Multilayer structures for transporting or storing gas or for exploiting offshore oil fields on the seabed
By using a polymer with a Tg higher than the operating temperature as the matrix and a polymer with a Tm lower than 280℃ as the sealing sheath in the composite pipe, and by using methods such as laser welding, the problem of insufficient mechanical strength and fatigue resistance of the composite pipe at high temperatures has been solved, and the stable use of the pipe at high temperatures has been achieved.
Patent Information
- Application Number
- CN202080055605.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-07-30
- Filing Date
- 2020-07-28
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-07-28
AI Technical Summary
When existing composite pipes are used at high temperatures, the matrix of the composite reinforcement is prone to rubberization, which leads to a decrease in mechanical strength. In addition, the rigidity and fatigue resistance of the sealing sheath are insufficient, affecting the service life and performance of the pipe.
Different polymers are used as the composite matrix and sealing sheath. The matrix of the composite reinforcement uses a semi-crystalline thermoplastic polymer P2j with a Tg greater than the maximum service temperature Tu+20℃, and the sealing layer uses a semi-crystalline thermoplastic polymer P1i with a Tm less than 280℃. The two are ensured to adhere well by means of laser welding and other methods.
Maintaining the high mechanical strength of the composite reinforcement and the flexibility of the sealing sheath at high temperatures improves the fatigue resistance and chemical stability of the pipeline, extending its service life.
Smart Images

Figure BDA0003495197300000171
Abstract
Description
Technical Field
[0001] The present patent application relates to a composite multilayer structure for transporting or storing gas, or for exploiting oil or gas fields on the seabed, and to a method for manufacturing said structure. Background Art
[0002] The exploitation of oil fields located in the oceans subjects the materials used, and in particular the pipelines that connect the various subsea installations of the platforms and transport the extracted hydrocarbons, which are generally transported at high temperatures and high pressures (eg 700 bar), to extreme conditions.
[0003] Therefore, during the operation of the plant, there are serious problems of mechanical strength and thermal and chemical resistance of the materials used. Such pipes must in particular withstand hot oil, gas, water, and mixtures of at least two of these products for a period of up to 20 years.
[0004] Conventionally, these pipes contain a non-sealed metal inner layer formed by spirally winding a profiled metal strip, such as a lock-seamed strip. This metal inner layer (which gives the pipe its shape) is coated (generally by extrusion) with a polymer layer intended to provide sealing.
[0005] The sheath must primarily:
[0006] capable of being extruded continuously, optionally on a support of an internal skeleton,
[0007] Sufficiently flexible to accommodate the bends imposed on the flexible pipe during the operations of its manufacture, laying and use on site (actions caused by expanding or lifting the flexible pipe to change the site of use),
[0008] Creep after being subjected to compressive forces, which is exacerbated by temperature levels. When the pipeline is subjected to the pressure of the effluent being transported, creep occurs in the gaps (voids or play) between the metal reinforcements (such as Z-joints or T-joints) on which the sheath is carried.
[0009] Sufficiently chemically stable so that its chemical properties and its seals do not deteriorate in a prohibitive manner during the life of the flexible conduit.
[0010] For the transport or storage of gas or for the exploitation of oil and gas fields, it is advantageous to use a composite pipe consisting of this sealing sheath, also called liner, reinforced by an external adhesive layer made of composite material (providing sealing and chemical and abrasion resistance of the pipe), manufactured by filament winding of unidirectional (UD) tapes deposited in successive layers on the liner at one or more orientation angles relative to the pipe axis, in order to provide the composite pipe with sufficient flexibility. The composite reinforcement enables the pipe to withstand pressure (internal pressure of the fluid and external pressure in the case of use in the sea at great depths).
[0011] This technology is that developed by the company Airborne and is described, for example, in document FR 2 964 173 .
[0012] More recently, Technip (WO2012118379) has shown interest in this pipe concept in combination with metallic external reinforcements (with the aim of getting rid of the internal skeleton of current offshore flexible pipes) and optionally the metallic reinforcements forming a pressure arch.
[0013] However, the solution envisaged for this type of composite pipes is based on using the same polymer for the liner and the matrix of the composite, in order to ensure excellent and durable adhesion between the liner and the composite.
[0014] For example, Airborne has developed a variety of flexible pipes without an internal skeleton and with a sealing sheath adhered to a composite reinforcement, comprising: a PA11 liner with a PA11 FC compound (JIP completed in 2011) or a PA12 liner with a PA12 FC compound, or even a PVDF liner with a PVDF FC compound. However, all these structures have the following disadvantages: the matrix of the composite reinforcement has a glass transition temperature Tg lower than the service temperature Tu of the pipe; that is, in the case of pipes based on PA11 or PA12, the Tg in the dry state is 50°C, while the pipe service temperature Tu is 60 to 80°C; and in the case of PVDF, the Tg is -40°C, while the service temperature in continuous operation is above 100°C and generally close to 130°C. In the specific case of PVDF, the stiffness (modulus) of the matrix remains high above its Tg until it reaches another transition (alpha transition) around 100°C, beyond which the behavior of the matrix becomes purely rubbery. Thus, in all the above industrial and commercial cases of TP matrix composite pipes, the matrix of the composite reinforcement is in a fully rubberized state at the composite pipe service temperature Tu.
[0015] To solve this problem and to ensure that the composite reinforcement, which gives the matrix a Tg above the maximum service temperature, is not in a rubbery state at the service temperature (130 °C in this case), Kutting & Total, and then Vitrex and Magma, have developed the following solution: a PEEK sealing sheath (or liner) which is also reinforced by a composite with a PEEK matrix. The Tg of PEEK is 140 °C and thus meets the requirement for high stiffness since this Tg is above the maximum service temperature. The drawback is that, as a result, the sealing sheath (liner) is also very rigid, which can limit its fatigue resistance and is a major drawback for the production of flexible pipes. In addition, the processing temperature of this type of sealing sleeve is very high (typically 380 - 400 °C) and this causes major difficulties in terms of tool operation and process control in the case of common conversion processes, which are pipe extrusion.
[0016] In addition, Ticona (Celanese), together with Airborne, offers composite pipes comprising a PPS FC reinforcement and a PPS sealing sheath.
