

[0328] ni: The number of glass fibers with fiber length Li.

[0329] Step (f); Calculate the fineness of the glass fiber based on 100 resin pellets used to measure the total weight A of the glass fiber obtained by step (b) and the number average fiber length Lm of the glass fiber obtained in step (e).

[0330] Fineness (unit: g / 1000m) = 1000 × 1000 (unit: m) / Lm (unit: mm) × A (unit: g) / 100

[0331] As a result, the fineness of the glass fibers in the resin pellet 1 was 1400 g / 1000 m.

[0332] [Measurement of Number Average Fiber Diameter of Glass Fibers in Resin Pellets]

[0333] The number average fiber diameter of the glass fibers in the resin pellets 1 was determined according to the following procedure.

[0334] The resin portion was removed from the resin pellets by the same method as in step (1) of calculating the length-weighted average fiber length of the glass fibers, the obtained glass fibers were observed using a scanning electron microscope (1000 times), and the number average of the fiber diameters of 500 randomly selected glass fibers was measured.

[0335] As a result, the number average fiber diameter of the glass fibers in the resin particles 1 was 11 μm.

[0336] 《Manufacturing of resin pellets 2》

[0337] As pure particles, the above-mentioned LCP1 and LCP2 were used.

[0338] A resin structure 13 containing 227 parts by mass of GF2: glass fiber roving (E glass, fiber diameter 17 μm, fineness 2300 g / 1000 m, manufactured by Nippon Electric Glass Co., Ltd.) was obtained relative to a total of 100 parts by mass of LCP1 and LCP2 (75 parts by mass of LCP1 and 25 parts by mass of LCP2).

[0339] It should be noted that the wire bundle diameter was adjusted using a die head having a nozzle diameter of 1.5 mm.

[0340] Except for this, the same method as in the production of the above resin pellets 1 was carried out to obtain resin pellets 2 having a cylindrical shape (length 12 mm).

[0341] It should be noted that the length-weighted average fiber length of the glass fibers in the resin pellets 2 is the same as the length of the pellets (12 mm). The fineness of the glass fibers in the resin pellets 2 is 2300 g / 1000 m. The number average fiber diameter of the glass fibers in the resin pellets 2 is 17 μm.

[0342] The flow start temperature of the resin particles 2 was 316°C.

[0343] 《Manufacturing of resin pellets 3》

[0344] As pure particles, the above-mentioned LCP1 and LCP2 were used.

[0345] A resin structure 13 containing 192 parts by mass of GF3: glass fiber roving (HME-glass, fiber diameter 17 μm, fineness 1180 g / 1000 m, manufactured by Nitto Bosho Co., Ltd.) was obtained relative to a total of 100 parts by mass of LCP1 and LCP2 (75 parts by mass of LCP1 and 25 parts by mass of LCP2).

[0346] It should be noted that the wire bundle diameter was adjusted using a die head having a nozzle diameter of 1.1 mm.

[0347] Except for this, the same method as in the production of the above-mentioned resin pellets 1 was carried out to obtain resin pellets 3 having a cylindrical shape (9 mm or 12 mm).

[0348] It should be noted that the length-weighted average fiber length of the glass fibers in the resin pellets 3 is the same as the length of the pellets (9 mm or 12 mm). The fineness of the glass fibers in the resin pellets 3 is 1180 g / 1000 m. The number average fiber diameter of the glass fibers in the resin pellets 3 is 17 μm.

[0349] The flow start temperature of the resin particles 3 was 314°C.

[0350] 《Manufacturing of resin pellets 4》

[0351] As pure particles, the above-mentioned LCP1 and LCP2 were used.

[0352] A resin structure 13 containing 192 parts by mass of GF4: glass fiber roving (HME-glass, fiber diameter 17 μm, fineness 3540 g / 1000 m) was obtained based on 100 parts by mass of LCP1 and LCP2 in total (75 parts by mass of LCP1 and 25 parts by mass of LCP2).

