A method for manufacturing carbon fiber bracket composite molding
Through mold filling materials and pulse stamping technology, combined with carbon fiber prepreg and foam core materials, the problems of operational hazards, high costs and finished product appearance in the carbon fiber composite molding method are solved, and carbon fiber products with high yield and low energy consumption are achieved. forming.
Patent Information
- Application Number
- CN202111514873.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-13
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-12-13
AI Technical Summary
Existing carbon fiber composite molding methods have problems such as operational hazards, long production cycles, high costs, and difficulty in ensuring the appearance of the finished product. In particular, the vacuum autoclave manufacturing process is expensive and energy-intensive.
The mold is used to fill the material at the intersection of the designed thickness and corners of the product. Through pulse stamping and segmented inflation technology, combined with carbon fiber prepreg and foam core materials, the embedded blocks are locked to improve structural strength and molding quality.
It improves the yield rate of carbon fiber products, reduces manufacturing costs and energy consumption, ensures a smooth and flat surface, reduces the risk of nylon air duct bursting, and shortens the manufacturing cycle.
Smart Images

Figure CN114211776B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of fiber composite molding, and in particular to a manufacturing method for composite molding of a carbon fiber bracket. Background Art
[0002] Traditional carbon fiber composite product manufacturing methods: 1. Hand lay-up process is to manually laminate carbon cloth under a standard atmospheric pressure, apply hand lay-up resin, and then solidify it into shape. This method has many disadvantages, especially it is extremely harmful to operators and the environment, and the production cycle is long; 2. Nylon duct blowing molding process, that is, after the prepreg is stacked and laminated in an orderly manner according to the design, the nylon duct is pre-embedded inside, and then the mold is closed and heated, and the nylon duct is blown and pressurized to fill the cavity with the prepreg and solidify it. This method is prone to air leakage during the inflation molding process, resulting in a defective rate; 3. Core material compression molding process, that is, using hard foam material as the core material (hard foam mostly uses PMI / PU / PVC / balsa wood, etc.), the hard foam is cut into the shape of the product by CNC, and then the prepreg is coated on the hard foam, and finally molded and solidified. This method mainly has the following problems: 1. The process is relatively complicated and the CNC cost is high, 2. The material cost is high (adhesive, hard foam) 3. The appearance of the product is difficult to guarantee. Fourth, the large vacuum autoclave manufacturing process is to seal the composite blank, honeycomb sandwich structure or adhesive structure on the mold with a vacuum bag, and in the autoclave, under vacuum (or non-vacuum) state, through heating, pressurization, heat preservation (medium or high temperature), cooling and pressure relief processes, so that it becomes the required shape and quality. The autoclave, which is the main production equipment for composite parts, is a large pressure vessel with an integral heating system. Its common structure is a cylinder with one end closed and the other end open, which provides the necessary heat and pressure for the compaction and curing of composite parts. For example, the curing temperature of commonly used aviation thermosetting materials (high temperature curing epoxy resin) is 150-175℃, and the curing pressure is 500-600kPa. Therefore, the vacuum autoclave tank itself requires a high manufacturing cost. At the same time, when using this process to form, the autoclave needs to consume huge electric energy to ensure that the tank can maintain a high temperature and high pressure state. Therefore, the manufacturing cost of the autoclave manufacturing process is quite expensive. Summary of the invention
[0003] In order to solve the above problems, the present invention provides a manufacturing method of composite molding of a carbon fiber bracket.
[0004] To achieve the above object, the present invention provides a method for manufacturing a carbon fiber bracket by composite molding, comprising the following steps:
[0005] S1, according to the designed thickness of the product, the prepreg is laminated on the mold layer by layer according to the stacking design in the mold, and the carbon fiber prepreg in the prepreg is laminated with the mold;
[0006] S2, fill the corners of the product with filling materials to divide the entire product into several independent and unconnected areas. Inside the filling materials, insert the embedded blocks into the carbon yarn and punch holes and lock them according to the actual installation requirements, and arrange the nylon air ducts respectively; after forming, the embedded blocks are integrated with the entire product;
[0007] S3, reverse wrap the carbon yarn, then cover the carbon yarn with carbon fiber prepreg cloth and close the mold cover, lock the mold and place it on the molding table, turn on the air compressor to punch in a pulse form and heat at 120-150℃ for 0.5-3h, preferably 0.5-1.5h.