[0017] For Tu > 90 °C, this structure causes the same problems for the composite matrix as the PVDF-based solution (i.e., Tg < Tu), and there are additionally problems with the transition temperature (typically 350 °C for PPS and 250 °C for PVDF).
[0018] For Tu < 90 °C, PPS is suitable as the matrix for the composite, but the problem of the extrusion temperature of the sealing sheath (liner) remains, as does its problem of high stiffness (which limits the flexibility of the composite pipe) and its problem of low fatigue resistance (due to a Tg greater than Tu).
[0019] Thus, it is still necessary to optimize, on the one hand, the matrix of the composite to optimize its mechanical strength at high temperatures and, on the other hand, the material forming the sealing liner to optimize its application temperature without deteriorating the adhesion of the composite reinforcement to the sealing liner. Thus, any optional changes made to the composition of the material forming the sealing sheath to ensure at least partial miscibility with the matrix of the composite should not result in a significant increase in the extrusion temperature of the liner compared to the temperatures currently practiced for polyamides and PVDF (i.e., remaining < 300 °C, preferably < 290 °C, even more preferably < 250 °C).
[0020] These problems are solved by providing the multi-layer structure of the present invention and in particular the flexible pipe, which is a fully integrated, "two-material" composite pipe and is formed by depositing a high-strength composite reinforcement (in particular by filament winding) on a liner extruded beforehand at a relatively low temperature. The adhesion between the composite and the liner is very good.
[0021] The present invention thus relates to a multilayer structure selected from tanks, pipes or tubes for transporting or storing gas or for exploiting oil or gas fields on the seabed, comprising, from the inside to the outside, at least one sealing layer and at least one composite reinforcement layer,
[0022] The innermost composite reinforcement layer is welded to the outermost adjacent sealing layer,
[0023] The sealing layer is composed of a composition that mainly comprises at least one semi-crystalline thermoplastic polymer P1i (i=1 to n, n is the number of sealing layers), whose Tm measured according to ISO 11357-3:2013 is less than 280°C, in particular less than 265°C,
[0024] The at least one thermoplastic polymer of each sealing layer may be identical or different, and at least one of the composite reinforcement layers consists of a fibrous material in the form of continuous fibers, which is impregnated with a composition that essentially comprises at least one thermoplastic polymer P2j, (j=1 to m, m being the number of reinforcement layers), in particular a semi-crystalline thermoplastic polymer P2j, said thermoplastic polymer P2j having a Tg greater than the maximum use temperature (Tu) of the structure measured according to ISO 11357-3:2013, wherein Tg≥Tu+20°C, Tu being greater than 50°C, in particular greater than 100°C,
[0025] Hydrogen is excluded from the gas transport or gas storage and multilayer structures selected from tanks, pipes or pipelines intended for transporting hydrogen are excluded.
[0026] Thus, the inventors unexpectedly discovered that using different polymers for the composite matrix and the liner, and in particular:
[0027] The matrix of the composite reinforcement is composed of a polymer having a Tg significantly greater than the maximum use temperature Tu of the tank or pipeline (typically, Tg>Tu+20°C) so as to still be in its glassy region and have a high stiffness, thereby enabling the composite to have a high mechanical strength,
[0028] The semi-crystalline polymer constituting the liner has a low melting point Tm, allowing it to be processed by extrusion, extrusion blow molding, rotational molding, injection or by winding a pure resin film (as the case may be) at moderate temperatures common to those skilled in the art, relative to the Tm of this polymer (less than 280°C, preferably less than 265°C). The currently known low-Tm semi-crystalline polymers also have a low Tg, which in most cases will be below the maximum use temperature. As a result, the polymer constituting the liner will work in its rubberized zone and will therefore be very flexible and therefore very resistant to fatigue. Its semi-crystalline nature ensures good resistance to chemical attack, wear and creep,
[0029] Furthermore, the two aforementioned polymers (the polymer constituting the matrix of the composite and the polymer constituting the liner) are sufficiently miscible to ensure weldability of the composite to the liner and thus excellent adhesion between the liner and the composite. The durability of the adhesion will be ensured by the durability of the materials constituting the mixture at the interface of the two materials, i.e. in the welded joint. The miscibility of the two polymers is expressed as follows: preferably by a single Tg; or when that is not possible, by the characteristic signature of a partially homogeneous mixture, for example by the presence of two Tg values intermediate to those of the two pure polymers.
[0030] The immiscibility of the two polymers results in the presence of two Tg's in the mixture of the two polymers, which correspond to the respective Tg's of the pure polymers taken separately.
[0031] "Multilayer structure" means, for example, a tank, a pipe or a pipeline comprising or consisting of several layers, in particular two layers.
[0032] The term "gas" refers to any gas, and in particular subsea extracted gas, especially natural gas, which does not include hydrogen.
[0033] The sealing layer(s) are the innermost layers compared to the composite reinforcement layer which is the outermost layer.
[0034] The sealing layer is in contact with the gas or oil and gas extracted from the seabed, even when there is an inner and therefore innermost non-sealing metal layer used to form the skeleton, which is formed by a spirally wound profiled metal strip, such as a strip with a crimped seam, on which the sealing layer(s) are coated by extrusion.
[0035] When there are several sealing layers, only the innermost of said sealing layers is in direct contact with the gas or oil and gas extracted at the seabed.
[0036] When only the sealing layer and the composite reinforcing layer are present, resulting in a multilayer structure of two layers, the two layers are welded and thereby adhered to each other, being in direct contact with each other.
[0037] When there are several sealing layers and / or several composite reinforcing layers, the outermost layer of the sealing layer (and thus the layer opposite the layer in contact with the gas or oil and gas extracted at the seabed) is welded to the innermost layer of the composite reinforcing layers and thus adheres to each other, being in direct contact with each other.
[0038] Other composite reinforcement layers are also welded together.
[0039] The other sealing layers are also welded together.
[0040] About Sealant Layers and Thermoplastic Polymers P1i
[0041] One or more sealing layers may be present.
[0042] Each of the layers consists of a composition which essentially comprises at least one thermoplastic polymer P1i, i corresponding to the number of layers present. i is from 1 to 10, in particular from 1 to 5, especially from 1 to 3, preferably i=1.
[0043] The term "predominantly" means that the at least one polymer is present in more than 50% by weight, relative to the total weight of the composition.