[0353] It should be noted that the wire bundle diameter was adjusted using a die head having a nozzle diameter of 2.0 mm.

[0354] Except for this, the same method as in the production of the above-mentioned resin pellet 1 was carried out to obtain a columnar resin pellet 4 (length 12 mm).

[0355] It should be noted that the length-weighted average fiber length of the glass fibers in the resin pellets 4 is the same as the length of the pellets (12 mm). The fineness of the glass fibers in the resin pellets 4 is 3540 g / 1000 m. The number average fiber diameter of the glass fibers in the resin pellets 4 is 17 μm.

[0356] The flow start temperature of the resin particles 4 was 312°C.

[0357] 《Manufacturing of resin pellets 5》

[0358] As pure particles, the above-mentioned LCP1 and LCP2 were used.

[0359] A resin structure 13 containing 161 parts by mass of GF5: glass fiber roving (E glass and HME-glass, fiber diameter 17 μm, fineness 3480 g / 1000 m) was obtained relative to a total of 100 parts by mass of LCP1 and LCP2 (75 parts by mass of LCP1 and 25 parts by mass of LCP2).

[0360] It should be noted that the wire bundle diameter was adjusted using a die head having a nozzle diameter of 2.0 mm.

[0361] Except for this, the same method as in the production of the above-mentioned resin pellet 1 was carried out to obtain a columnar resin pellet 5 (length 12 mm).

[0362] It should be noted that the length-weighted average fiber length of the glass fibers in the resin pellets 5 is the same as the length of the pellets (12 mm). The fineness of the glass fibers in the resin pellets 5 is 3480 g / 1000 m. The number average fiber diameter of the glass fibers in the resin pellets 5 is 17 μm.

[0363] The flow start temperature of the resin particles 5 was 311°C.

[0364] Table 1 shows the compositions of resin pellets 1 to 5, the number average fiber diameter of the glass fibers in the resin pellets, and the fineness of the glass fibers in the resin pellets.

[0365] [Table 1]

[0366]

[0367] <Manufacturing of molded body>

[0368] (Examples 1 to 4, Comparative Examples 1 to 2)

[0369] The resin compositions of each example are prepared by mixing the components shown in Tables 2 and 3, and the resin compositions are injection molded to produce respective molded bodies (injection molded products). Specifically, the components shown in Tables 2 and 3 are mixed and respectively put into the hopper of the injection molding machine TR450EH3 (manufactured by Sodick Co., Ltd.). By melt-kneading in the injection molding machine at a melt-kneading temperature (plasticizing section) of 300°C and injecting into a mold at a mold temperature of 100°C at an injection speed of 20mm / sec, a flat plate-shaped molded product of 150mm×150mm×4mm in thickness is formed. It should be noted that the gate is a film gate with a thickness of 4mm from one side of the molded product on the flat plate.

[0370] Other injection conditions: plunger temperature 360°C, screw speed (plasticizing part) 100 rpm, back pressure 1 MPa, holding pressure 100 MPa, holding time 5 seconds.

[0371] It should be noted that the abbreviations in Tables 2 and 3 have the following meanings.

[0372] ·Higher fatty acid metal salts

[0373] S1: Magnesium behenate (melting point: 117°C, manufactured by Nitto Chemical Industry Co., Ltd.)

[0374] The melting point of the higher fatty acid metal salt was measured using a differential scanning calorimeter (DSC-50 manufactured by Shimadzu Corporation). The position of the highest temperature endothermic peak that appeared when the higher fatty acid metal salt was heated at a rate of 10°C / min was taken as the melting point of the higher fatty acid metal salt.

[0375] [Measurement of the length-weighted average fiber length of glass fibers in molded articles]

[0376] Step (1): A test piece of 20 mm in width × 20 mm in length × 4 mm in thickness was cut out from the center of a flat plate-shaped molded product (150 mm × 150 mm × 4 mm in thickness) and heated at 600°C for 4 h in a muffle furnace to remove the resin portion.