[0008] S4, cooling and demoulding the mold, and simultaneously extracting the nylon air duct in the fiber product, thereby obtaining a carbon fiber bracket.
[0009] Furthermore, the prepreg in step S1 is carbon fiber prepreg cloth, angle yarn and zero-degree yarn, wherein the angle yarn and zero-degree yarn are staggered and laminated to increase the overall structural strength.
[0010] Furthermore, the embedded block in step S2 is made of a material with heat conduction function, preferably a silicone block or a metal block or an engineering plastic block resistant to temperatures above 130 degrees; more preferably, the metal block is made of pure metal or alloy; most preferably, the pure metal is aluminum, iron, copper or titanium; the alloy is aluminum alloy, iron alloy, copper alloy, titanium alloy or stainless steel. The high temperature resistant engineering plastic block is a plastic block resistant to temperatures of 130°C, such as PEEK polyetheretherketone.
[0011] Furthermore, the filling material in the step S2 is a light, high-strength material that can withstand high temperatures of 150°C.
[0012] Furthermore, the filling material in step S2 is any one of the following:
[0013] 1) First, cut the PU block or PMI, PVC according to the shape of the intersection, and then cover it with a layer of 1-4mm foam core material to obtain the filling material;
[0014] 2) After heating the foam core material to preform the shape of the intersection, it is then coated with a layer of 1-4 mm foam core material to obtain the filling material;
[0015] The foaming core material can be foamed at 120-150°C; preferably, the foaming core material is HR-313-8; HR-330 product.
[0016] Furthermore, in the S3 step, the air compressor adopts segmented stamping in a pulse form; the first section: 2 kg force for 2 min; the second section: 4 kg force for inflation for 28 s and deflation for 2 s, and the inflation and deflation are repeated 4 times; the third section: 8 kg force for 2 min; the fourth section: 11 kg force for 50 min.
[0017] Furthermore, the carbon fiber support is a radiation beam, or a support leg, or a transverse support plate, or a rod-shaped or square tube.
[0018] The first step is to design the thickness of the product (such as Figure 1 ), in the mold, the prepreg is laminated layer by layer on the mold according to the stacking design. The prepreg is carbon fiber prepreg cloth, angle yarn and zero-degree yarn, where the carbon fiber prepreg cloth is laminated to the mold. The lamination order of the prepreg is: carbon fiber prepreg cloth, angle yarn and zero-degree yarn, where the angle yarn and zero-degree yarn are laminated alternately to increase the overall structural strength. Make a stacking design table based on the thickness, such as Figure 1 The thickness of the prepreg in area A is 3mm, the thickness of the prepreg in area B is 7mm, and the thickness of the prepreg in area C is 9mm. The basic principle is to paste the zero-degree yarn after the angle yarn. If the thickness requirement cannot be met, two layers of zero-degree yarn can be pasted and then the angle yarn. The thickness of carbon fiber prepreg on the market is generally 0.19mm, the thickness of the angle yarn is 0.2mm, 0.3mm, 0.4mm, and the thickness of the zero-degree yarn is 0.1 / 0.2 / 0.3 / 0.4mm.
[0019] The second step is, Figure 2 As shown, at the corner intersection of the product (such as Figure 2 Fill the filling material at the places marked 1-8) to divide the whole product into several independent and unconnected areas. Then, according to the actual installation requirements, the embedded blocks (the size and shape of the embedded blocks can be placed in the mold) are placed in the carbon yarn, punched and locked, and nylon air ducts are arranged separately. The embedded blocks are generally metal blocks or high-temperature resistant engineering plastic blocks. The metal materials are mostly aluminum, iron, copper, stainless steel and other metal blocks. They are used to lock the screws of the various components in the later stage to achieve the effect of fixing; wrap the embedded blocks with carbon yarn and then punch and lock them. After forming, the embedded blocks are integrated with the whole product and are not easy to loosen or move.
[0020] The filling material has the characteristics of light weight and high strength, and can withstand high temperature of 150℃, and will not shrink or collapse at this temperature. There are two kinds of filling materials: 1) Cut the PU block or PMI, PVC according to the shape of the intersection, and then cover it with a layer of 1-4mm foam core material to obtain the filling material; 2) Heat the foam core material to pre-form the shape of the intersection; then cover it with a layer of 1-4mm foam core material to obtain the filling material.