[0044] Advantageously, the at least one principal polymer is present in an amount greater than 60% by weight, in particular greater than 70% by weight, in particular greater than 80% by weight, more particularly greater than or equal to 90% by weight, relative to the total weight of the composition.
[0045] The composition may further comprise impact modifiers and / or additives.
[0046] The additive may be selected from antioxidants, heat stabilizers, UV absorbers, light stabilizers, lubricants, inorganic fillers, flame retardants, nucleating agents, plasticizers, dyes, carbon black, and carbonaceous nanofillers.
[0047] Advantageously, the composition consists essentially of the thermoplastic polymer P1i, 0 to 5% by weight of an impact modifier, 0 to 5% by weight of additives, the sum of the constituents of the composition being equal to 100% (based on a maximum of 90% P2i).
[0048] The at least one principal polymer in each layer may be the same or different.
[0049] In one embodiment, a single primary polymer is present in at least the sealing layer welded to the composite reinforcement layer.
[0050] Thermoplastic polymer P1i
[0051] Thermoplastics or thermoplastic polymers refer to semi-crystalline materials that are generally solid at ambient temperature and soften during temperature increase, particularly after exceeding their glass transition temperature (Tg), and may exhibit a sharp transition above what is known as their melting point (Tm), and become solid again when the temperature is reduced below their crystallization temperature.
[0052] Tg, Tc and Tm are determined by differential scanning calorimetry (DSC) according to standards 11357-2:2013 and 11357-3:2013, respectively.
[0053] The number average molecular weight Mn of the thermoplastic polymer is preferably in the range from 10 000 to 40 000, preferably from 12 000 to 30 000. These Mn values may correspond to an intrinsic viscosity greater than or equal to 0.8, as determined according to standard ISO 307:2007 but by changing the solvent in m-cresol (m-cresol is used instead of sulfuric acid and the temperature is 20° C.).
[0054] Examples of suitable semi-crystalline thermoplastic polymers in the present invention include:
[0055] Polyamides, including copolymers such as polyamide-polyether copolymers, polyesters, PVDF, and PVDF / PEI blends (where PVDF is predominant).
[0056] Very particular preference is given among the semi-crystalline polymers to polyamides and their semi-crystalline copolymers.
[0057] The nomenclature used to define polyamides is described in ISO Standard 1874-1:2011 “Plastiques—Material aux polyamides (PA) pour moulage et extrusion—Partie 1: Designation”, in particular on page 3 (Tables 1 and 2), and is familiar to the skilled person.
[0058] The polyamide may be a homopolyamide, or a copolyamide, or a mixture thereof.
[0059] Advantageously, the thermoplastic polymer is a long-chain aliphatic polyamide, ie a polyamide having an average number of carbon atoms greater than 8.5, preferably greater than 9, per nitrogen atom.
[0060] In particular, the long-chain aliphatic polyamide is selected from:
[0061] Polyamide 11 (PA11), polyamide 12 (PA12), polyamide 1010 (PA1010), polyamide 1012 (PA1012), polyamide 1212 (PA1012), or mixtures or copolyamides thereof, in particular PA11 and PA12.
[0062] Advantageously, the thermoplastic polymer is a long-chain semiaromatic polyamide, ie a polyamide having an average number of carbon atoms greater than 8.5, preferably greater than 9, per nitrogen atom and a melting point between 240 and 280°C.
[0063] In particular, the long-chain semiaromatic polyamide is selected from polyamide 11 / 5T or 11 / 6T or 11 / 10T. In this context it is obvious that the content of 11 should be carefully chosen so that the Tm of the polymer is less than 280°C, preferably less than 265°C.
[0064] Advantageously, each sealing layer consists of a composition comprising the same type of polymer, in particular a polyamide.
[0065] Advantageously, said composition comprising said polymer P1i is black in colour and is capable of absorbing radiation suitable for welding.
[0066] There are various methods for welding thermoplastic polymer parts (parts). Thus, contact or non-contact heating blades, ultrasound, infrared, vibration, rotating one element to be welded relative to the other, or even laser welding can be used.
[0067] The welding of thermoplastic polymer elements, in particular by laser welding, requires that the two elements to be welded have different properties with respect to radiation, in particular laser radiation: one of the elements must be transparent to the radiation, in particular laser radiation, and the other must absorb the radiation, in particular laser radiation. The radiation, in particular laser radiation, passes through the transparent component and then reaches the absorbing element, where it is converted into heat. This allows the contact area between the two elements to melt and thus for welding to occur.
[0068] In some applications, it is desirable that both parts to be welded be black, including parts that are transparent to laser radiation.
[0069] In order to make them absorptive, it is known to add various additives, including for example carbon black, which gives the polymer a black color and allows it to absorb radiation suitable for welding.
[0070] In one embodiment, the welding is performed by a system selected from laser, IR heating or induction heating.
[0071] In the case where the welding is carried out by laser welding, then the composition P1i comprises a non-agglomerated or non-aggregated carbonaceous filler.
[0072] In the case where welding is carried out by induction, then said composition P1i comprises metal particles.
[0073] Advantageously, the welding is performed by means of a laser system.
[0074] About composite reinforcements and thermoplastic polymers P2j
[0075] There may be one or more composite reinforcement layers.
[0076] Each of the layers consists of a composition consisting essentially of at least one thermoplastic polymer P2j, j corresponding to the number of layers present.
[0077] j comprises 1 to 10, in particular 1 to 5, especially 1 to 3, preferably j=1.
[0078] The term “predominantly” means that the at least one polymer is present in more than 50% by weight, relative to the total weight of the composition.
[0079] Advantageously, said at least one principal polymer is present in an amount greater than 60% by weight, in particular greater than 70% by weight, in particular greater than 80% by weight and more particularly greater than or equal to 90% by weight relative to the total weight of the composition.
[0080] The composition may further comprise impact modifiers and / or additives.
[0081] The additive may be selected from antioxidants, heat stabilizers, UV absorbers, light stabilizers, lubricants, inorganic fillers, flame retardants, nucleating agents, plasticizers, and dyes.
[0082] Advantageously, said composition consists essentially of said thermoplastic polymer P2j, 0 to 5% by weight of impact modifier, 0 to 5% by weight of additives, the sum of the constituents of the composition being equal to 100% (based on a maximum of 90% of P2j).
[0083] The at least one principal polymer in each layer may be the same or different.