[0377] Step (2): The material (only glass fiber) obtained by removing the resin portion from the flat plate-shaped molded product was dispersed in 1000 mL of an aqueous solution to which 0.05% by volume of a surfactant (Micro90, manufactured by INTERNATIONAL PRODUCTS CORPORATION) was added to prepare a dispersion.

[0378] Step (3): 100 mL was taken out from the dispersion and diluted to 15 times with pure water. 50 mL was taken out from the diluted dispersion and dispersed in a culture dish. Then, the glass fibers dispersed in the culture dish were observed using a microscope (VH-ZST (manufactured by Keyence Corporation) with a magnification of 20 times), and 10 images were taken for each sample in a manner that the shooting areas did not overlap.

[0379] Step (4): Use the microscope's measuring tool to measure the length of all fibers in one image. It should be noted that the bent fibers are measured by multi-point measurement. The same operation is performed in 10 images taken in sequence until the total number of measured fibers exceeds 500 to measure the fiber length.

[0380] Step (5): From the fiber length of the glass fibers measured in step (4), the length-weighted average fiber length lm of the glass fibers in the molded article is calculated = (Σli 2 ×ni) / (Σli×ni), (Σni>500).

[0381] li: fiber length of glass fiber.

[0382] ni: The number of glass fibers with fiber length li.

[0383] The results are shown in Tables 2 and 3.

[0384] [Bending strength of molded product in MD direction]

[0385] ·Preparation of test pieces for MD direction evaluation of molded products

[0386] The 120 mm × 120 mm portion of the central portion of the flat plate-shaped molded product was cut into a shape of 10 mm in width × 80 mm in length × 4 mm in thickness in a manner such that the longitudinal direction was MD, and 10 plate-shaped test pieces (test pieces for evaluation in the MD direction) were obtained from one flat plate-shaped molded product. It should be noted that the numbers 1 to 10 were marked in sequence starting from the left side when the gate of the flat plate-shaped molded product was facing upward.

[0387] Evaluation of MD bending strength of molded products

[0388] Using the obtained MD direction evaluation test pieces with odd numbers, the bending strength was measured five times in accordance with ISO 178. The bending strength of the molded article was the average of the obtained measured values. The results are shown in Tables 2 and 3.

[0389] [Bending strength of molded product in TD direction]

[0390] ·Preparation of test pieces for TD direction evaluation of molded products

[0391] The 120 mm × 120 mm portion of the central portion of the flat plate-shaped molded product was cut into a shape of 10 mm in width × 80 mm in length × 4 mm in thickness in the longitudinal direction TD, and 10 plate-shaped test pieces (test pieces for TD direction evaluation) were obtained from one flat plate-shaped molded product. It should be noted that the numbers 1 to 10 were marked in order from the gate close to the flat plate-shaped molded product.

[0392] Evaluation of TD bending strength of molded products

[0393] Using the obtained TD direction evaluation test pieces with odd numbers, the bending strength was measured five times in accordance with ISO 178. The bending strength of the molded body was the average of the obtained measured values. The results are shown in Tables 2 and 3.

[0394] [Charpy impact strength of molded product in MD direction]

[0395] Using the 5 MD direction evaluation test pieces marked with even numbers in the above MD direction evaluation test pieces, a notch tool (Notching Tool, ノッチングツール) (Model A-4, Toyo Seiki) was used to process a 45° V-groove with a depth of 2 mm in the width direction of the central part of the plate-shaped test piece according to ISO 2818 and JIS K7144 (notch front end radius: 0.25 mm ± 0.05 mm). Using the obtained 5 notched plate-shaped test pieces, the Charpy impact strength was measured 5 times using a pendulum 7.5 J according to ISO179. The Charpy impact strength of the molded body adopts the average value of the measured values ​​obtained. The results are shown in Tables 2 and 3.