[0021] Among them, PU blocks (polyurethane), PVC (polyvinyl chloride), and PMI (polymethacrylimide foam) do not have the function of expansion when heated. The foaming core material can be foamed at a high temperature of 120-150℃, so as to make the filling fuller, such as the foaming core material of Haoer, such as the foaming core material of Haoer: HR-313-8; HR-330.
[0022] The third step is to reverse the carbon yarn, then cover the carbon yarn with carbon fiber prepreg cloth, close the mold cover, lock the mold and place it on the molding table, turn on the air compressor to punch in pulse form and heat at 120-150℃ for 0.5-1.5h. For example, the temperature can be 120℃, 121℃, 125℃, 130℃, 135℃, 140℃, 145℃, 150℃, but not limited to these temperatures, and can be any temperature from 120-150℃; heating molding 0.5h, 0.6h, 0.7h, 0.8h, 0.9h, 1.0h, 1.1h, 1.2h, 1.3h, 1.4h, 1.5h, not limited to these times, and can be any time from 0.5-1.5h.
[0023] Figure 2 Inflatable holes are set at the places with the middle number 1, 2, 4, 6, and 7. In order to prevent the blow-out, the air compressor uses segmented inflation when inflating the nylon air duct; the first section: 2 kg force for 2 minutes; the second section: 4 kg force for 28 seconds to inflate and 2 seconds to deflate, and the inflation and deflation are repeated 4 times; the third section: 8 kg force for 2 minutes; the fourth section: 11 kg force for 50 minutes.
[0024] The fourth step is to cool and demold the mold (for example, the cooling table temperature can be set to 20°C and cooled to room temperature), and at the same time, the nylon duct in the fiber product is pulled out (each section of the duct is not long and the duct will be soaked with a release agent before wrapping, which is convenient for pulling out after molding), so as to obtain the radar radiation beam and support legs or rod-shaped or square tubes.
[0025] The present invention fills the corner intersection with filling materials including foam material and arranges the nylon air duct in sections, thereby ensuring that each section of the nylon air duct has sufficient force to expand outward and is not easily damaged. For the corner intersection that is most prone to damage and collapse, the foam material will continue to provide outward force and can also ensure the quality of the product.
[0026] Advantages of the present invention:
[0027] 1. Compared with other molding methods, the method of the present invention improves the yield rate of carbon fiber product molding (the yield rate reaches 98.5%) and saves development and manufacturing costs.
[0028] 2. Compared with air blowing, this molding method has a simpler layout of the nylon duct. Filling materials are placed at the corner intersections, and the duct is inflated in sections, which further reduces the risk of the nylon duct bursting during blowing and causing molding failure. The corner intersections that are most prone to bursting and leaking are filled and separated by foaming materials. After filling these areas with foaming materials, the nylon duct will not expand excessively during inflation, which indirectly reduces the risk of leakage and bursting of the nylon duct.
[0029] 3. The surface of the large carbon fiber product formed by the method of the present invention is smooth and flat, and is not prone to bulging, lack of glue, etc.
[0030] 4. The present invention utilizes the thermal self-expansion property of low-density foam core material in combination with carbon fiber to manufacture carbon fiber products, which shortens the manufacturing cycle and reduces costs compared to vacuum autoclave molding. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 is the distribution diagram of the stent thickness.
[0032] Figure 2 It is a map of the filling area and the inflation holes. DETAILED DESCRIPTION
[0033] Embodiments of the present invention are described in detail below, and the examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals represent the same or similar elements or elements with the same or similar functions from beginning to end. The embodiments described below by reference to the accompanying drawings are exemplary, are intended to be used to explain the present invention, and are not to be construed as limitations of the present invention. Those who do not indicate specific techniques or conditions in the embodiments are carried out according to the techniques or conditions described in the documents in this area or according to the product specification. Those who do not indicate the manufacturer of reagents or instruments used are all conventional products that can be obtained commercially.
[0034] Example 1: Preparation of radar radiation beam and support legs
[0035] The first step is to design the thickness of the product (such as Figure 1 ), in the mold, the prepreg is laminated layer by layer on the mold according to the stacking design. The prepreg is carbon fiber prepreg cloth, angle yarn and zero-degree yarn, where the carbon fiber prepreg cloth is laminated to the mold. The lamination order of the prepreg is: carbon fiber prepreg cloth, angle yarn and zero-degree yarn, where the angle yarn and zero-degree yarn are laminated alternately to increase the overall structural strength. Make a stacking design table based on the thickness, such as Figure 1The thickness of the prepreg in area A is 3mm, the thickness of the prepreg in area B is 7mm, and the thickness of the prepreg in area C is 9mm. The basic principle is to paste the zero-degree yarn after the angle yarn. If the thickness requirement cannot be met, two layers of zero-degree yarn can be pasted and then the angle yarn. The thickness of carbon fiber prepreg on the market is generally 0.19mm, the thickness of the angle yarn is 0.2mm, 0.3mm, 0.4mm, and the thickness of the zero-degree yarn is 0.1 / 0.2 / 0.3 / 0.4mm.