[0084] In one embodiment, a single primary polymer is present in at least the composite reinforcement layer that is welded to the sealing layer.
[0085] In one embodiment, each reinforcement layer comprises the same type of polymer, in particular polyamide.
[0086] Thermoplastic polymer P2j
[0087] Thermoplastics or thermoplastic polymers are intended to mean materials which are generally solid at ambient temperature, which may be semicrystalline or amorphous, in particular semicrystalline, and which soften during temperature increase, in particular after exceeding their glass transition temperature (Tg), and flow at higher temperatures when they are amorphous, or which may exhibit precise melting as soon as their melting point (Tm) is exceeded when they are semicrystalline, and which become solid again when the temperature is reduced to below their crystallization temperature (for semicrystalline) or below their glass transition temperature (for amorphous).
[0088] Tg, Tc, and Tm are determined by differential scanning calorimetry (DSC) according to standards 11357-2:2013 and 11357-3:2013, respectively.
[0089] The polymer P2j of the composition of at least one of the composite reinforcing layers is such that its Tg is greater than the maximum use temperature (Tu) of the structure and in particular Tg ≥ Tu + 20°C.
[0090] In one embodiment, polymer P2j has a Tg ≥ Tu + 20° C., regardless of the position of the reinforcement layer.
[0091] In another embodiment, the reinforcement layer consisting of the composition comprising a polymer P2j having a Tg ≥ Tu + 20° C. is the layer welded to the sealing layer.
[0092] In another embodiment, the reinforcing layer consisting of a composition comprising a polymer P2j having a Tg ≥ Tu + 20° C. is the outermost reinforcing layer of the structure. The number average molecular weight Mn of the thermoplastic polymer is preferably in the range from 10 000 to 40 000, preferably from 12 000 to 30 000. These Mn values may correspond to an intrinsic viscosity greater than or equal to 0.8, as determined according to standard ISO 307:2007 but by changing the solvent in m-cresol (m-cresol is used instead of sulfuric acid and the temperature is 20° C.).
[0093] Examples of suitable semi-crystalline thermoplastic polymers in the present invention include:
[0094] Polyamides, in particular polyamides containing aromatic and / or cycloaliphatic structures, including copolymers, for example polyamide-polyether copolymers, polyesters,
[0095] Polyaryletherketone (PAEK),
[0096] Polyetheretherketone (PEEK),
[0097] Polyetherketoneketone (PEKK),
[0098] Polyetherketoneetherketoneketone (PEKEKK),
[0099] Polyimides, in particular polyetherimide (PEI) or polyamide-imide,
[0100] Polysulfones (PSU), in particular polyarylsulfones, such as polyphenylsulfone (PPSU),
[0101] Polyethersulfone (PES).
[0102] Semicrystalline polymers are more particularly preferred, and in particular polyamides and semicrystalline copolymers thereof.
[0103] The nomenclature used to define polyamides is described in ISO Standard 1874-1:2011 “Plastiques—Material aux polyamides (PA) pour moulage et extrusion—Partie 1: Designation”, in particular on page 3 (Tables 1 and 2), and is familiar to the skilled person.
[0104] The polyamide may be a homopolyamide, or a copolyamide, or a mixture thereof.
[0105] Advantageously, the semicrystalline polyamide is a semiaromatic polyamide, in particular a semiaromatic polyamide of formula X / YAr as described in EP1505099, in particular a semiaromatic polyamide of formula A / XT, in which A is chosen from units obtained from amino acids, units obtained from lactams, and units corresponding to the formula (Ca diamine).(Cb diacid), in which a represents the number of carbon atoms of the diamine and b represents the number of carbon atoms of the diacid, a and b are each between 4 and 36, advantageously between 9 and 18, the units (Ca diamine) are chosen from linear or branched aliphatic diamines, cycloaliphatic diamines and alkylaromatic diamines, and the units (Cb diacid) are chosen from linear or branched aliphatic diacids, cycloaliphatic diacids and aromatic diacids;
[0106] XT represents a unit obtained by the polycondensation of a Cx diamine and terephthalic acid, wherein x represents the number of carbon atoms of the Cx diamine, x being between 6 and 36, advantageously between 9 and 18, especially a polyamide of formula A / 6T, A / 9T, A / 10T, or A / 11T, A being as defined above, in particular a polyamide selected from the group consisting of PA MPMDT / 6T, PA 11 / 10T, PA 5T / 10T, PA 11 / BACT, PA 11 / 6T / 10T, PA MXDT / 10T, PA MPMDT / 10T, PA BACT / 10T, PA BACT / 6T, PA BACT / 10T / 6T, PA 11 / BACT / 6T, PA 11 / MPMDT / 6T, PA 11 / MPMDT / 10T, PA 11 / BACT / 10T, PA 11 / MXDT / 10T, 11 / 5T / 10T.
[0107] T corresponds to terephthalic acid, MXD corresponds to meta-xylylenediamine, MPMD corresponds to methylpentamethylenediamine, and BAC corresponds to bis(aminomethyl)cyclohexane.
[0108] Advantageously, each composite reinforcing layer consists of a composition comprising the same type of polymer, in particular a polyamide.
[0109] Advantageously, said composition comprising said polymer P2j is transparent to radiation suitable for welding.
[0110] For the purposes of welding, especially laser welding, thermoplastic polymers are generally transparent. Carbonaceous nanofillers make it possible to impart a black color to a layer of a composition comprising a thermoplastic polymer while maintaining the transparency of said layer to laser radiation.
[0111] Advantageously, the carbonaceous nanofiller is non-agglomerated or non-aggregated.
[0112] Advantageously, the carbonaceous nanofiller is incorporated into the composition in an amount ranging from 100 ppm to 500 ppm and preferably from 100 ppm to 250 ppm.
[0113] Advantageously, the carbonaceous nanofiller is selected from carbon nanotubes (CNTs), carbon nanofibers, graphene, nanoscale carbon black, and mixtures thereof.
[0114] Advantageously, the carbonaceous nanofiller does not contain nano carbon black.
[0115] In one embodiment, the welding is performed by a system selected from laser, IR heating, or induction heating.
[0116] Advantageously, the welding is performed by a laser system.
[0117] Advantageously, the laser radiation is infrared laser radiation and preferably has a wavelength between 700 nm and 1200 nm and preferably between 800 nm and 1100 nm.