[0396] [Charpy impact strength of molded product in TD direction]

[0397] Using the 5 TD direction evaluation test pieces marked with even numbers among the above TD direction evaluation test pieces, a notch tool (Notching Tool) (Model A-4, manufactured by Toyo Seiki) was used to process a 45° V-groove with a depth of 2 mm in the width direction of the central part of the plate-shaped test piece (notch front end radius: 0.25 mm ± 0.05 mm) according to ISO 2818 and JIS K7144. Using the obtained 5 notched plate-shaped test pieces, the Charpy impact strength was measured 5 times using a pendulum 7.5J according to ISO179. The Charpy impact strength of the molded body adopts the average value of the measured values ​​obtained. The results are shown in Tables 2 and 3.

[0398] [Table 2]

[0399]

[0400] [Table 3]

[0401]

[0402] From the results shown in Tables 2 and 3, the injection molded products made using the resin compositions of Examples 1 to 4 have higher mechanical strength (bending strength, impact strength) not only in the MD direction but also in the TD direction, compared with the injection molded products made using the resin compositions of Comparative Examples 1 and 2, and the MDTD anisotropy of the mechanical strength is reduced.

[0403] As described above, it was confirmed that the resin composition according to the present embodiment can further improve the strength of a molded body and reduce the MDTD anisotropy of the strength of the molded body.

[0404] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to these embodiments. The configurations may be added, omitted, replaced, or otherwise modified without departing from the spirit of the present invention. The present invention is not limited to the foregoing description, but is limited only by the scope of the appended claims.

[0405] Description of Reference Numerals

[0406] 100: manufacturing device; 101 to 109: conveying rollers; 120: extruder; 121: preheating section; 123: impregnation section; 125: cooling section; 127: pulling section; 129: cutting section.

Claims

1. A resin composition, in, contain: Resin pellets comprising a first thermoplastic resin and glass fibers; as well as The second thermoplastic resin, The second thermoplastic resin has a flow start temperature lower than that of the resin particles, The fineness of the glass fiber in the resin pellet is 500 g / 1000 m or more and 3400 g / 1000 m or less, The first thermoplastic resin and the second thermoplastic resin are both liquid crystal polyester resins.

2. The resin composition according to claim 1, in, The content of the glass fiber is more than 35 parts by mass and less than 65 parts by mass based on 100 parts by mass of the total amount of the resin particles and the second thermoplastic resin.

3. The resin composition according to claim 1, in, The content of the second thermoplastic resin is 10 to 45 parts by mass based on 100 parts by mass of the total amount of the resin particles and the second thermoplastic resin.

4. The resin composition according to claim 2, in, The content of the second thermoplastic resin is 10 to 45 parts by mass based on 100 parts by mass of the total amount of the resin particles and the second thermoplastic resin.

5. The resin composition according to any one of claims 1 to 4, in, The length-weighted average fiber length of the glass fibers is 5 to 20 mm.

6. The resin composition according to any one of claims 1 to 4, in, The number average fiber diameter of the glass fiber is 10 to 20 μm.

7. The resin composition according to claim 5, in, The number average fiber diameter of the glass fiber is 10 to 20 μm.

8. The resin composition according to any one of claims 1 to 4 and 7, in, When a notched Charpy impact strength test was performed on a molded body having a size of 10 mm in width, 80 mm in length, and 4 mm in thickness produced using the resin composition, Impact strength in MD direction i Impact strength in TD direction i TD i / MD i It is above 0.

5.

9. The resin composition according to claim 5, in, When a notched Charpy impact strength test was performed on a molded body having a size of 10 mm in width, 80 mm in length, and 4 mm in thickness produced using the resin composition, Impact strength in MD direction i Impact strength in TD direction i TD i / MD i It is above 0.

5.

10. The resin composition according to claim 6, in, When a notched Charpy impact strength test was performed on a molded body having a size of 10 mm in width, 80 mm in length, and 4 mm in thickness produced using the resin composition, Impact strength in MD direction i Impact strength in TD direction i TD i / MD i It is above 0.

5.

11. A molded body, in, This is a molded body produced using the resin composition according to any one of claims 1 to 10.