[0036] The second step is, Figure 2 As shown, at the corner intersection of the product (such as Figure 2 Fill the places marked 1-8 with filling materials to divide the whole product into several independent and unconnected areas. Inside the filling materials, according to the actual installation requirements, the embedded blocks (the size and shape of the embedded blocks can be placed in the mold as the standard) are placed in the carbon yarn, punched and locked, and nylon air ducts are arranged separately. The embedded blocks are metal blocks made of aluminum blocks, which are used to lock the screws in the later assembly of various components to achieve the effect of fixing; wrap the embedded blocks with carbon yarn and then punch and lock them. After forming, the embedded blocks are integrated with the whole product and are not easy to loosen or move.
[0037] The filling material has the characteristics of light weight and high strength, and can withstand high temperature of 150℃ without shrinking or collapsing at this temperature. The filling material is: first cut the PU block according to the shape of the intersection, and then cover it with a layer of 1-4mm foam core material to obtain the filling material;
[0038] The PU block does not have the function of expansion when heated. The foam core material can be foamed at a high temperature of 120-150℃, so as to make the filling fuller, such as the foam core material of Haoer, such as the foam core material of Haoer: HR-313-8; replacing it with HR-330 can also achieve the same effect.
[0039] The third step is to reverse the carbon yarn, then cover the carbon yarn with carbon fiber prepreg cloth and close the mold cover, lock the mold and place it on the molding table, turn on the air compressor to punch in a pulse form and heat at 150℃ for 1 hour.
[0040] Figure 2 Inflatable holes are set at the places with the middle number 1, 2, 4, 6, and 7. In order to prevent the blow-out, the air compressor uses segmented inflation when inflating the nylon air duct; the first section: 2 kg force for 2 minutes; the second section: 4 kg force for 28 seconds to inflate and 2 seconds to deflate, and the inflation and deflation are repeated 4 times; the third section: 8 kg force for 2 minutes; the fourth section: 11 kg force for 50 minutes.
[0041] The fourth step is to cool and demould the mold (for example, the cooling table temperature can be set to 20°C and cooled to room temperature), and at the same time, the nylon air duct in the fiber product is pulled out (each section of the air duct is not long and the air duct will be soaked with a release agent before wrapping, which is convenient for pulling out after the molding is completed), and the radar radiation beam and support leg are obtained. The prepared radar radiation beam and support leg have a smooth surface without bulging, lack of glue, etc.
[0042] In this embodiment, 80 products were made, and 79 of them were qualified as excellent products, with a good product rate of nearly 99%.
[0043] The same result can be obtained by replacing the material of the embedded blocks with iron, copper, titanium, or corresponding alloys of various metals or stainless steel.
[0044] The same result can be achieved by replacing the PU block with PMI or PVC.
[0045] Example 2: Preparation of radar radiation beam and support legs
[0046] The first step is to design the thickness of the product (such as Figure 1 ), in the mold, the prepreg is laminated layer by layer on the mold according to the stacking design. The prepreg is carbon fiber prepreg cloth, angle yarn and zero-degree yarn, where the carbon fiber prepreg cloth is laminated to the mold. The lamination order of the prepreg is: carbon fiber prepreg cloth, angle yarn and zero-degree yarn, where the angle yarn and zero-degree yarn are laminated alternately to increase the overall structural strength. Make a stacking design table based on the thickness, such as Figure 1 The thickness of the prepreg in area A is 3mm, the thickness of the prepreg in area B is 7mm, and the thickness of the prepreg in area C is 9mm. The basic principle is to paste the zero-degree yarn after the angle yarn. If the thickness requirement cannot be met, two layers of zero-degree yarn can be pasted and then the angle yarn. The thickness of carbon fiber prepreg on the market is generally 0.19mm, the thickness of the angle yarn is 0.2mm, 0.3mm, 0.4mm, and the thickness of the zero-degree yarn is 0.1 / 0.2 / 0.3 / 0.4mm.