[0118] About Structure
[0119] Thus, the multilayer structure comprises at least one sealing layer and at least one composite reinforcement layer welded together.
[0120] In one embodiment, in the multilayer structure, each polymer P1i of each sealing layer is partially or completely miscible with each polymer P1i of an adjacent layer, each polymer P2j of each reinforcing layer is partially or completely miscible with each polymer P2j of an adjacent layer, and each polymer P2j is partially or completely miscible with each polymer P1i (when they are adjacent), and polymer P21 is partially or completely miscible with polymer P11 adjacent to it, and the complete or partial miscibility of the polymers is defined by the difference in glass transition temperature of the two resins in the mixture relative to the difference in glass transition temperature of the two resins before mixing, and the miscibility is complete when the difference is equal to 0, and the miscibility is partial when the difference is different from 0, excluding the immiscibility of polymer P2j and polymer P1i.
[0121] When the miscibility of the polymers is partial, the difference is such that the greater the miscibility, the smaller the difference.
[0122] Advantageously, when the miscibility of said polymers is partial, said difference is less than 30%, preferentially less than 20%, in absolute terms.
[0123] In one embodiment, the glass transition temperature of the mixture, depending on whether the miscibility is complete or partial, is necessarily between the glass transition temperatures of the polymers before blending and differs therefrom by at least 5°C, preferably at least 10°C.
[0124] The expression "completely miscible" means that when, for example, two polymers P11 and P12, having Tg11 and Tg12 respectively, are present in two adjacent sealing layers or two adjacent reinforcing layers, the mixture of the two polymers has only one Tg1112, whose value is between Tg11 and Tg12.
[0125] Furthermore, this Tg1112 value is at least 5°C, in particular at least 10°C greater than Tg11, and at least 5°C, in particular at least 10°C lower than Tg12.
[0126] The expression "partially miscible" means that when, for example, two polymers P11 and P12 (having Tg11 and Tg12, respectively) are present in two adjacent sealing layers or two adjacent reinforcing layers, respectively, the mixture of the two polymers has two Tg'11 and Tg'12, wherein Tg11 <Tg’11<Tg’12<Tg12。
[0127] Furthermore, these Tg'11 and Tg'12 values are at least 5°C, particularly at least 10°C greater than Tg11, and at least 5°C, particularly at least 10°C lower than Tg12.
[0128] The immiscibility of the two polymers results in the presence of two Tg's in the mixture of the two polymers: Tg11 and Tg12, which correspond to the respective Tg's, Tg11 and Tg12, of the pure polymers taken separately.
[0129] Advantageously, the welded sealing layer and the reinforcing layer are made of compositions comprising different polymers, respectively.
[0130] Nevertheless, the different polymers may be of the same type.
[0131] Thus, if one of the two welded composite reinforcement and sealing layers is made of a composition comprising an aliphatic polyamide, the other layer is made of a composition comprising a polyamide that is non-aliphatic and is, for example, a semiaromatic polyamide, to have a high Tg polymer as matrix for the composite reinforcement.
[0132] The multilayer structure may comprise up to 10 sealing layers and up to 10 composite reinforcement layers.
[0133] It is obvious that the multilayer structure does not have to be symmetrical and it may therefore comprise more sealing layers than composite layers, or vice versa.
[0134] Advantageously, the multilayer structure comprises one, two, three, four, five, six, seven, eight, nine, or ten sealing layers and one, two, three, four, five, six, seven, eight, nine, or ten composite reinforcement layers.
[0135] Advantageously, the multilayer structure comprises one, two, three, four or five sealing layers and one, two, three, four or five composite reinforcement layers.
[0136] Advantageously, the multilayer structure comprises one, two, or three sealing layers, and one, two, or three composite reinforcement layers.
[0137] Advantageously, they consist of compositions each comprising different polymers.
[0138] Advantageously, they consist of a composition comprising the polyamides corresponding to polyamides P1i and P2j, respectively.
[0139] Advantageously, they consist of compositions each comprising different polyamides.
[0140] In one embodiment, the multilayer structure comprises a single sealing layer and several reinforcement layers, the sealing layer being welded to the adjacent reinforcement layers.
[0141] In another embodiment, the multilayer structure comprises a single reinforcement layer and several sealing layers, the reinforcement layer being welded to the adjacent sealing layers.
[0142] In an advantageous embodiment, the multilayer structure comprises a single sealing layer and a single composite reinforcement layer that are welded.
[0143] Therefore, all combinations of these two layers are within the scope of the present invention, provided that at least the innermost composite reinforcement layer is fused to the outermost adjacent sealing layer, and the other layers are either fused together or not fused together.
[0144] Advantageously, in said multilayer structure, each sealing layer consists of a composition comprising polymers P1i of the same type, in particular polyamides.
[0145] The expression "same type of polymer" means, for example, polyamide which may be the same or different polyamide depending on the layer.
[0146] Advantageously, said polymer P1i is a polyamide and said polymer P2j is a polyamide.
[0147] Advantageously, the polyamide P1i is the same for all sealing layers.
[0148] Advantageously, the polymer P1i is a long-chain aliphatic polyamide, in particular PA1010, PA 1012, PA 1212, PA11, PA12, especially PA 11 or PA12.
[0149] Advantageously, the polyamide P1i is a long-chain semiaromatic polyamide, in particular PA 11 / 5T, PA 11 / 6T or PA 11 / 10T. In this case it is obvious that the content of 11 must be carefully chosen so that the Tm of the polymer is less than 280°C, in particular less than 265°C.
[0150] Advantageously, in said multilayer structure, each reinforcing layer consists of a composition comprising the same type of polymer P2j, in particular a polyamide.
[0151] Advantageously, the polyamide P2j is the same for all the reinforcement layers.
[0152] Advantageously, the polymer P2j is a semiaromatic polyamide, in particular chosen from PA MXDT / 6T, PA11 / 10T, PA 11 / BACT, PA 5T / 10T, PA 11 / 6T / 10T, PA MXDT / 10T, PA MPMDT / 10T, PA BACT / 10T, PA BACT / 6T, PA BACT / 10T / 6T, PA11 / BACT / 6T, PA 11 / MPMDT / 6T, PA 11 / MPMDT / 10T, PA 11 / BACT / 10T, PA11 / MXDT / 10T and PA 5T / 10.
[0153] Advantageously, in said multilayer structure, each sealing layer consists of a composition comprising the same type of polymer P1i, in particular a polyamide, and each reinforcing layer consists of a composition comprising the same type of polymer P2j, in particular a polyamide, with the proviso that the polyamides P1i and P2j are different, i.e. if the sealing layer consists of a composition comprising a long-chain aliphatic polyamide, then the sealing layer consists of a composition comprising a semiaromatic polyamide.
[0154] Advantageously, the polymer P1i is a long-chain aliphatic polyamide, in particular PA1010, PA 1012, PA 1212, PA11, PA12, especially PA 11 or PA12, and the polymer P2j is a semiaromatic polyamide, in particular chosen from PA MPMDT / 6T, PA PA11 / 10T, PA 11 / BACT, PA 5T / 10T, PA 11 / 6T / 10T, PA MXDT / 10T, PA MPMDT / 10T, PABACT / 10T, PA BACT / 6T, PA BACT / 10T / 6T, PA 11 / BACT / 6T, PA 11 / MPMDT / 6T, PA 11 / MPMDT / 10T, PA 11 / BACT / 10T, PA 11 / MXDT / 10T and PA 5T / 10T.
[0155] Advantageously, the multilayer structure consists of a single reinforcement layer and a single sealing layer, wherein the polymer P1i is a long-chain aliphatic polyamide, in particular PA1010, PA 1012, PA 1212, PA11, PA12, especially PA 11 or PA12, and the polymer P2j is a semi-aromatic polyamide, in particular chosen from PA MPMDT / 6T, PA PA11 / 10T, PA 11 / BACT, PA 11 / 6T / 10T a PA MXDT / 10T, PA MPMDT / 10T, PA BACT / 10T, PA BACT / 6T, PA BACT / 10T / 6T, PA11 / BACT / 6T, PA 11 / MPMDT / 6T, PA 11 / MPMDT / 10T, PA 11 / BACT / 10T, PA11 / MXDT / 10T.
[0156] Advantageously, the multilayer structure is a flexible pipe.
[0157] The maximum use temperature Tu of the multilayer structure is 50° C. or higher, particularly 100° C. or higher.
[0158] In one embodiment, the multilayer structure defined above has reduced pressure resistance and drying capability.
[0159] Indeed, when storing or transporting gases, said gases may diffuse from the interior of the pipeline or tank through the sealing layers, due to their permeability to the gases transported or stored, to the interface between the final sealing layer and the first composite reinforcement. The accumulation of gases at this location may generate pressures which, when the internal pressure of the pipeline or tank is lower than the pressure at the interface with the composite reinforcement (this may occur in particular when the pumping or transport of the gas is stopped during a production stoppage, resulting in a pressure drop of several hundred bars to atmospheric pressure, or when the storage tank is empty), will lead to a collapse of the sealing layer. The same applies during internal hydrostatic testing of the tank: this water may migrate by permeation to the interface between the composite reinforcement and the final sealing layer and will then be very difficult to remove, leading to long and expensive drying cycles of said storage tank, especially under vacuum.
[0160] In another embodiment, the multilayer structure defined above further comprises a metal skeleton located within the sealing layer.
[0161] This metal skeleton is not leak-proof and is the innermost layer.
[0162] Advantageously, the multilayer structure further comprises at least one outer layer, in particular a metal layer, said layer being the outermost layer of the multilayer structure.
[0163] The outer layer is a second reinforcement layer, but is metallic rather than composite (composite).
[0164] There may also be a polymeric protective layer (outermost layer) on the structure which has an anti-wear effect or which allows an inscription to be placed on the structure.
[0165] About Fibrous Materials
[0166] As regards the fibres constituting the fibrous material, they are in particular mineral, organic or vegetable fibres.
[0167] Advantageously, the fibrous material may be sized or unsized.
[0168] Thus, the fibrous material may contain up to 0.1% by weight of an organic material (thermosetting or thermoplastic resin type) known as a sizing.
[0169] Among the fibers of mineral origin, mention may be made, for example, of carbon fibers, glass fibers, basalt fibers or fibers based on basalt, silica fibers, or silicon carbide fibers. Organic fibers include fibers based on thermoplastic or thermosetting polymers, such as semi-aromatic polyamide fibers, aramid fibers, or polyolefin fibers. Preferably, they are based on amorphous thermoplastic polymers and have a glass transition temperature Tg that is higher than the Tg of the polymer or thermoplastic polymer mixture constituting the prepreg matrix (when the latter is amorphous), or that is higher than the Tm of the polymer or thermoplastic polymer mixture constituting the prepreg matrix (when the latter is semi-crystalline). Advantageously, they are based on semi-crystalline thermoplastic polymers and have a melting temperature Tm that is higher than the Tg of the polymer or thermoplastic polymer mixture constituting the prepreg matrix (when the latter is amorphous), or that is higher than the Tm of the polymer or thermoplastic polymer mixture constituting the prepreg matrix (when the latter is semi-crystalline). Thus, there is no risk of melting of the organic fibers constituting the fibrous material during the impregnation with the thermoplastic matrix of the final composite. The plant fibers include natural flax, hemp, lignin, bamboo, silk, in particular spider silk, sisal, and other cellulosic fibers, in particular viscose. These plant fibers can be used pure, treated, or coated with a coating to facilitate the attachment and impregnation of the thermoplastic polymer matrix.
[0170] The fibrous material may also be woven, knitted, or woven from fibers.
[0171] It may correspond to a fiber having a support thread.
[0172] These component fibers can be used alone or in a mixture. Thus, organic fibers can be mixed with mineral fibers to be pre-impregnated with thermoplastic polymer powder and form a pre-impregnated fibrous material.
[0173] The organic fiber strands may have several grammages. They may further have several geometric shapes. The constituent fibers of the fibrous material may further be in the form of a mixture of these reinforcing fibers having different geometric shapes.
[0174] The fibers are continuous fibers.
[0175] The fibrous material is preferably selected from glass fibers, carbon fibers, basalt fibers and basalt-based fibers.
[0176] More advantageously, the fibrous material is selected from carbon fibers, basalt fibers and basalt-based fibers.
[0177] It is used in the form of a roving or several rovings.
[0178] According to another aspect, the invention relates to a method for manufacturing a multilayer structure as defined above, characterized in that it comprises a step of welding a reinforcing layer as defined above to a sealing layer as defined above.