[0047] The second step is, Figure 2 As shown, at the corner intersection of the product (such as Figure 2 Fill the places marked 1-8 with filling materials to divide the whole product into several independent and unconnected areas. Inside the filling materials, according to the actual installation requirements, the embedded blocks (the size and shape of the embedded blocks can be placed in the mold as the standard) are placed in the carbon yarn, punched and locked, and nylon air ducts are arranged separately. The embedded blocks are generally high-temperature resistant engineering plastic blocks (PEEK polyetheretherketone), which are used to lock the screws for the later assembly of various components to achieve the effect of fixing; wrap the embedded blocks with carbon yarn and then punch and lock them. After molding, the embedded blocks are integrated with the whole product and are not easy to loosen or move.
[0048] The filling material has the characteristics of light weight and high strength, and can withstand high temperature of 150°C without shrinking or collapsing at this temperature. The filling material is obtained by preforming the shape of the intersection with the heated foam core material and then coating it with a layer of 1-4mm foam core material.
[0049] The foam core material can be foamed at a high temperature of 120-150°C to make the filling fuller, such as Haoer's foam core material: HR-313-8; replacing it with HR-330 can also achieve the same effect.
[0050] The third step is to reverse the carbon yarn, then cover the carbon yarn with carbon fiber prepreg cloth and close the mold cover, lock the mold and place it on the molding table, turn on the air compressor to punch in a pulse form and heat at 120℃ for 3 hours.
[0051] Figure 2 Inflatable holes are set at the places with the middle number 1, 2, 4, 6, and 7. In order to prevent the blow-out, the air compressor uses segmented inflation when inflating the nylon air duct; the first section: 2 kg force for 2 minutes; the second section: 4 kg force for 28 seconds to inflate and 2 seconds to deflate, and the inflation and deflation are repeated 4 times; the third section: 8 kg force for 2 minutes; the fourth section: 11 kg force for 50 minutes.
[0052] The fourth step is to cool and demould the mold (for example, the cooling table temperature can be set to 20°C and cooled to room temperature), and at the same time, the nylon air duct in the fiber product is pulled out (each section of the air duct is not long and the air duct will be soaked with a release agent before wrapping, which is convenient for pulling out after the molding is completed), and the radar radiation beam and support leg are obtained. The prepared radar radiation beam and support leg have a smooth surface without bulging, lack of glue, etc.
[0053] 66 products were prepared, 65 of which were qualified as excellent products, with a good product rate of 98.5%.
[0054] Example 3: Preparation of square tubes
[0055] The first step is to laminate the prepreg layer by layer on the mold according to the stacking design according to the designed thickness of the product. The prepreg is carbon fiber prepreg cloth, angle yarn and zero-degree yarn, and the carbon fiber prepreg cloth is laminated to the mold. The lamination order of the prepreg is: carbon fiber prepreg cloth, angle yarn and zero-degree yarn, and the angle yarn and zero-degree yarn are laminated alternately to increase the overall structural strength. Make a stacking design table based on the thickness. The basic principle is to laminate the zero-degree yarn after the angle yarn. If the thickness requirement cannot be met, two layers of zero-degree yarn and then the angle yarn can also be laminated). The thickness of carbon fiber prepreg cloth on the market is generally 0.19mm, the thickness of the angle yarn is 0.2mm, 0.3mm, 0.4mm, and the thickness of the zero-degree yarn is 0.1 / 0.2 / 0.3 / 0.4mm.
[0056] The second step is to fill the corners of the product with filling materials to divide the entire product into several independent and unconnected areas. Inside the filling materials, according to the actual installation requirements, the embedded blocks (the size and shape of the embedded blocks can be placed in the mold as the standard) are placed in the carbon yarn, punched and locked, and nylon air ducts are arranged separately. The embedded blocks are generally high-temperature resistant engineering plastic blocks (PEEK polyetheretherketone), which are used to lock the screws in the later assembly of various components to achieve the effect of fixing; the embedded blocks are wrapped with carbon yarn and then punched and locked. After molding, the embedded blocks are integrated with the entire product and are not easy to loosen or move.
[0057] The filling material has the characteristics of light weight and high strength, and can withstand high temperature of 150°C without shrinking or collapsing at this temperature. The filling material is obtained by preforming the shape of the intersection with the heated foam core material and then coating it with a layer of 1-4mm foam core material.