[0179] Advantageously, the welding step is performed by a system chosen from laser, infrared heating, or induction heating.
[0180] Advantageously, the method comprises a step of extruding the sealing layer onto the metal skeleton and a step of welding the reinforcing layer onto the sealing layer.
[0181] According to another aspect, the invention relates to the use of a multilayer structure selected from tanks or pipes or pipelines for the production of tanks or pipelines for the transport or storage of gases or for the exploitation of oil or gas fields on the seabed, excluding the transport or storage of hydrogen, and of tanks or pipelines or pipelines for the transport or storage of gases, the multilayer structure comprising, from the inside to the outside, at least one sealing layer as defined above and at least one composite reinforcement layer as defined above,
[0182] The innermost composite reinforcement layer is welded to the outermost adjacent sealing layer,
[0183] The sealing layer is composed of a composition that mainly comprises at least one semi-crystalline thermoplastic polymer P1i (i=1 to n, n is the number of sealing layers), whose Tm measured according to ISO 11357-3:2013 is less than 280°C, in particular less than 265°C,
[0184] The at least one thermoplastic polymer of each sealing layer may be identical or different, and at least one of the composite reinforcement layers consists of a fibrous material in the form of continuous fibers, which is impregnated with a composition that essentially comprises at least one thermoplastic polymer P2j (in particular semi-crystalline), (j=1 to m, m being the number of reinforcement layers), the thermoplastic polymer P2j having a Tg greater than the maximum use temperature (Tu) of the structure measured according to ISO11357-3:2013, wherein Tg≥Tu+20°C, in particular Tg≥Tu+30°C, Tu is greater than 50°C, in particular greater than 100°C,
[0185] Also excluded are multilayer structures selected from tanks, pipes or pipelines for transporting or storing hydrogen. Example
[0186] In all the examples, the tanks are obtained by rotomoulding of the liner at a temperature adapted to the nature of the thermoplastic resin used, but in all cases below 280°C.
[0187] The pipes are obtained by extrusion of the liner at a temperature adapted to the nature of the thermoplastic resin used, but in all cases below 280°C.
[0188] In the case of epoxy, a wet filament winding process is used, which consists of winding a fiber around the mat, the fiber being pre-impregnated in a bath of liquid epoxy. The tank is then polymerized in an oven for 2 hours.
[0189] In all other cases, a fibrous material (tape) previously impregnated with a thermoplastic resin was used. This tape was deposited by filament winding at a speed of 12 m / min using an automatic machine including a 1500 W laser heater.
[0190] Embodiment 1 (comparative example):
[0191] Flexible wastewater transport pipeline (offshore application) consisting of epoxy (Tg 130°C)-T700SC31E carbon fiber composite reinforcement and HDPE sealing layer: there is no miscibility between the two resins (see Table I), which hinders any welding between the fibrous reinforcement and the sealing layer.
[0192] Example 2: Type IV or V gas (natural gas) storage tank consisting of BACT / 10T-T700SC31E carbon fiber composite reinforcement and PA6 sealing layer: good partial miscibility between the two resins (see Table 1), which allows good welding between the fibrous reinforcement and the sealing layer.
[0193] Example 3: Type IV or V gas (natural gas) storage tank consisting of BACT / 10T-T700SC31E carbon fiber composite reinforcement and PA66 sealing layer: good partial miscibility between the two resins (see Table 1), which allows good welding between the fibrous reinforcement and the sealing layer.
[0194] Example 4: Flexible pipe for pumping oil, consisting of BACT / 10T-T700SC31E carbon fiber composite reinforcement and PA11 sealing layer deposited on an internal metal skeleton: low partial miscibility between the two resins (see Table 1), which leads to low-quality welding between the fibrous reinforcement and the sealing layer.
[0195] Example 5: Flexible pipe for pumping oil, consisting of 11 / BACT / 10T-T700SC31E carbon fiber composite reinforcement and PA11 sealing layer deposited on an internal metal skeleton: good partial miscibility between the two resins (see Table 1), which leads to good welding between the fibrous reinforcement and the sealing layer.
[0196] In all examples in Table 1 below, to evaluate the miscibility of the resins, the mixtures were made from powders with a particle size of about 150 μm on a micro DSM with a recirculation time of 1 minute after melting. All mixtures were made at 300°C, except for the epoxy-polyethylene mixture, which was made at 220°C.
[0197] At the end of the mixing process, the mixture is injected into a mold to produce a test piece that will be characterized in the DMA.
[0198] Table 1
[0199]
[0200] Miscibility test results:
[0201] - Column 4: Glass transition temperature of each resin before mixing
[0202] - Column 5: Glass transition temperature of the resin in the mixture
[0203] - Column 6: Ratio between the difference in glass transition temperature of the resins in the mixture and before mixing.
[0204] 100% indicates the immiscibility of the resin,
[0205] <80% indicates low miscibility,
[0206] <30% indicates good but partial miscibility,
[0207] 0 indicates complete miscibility.
Claims
1. A multilayer structure selected from a tank or a pipeline for transporting or storing gas or for exploiting oil or gas fields on the seabed, comprising from the inside to the outside at least one sealing layer and at least one composite reinforcement layer, The innermost composite reinforcement layer is welded to the outermost adjacent sealing layer, The sealing layer is composed of the following composition: The composition mainly comprises at least one semi-crystalline thermoplastic polymer P1i, i=1 to n, n being the number of sealing layers, having a Tm measured according to ISO 11357-3: 2013 of less than 280°C, The at least one thermoplastic polymer of each sealing layer may be the same or different, and at least one of the composite reinforcement layers consists of a fibrous material in the form of continuous fibers, which is impregnated with a composition that essentially comprises at least one thermoplastic polymer P2j, j=1 to m, m being the number of reinforcement layers, the thermoplastic polymer P2j having a Tg greater than the maximum use temperature (Tu) of the structure measured according to ISO 11357-3: 2013, wherein Tg ≥ Tu+ 20°C, Tu is greater than 50°C, Excluding hydrogen from the gas transport or gas storage, and excluding a multilayer structure selected from a tank or a pipeline for transporting or storing hydrogen, The polymer P1i is a long-chain aliphatic polyamide or a semi-aromatic polyamide, and the polymer P2j is a semi-aromatic polyamide.
2. The multilayer structure according to claim 1, wherein the multilayer structure is a pipeline for transporting or storing gas or for exploiting oil or gas fields on the seabed, and excludes multilayer structures selected from pipelines for transporting or storing hydrogen.
3. The multilayer structure according to claim 1, wherein the semi-crystalline thermoplastic polymer P1i has a Tm measured according to ISO 11357-3: 2013 of less than 265°C.
4. The multilayer structure according to claim 1, wherein the thermoplastic polymer P2j is a semicrystalline thermoplastic polymer P2j.
5. The multilayer structure according to claim 1, wherein Tu is greater than 100°C.
6. A multilayer structure according to claim 1, wherein each polymer P1i of each sealing layer is partially or completely miscible with each polymer P1i of an adjacent layer, each polymer P2j of each reinforcing layer is partially or completely miscible with each polymer P2j of an adjacent layer, and polymer P21 is partially or completely miscible with polymer P11 adjacent thereto, The complete or partial miscibility of the polymers is defined by the difference in the glass transition temperatures of the two resins in the mixture relative to the difference in the glass transition temperatures of the two resins before mixing, the miscibility being complete when the difference is equal to 0 and partial when the difference is different from 0.
7. The multilayer structure according to any one of claims 1 to 6, characterized in that Each sealing layer comprises the same type of polymer.
8. The multilayer structure according to claim 7, characterized in that The same type of polymer is polyamide.
9. The multilayer structure according to any one of claims 1 to 6, characterized in that Each reinforcement layer comprises the same type of polymer.
10. The multilayer structure according to claim 9, characterized in that The same type of polymer is polyamide.
11. The multilayer structure according to any one of claims 1 to 6, characterized in that Each sealing layer comprises the same type of polymer, and each reinforcing layer comprises the same type of polymer.
12. The multilayer structure according to claim 11, characterized in that The same type of polymer in each sealing layer is polyamide, and the same type of polymer in each reinforcing layer is polyamide.
13. The multilayer structure according to any one of claims 1 to 6, characterized in that It has a single sealing layer and a single reinforcement layer.
14. The multilayer structure according to any one of claims 1 to 6, characterized in that The structure is a flexible pipe.
15. The multilayer structure according to any one of claims 1 to 6, characterized in that The composition comprising the polymers P1 and P2 also comprises additives enabling them to absorb radiation suitable for welding.
16. The multilayer structure according to claim 15, characterized in that The additive is selected from carbon black, carbon nanotubes (CNT), or graphene.
17. The multilayer structure according to any one of claims 1 to 6, characterized in that Said composition comprising said polymer P2j is transparent to radiation suitable for welding.
18. The multilayer structure according to any one of claims 1 to 6, characterized in that The welding is performed by a system selected from laser, IR heating or induction heating.
19. The multilayer structure according to any one of claims 1 to 6, characterized in that The polymer P1i is a long-chain aliphatic polyamide selected from PA1010, PA1012, PA1212, PA11, PA12; or a semi-aromatic one selected from PA11 / 5T, PA11 / 6T, and PA11 / 10T.
20. The multilayer structure according to claim 19, characterized in that The polymer P1i is a long-chain aliphatic polyamide selected from PA 11 or PA12.
21. The multilayer structure according to any one of claims 1 to 6, characterized in that The polymer P2j is a semi-aromatic polyamide selected from PA MPMDT / 6T, PA 11 / 10T, PA 11 / BACT, PA 5T / 10T, PA 11 / 6T / 10T, PA MXDT / 10T, PAMPMDT / 10T, PA BACT / 10T, PA BACT / 6T, PA BACT / 10T / 6T, PA 11 / BACT / 6T, PA 11 / MPMDT / 6T, PA 11 / MPMDT / 10T, PA 11 / BACT / 10T, PA 11 / MXDT / 10T, PA11 / 5T / 10T.
22. The multilayer structure according to any one of claims 1 to 6, characterized in that The polymer P1i is a long chain aliphatic polyamide selected from PA1010, PA 1012, PA 1212, PA11, PA12, or a semiaromatic one selected from PA 11 / 5T, PA 11 / 6T, or PA 11 / 10T; and the polymer P2j is a semiaromatic polyamide selected from PA MPMDT / 6T, PA PA11 / 10T, PA11 / BACT, PA 5T / 10T, PA 11 / 6T / 10T, PA MXDT / 10T, PA MPMDT / 10T, PA BACT / 10T, PA BACT / 6T, PA BACT / 10T / 6T, PA 11 / BACT / 6T, PA 11 / MPMDT / 6T, PA 11 / MPMDT / 10T, PA 11 / BACT / 10T, PA 11 / MXDT / 10T, PA11 / 5T / 10T.
23. The multilayer structure according to claim 22, characterized in that The polymer P1i is a long-chain aliphatic polyamide selected from PA 11 or PA12.
24. The multilayer structure according to any one of claims 1 to 6, characterized in that It has reduced pressure tolerance and drying capabilities.
25. The multilayer structure according to any one of claims 1 to 6, characterized in that The structure further comprises a metal skeleton located within the sealing layer.
26. The multilayer structure according to any one of claims 1 to 6, characterized in that The structure further comprises at least one outer layer.
27. The multilayer structure according to claim 26, characterized in that The at least one outer layer is a metal layer, and the metal layer is the outermost layer of the multilayer structure.
28. The multilayer structure according to any one of claims 1 to 6, characterized in that The fibrous material is selected from the group consisting of glass fibers, carbon fibers, basalt fibers, and basalt-based fibers.
29. Method for producing a multilayer structure as defined in any one of claims 1 to 28, characterized in that It comprises the step of welding a reinforcing layer as defined in claim 1 to a sealing layer as defined in claim 1 .
30. The method according to claim 29, characterized in that The welding step is performed by a system selected from laser, infrared heating or induction heating.
31. The method according to claim 29 or 30, characterized in that The method comprises the steps of extruding the sealing layer onto the metal skeleton and welding the reinforcing layer onto the sealing layer.
Citation Information
Patent Citations
Method for manufacturing continuous composite tube, apparatus for manufacturing continuous composite tube
WO2012118379A1
Polyamide-based composition for pipes containing oil or gas
CN109071803A
Semi-aromatic polyamides with low moisture regain
CN1590461A
Assembly method and a plastic composite tube
CN1638946A