[0058] The foam core material can be foamed at a high temperature of 120-150°C to make the filling fuller, such as Haoer's foam core material: HR-313-8; replacing it with HR-330 can also achieve the same effect.
[0059] The third step is to reverse the carbon yarn, then cover the carbon yarn with carbon fiber prepreg cloth and close the mold cover, lock the mold and place it on the molding table, turn on the air compressor to punch in a pulse form and heat at 150℃ for 1.5 hours.
[0060] In order to prevent the nylon air duct from bursting due to blowing, the air compressor uses segmented inflation when inflating the nylon air duct; the first segment: 2 kg force for 2 minutes; the second segment: 4 kg force for 28 seconds and deflation for 2 seconds, and the inflation and deflation are repeated 4 times; the third segment: 8 kg force for 2 minutes; the fourth segment: 11 kg force for 50 minutes.
[0061] The fourth step is to cool and demold the mold (for example, the cooling table temperature can be set to 20°C and cooled to room temperature), and at the same time, the nylon duct in the fiber product is pulled out (each section of the duct is not long and the duct will be soaked with a release agent before wrapping, which is convenient for pulling out after the molding is completed), and the square tube is obtained. The surface of the prepared square tube is smooth and flat, without bulging, lack of glue, etc.
[0062] 66 products were prepared, 65 of which were qualified as excellent products, with a good product rate of 98.5%.
[0063] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention without departing from the principles and intent of the present invention.
Claims
1. A method for manufacturing a carbon fiber bracket composite molding, characterized in that: The steps include: S1, according to the designed thickness of the product, the prepreg is laminated on the mold layer by layer according to the stacking design in the mold, and the carbon fiber prepreg in the prepreg is laminated with the mold; the prepreg is a carbon fiber prepreg, angle yarn and zero-degree yarn, wherein the angle yarn and the zero-degree yarn are laminated alternately to increase the overall structural strength; S2, filling the corners of the product with filling materials to divide the entire product into several independent and unconnected areas. Inside the filling materials, the embedded blocks are placed in the carbon yarn and punched and locked according to the actual installation requirements, and nylon air ducts are arranged respectively. After forming, the embedded blocks are integrated with the entire product. The material of the embedded blocks is a material with heat conduction function. S3, reverse wrapping the carbon yarn, then covering the carbon yarn with carbon fiber prepreg cloth, closing the mold cover, locking the mold and placing it on the molding table, turning on the air compressor to punch in a pulse form and heat at 120-150°C for 0.5-3h; the air compressor uses segmented punching in a pulse form; The first stage: 2 kg force for 2 min; The second stage: 4 kg force, inflate for 28 seconds and deflate for 2 seconds, repeat 4 times; the third stage: 8 kg force for 2 minutes; the fourth stage: 11 kg force for 50 minutes; S4, cooling and demoulding the mold, and simultaneously extracting the nylon air duct in the fiber product, thereby obtaining a carbon fiber bracket.
2. The method according to claim 1, characterized in that The embedded blocks in step S2 are silicone blocks, metal blocks or engineering plastic blocks that can withstand temperatures above 130 degrees.
3. The method according to claim 2, characterized in that The material of the metal block is pure metal or alloy.
4. The method according to claim 3, characterized in that The pure metal is aluminum, iron, copper or titanium; the alloy is aluminum alloy, iron alloy, copper alloy, titanium alloy or stainless steel.
5. The method according to claim 1, characterized in that The filling material in the step S2 is a light, high-strength material that can withstand high temperatures of 150°C.
6. The method according to claim 1, characterized in that The filling material in step S2 is any of the following: 1) First, cut the PU block or PMI, PVC according to the shape of the intersection, and then cover it with a layer of 1-4mm foam core material to obtain the filling material; 2) After heating the foam core material to preform the shape of the intersection, it is then coated with a layer of 1-4 mm foam core material to obtain the filling material; The foaming core material can be foamed at 120-150°C.
7. The method according to claim 6, characterized in that The foam core material is HR-313-8; HR-330 foam material.
8. The method according to claim 1, characterized in that In the step S3, the heating and molding is performed for 0.5-1.5 hours.
9. The method according to claim 1, characterized in that The carbon fiber support is a radiation beam, or a support leg, or a transverse support plate, or a rod-shaped or square tube.
Citation Information
Patent Citations
Forming technology for carbon fiber antenna back frame or antenna supporting arm
CN105235239A
Vacuum thermal expansion molding process for composite
CN105690803A