Heterogeneous semiconductor nanoparticles and method for preparing triboelectric film

By using TiO2@Cu2O heterosemiconductor nanoparticles in the triboelectric nanogenerator, the wavelength range of photogenerated carriers is broadened, the problems of low output power and inconvenient control of the triboelectric nanogenerator are solved, and efficient output performance and real-time performance are achieved. Control, suitable for a variety of application scenarios.

CN114249296BActive Publication Date: 2024-10-01HEBEI UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111556887.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-18
Publication Date
2024-10-01
Estimated Expiration
2041-12-18

AI Technical Summary

Technical Problem

Triboelectric nanogenerators have problems in engineering applications such as low output power, low surface charge density, serious charge leakage, and inconvenient control. Existing technology cannot effectively improve its output performance and real-time control capabilities.

Method used

Heterogeneous semiconductor nanoparticles TiO2@Cu2O are used. By uniformly loading Cu2O nanoparticles on the surface of TiO2 particles, the narrow band gap semiconductor Cu2O is used to sensitize the wide band gap semiconductor TiO2 to broaden the wavelength range of photogenerated carriers and improve the surface charge of the triboelectric film. Density and dielectric properties to achieve broad spectrum control of triboelectric films.

Benefits of technology

It improves the output performance and control spectral bandwidth of the triboelectric nanogenerator, realizes real-time control of the output performance, enhances the carrier concentration and charge capture capability, and is suitable for mechanical vibration energy collection and self-power supply systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114249296B_ABST
    Figure CN114249296B_ABST
Patent Text Reader

Abstract

The invention relates to a heterogeneous semiconductor nanoparticle and a method for preparing a triboelectric film. The method for preparing the heterogeneous semiconductor nanoparticle comprises the following steps: dissolving copper acetate powder in anhydrous ethanol, adding TiO2 powder, dispersing, stirring and degassing to obtain a suspension A, heating the suspension, adding glucose solution and NaOH solution to obtain a suspension B; drying the suspension B with a centrifugal dryer to obtain a precipitate, washing the precipitate with anhydrous ethanol and finally drying the suspension; the method for preparing the triboelectric film comprises the following steps: adding the heterogeneous semiconductor nanoparticle to liquid polydimethylsiloxane, mixing the mixture with a curing agent and obtaining a component B; weighing the polydimethylsiloxane again, adding a curing agent and obtaining a component C; firstly spin-coating the component C on an electrode surface, then spin-coating the component B on the surface of the component C, and finally drying the mixture; the invention realizes wide spectrum regulation of surface charge density of the triboelectric film and improves its dielectric properties.
Need to check novelty before this filing date? Find Prior Art

Description

(I) Technical field:

[0001] The invention relates to heterogeneous semiconductor nanoparticles and a method for preparing a triboelectric film. (II) Background technology:

[0002] With the rapid development of new generation information technologies such as the Internet of Things, big data, and artificial intelligence, the demand for various sensors for interactive communication has increased dramatically. How to solve the power supply problem of massive sensor nodes has become a bottleneck in the development of modern information technology. Through energy harvesting technology, the abundant and widely distributed renewable clean energy in the environment is converted into electrical energy to power wireless sensor network nodes, which is an effective solution to break the limitations of traditional power supply methods. As a new disruptive energy harvester, the triboelectric nanogenerator (TENG) has unprecedented output performance and relatively low cost, and has been proven to be one of the effective ways to achieve efficient acquisition and conversion of environmental energy. However, in the process of engineering application of triboelectric nanogenerators, there is a problem of low output power, which has become a bottleneck for its further promotion and application. The surface charge density of the friction material is a key factor affecting the output power of the triboelectric nanogenerator. At present, although the existing technologies such as surface morphology modification, high dielectric nanoparticle doping, chemical functional group grafting, charge injection, and light regulation enhancement have optimized the electrification properties of the triboelectric nanogenerator to a certain extent, the triboelectric nanogenerator still has bottleneck problems such as low surface charge density, serious charge leakage, and poor robustness. Moreover, these technologies cannot achieve real-time and effective regulation of the friction surface charge. Although the emerging light-controlled friction surface charge technology can, to a certain extent, control the output performance of the friction nanogenerator in real time through light, it still has problems such as small electrical output, narrow control spectrum (surface plasmon resonance can only be excited at a certain wavelength, and the photogenerated carrier (hot electron-hole pair) effect of broadband semiconductor TiO2 can only be excited by ultraviolet light), and low light energy utilization efficiency. The band gap width of semiconductor TiO2 is 3.2eV. When semiconductor TiO2 is irradiated with light with energy greater than the band gap width, the electrons in its valence band are excited and transition to the conduction band, generating corresponding holes in the valence band, thereby generating hot electron-hole pairs. At present, semiconductor TiO2 can only be excited by ultraviolet light, and the concentration of carriers (hot electron-hole pairs) it generates is low. (III) Summary of the invention:

[0003] The technical problem to be solved by the present invention is: to provide a heterogeneous semiconductor nanoparticle and a method for preparing a triboelectric film, wherein the Cu2O nanoparticles in the heterogeneous semiconductor nanoparticles are uniformly loaded on the surface of the TiO2 particles, such a structure can not only effectively increase the contact interface between the Cu2O nanoparticles and the TiO2 particles, but also can ensure that the Cu2O nanoparticles and the TiO2 particles fully receive light at the same time, and the method for preparing the triboelectric film modifies the triboelectric film by doping the heterogeneous semiconductor nanoparticles, thereby realizing wide spectrum regulation of the surface charge density of the triboelectric film, improving the dielectric properties of the triboelectric film, and making the triboelectric nanogenerator using the triboelectric film have the advantages of good output performance, wide spectrum regulation, real-time, simplicity and reliability.

[0004] The technical solution of the present invention:

[0005] A method for preparing heterogeneous semiconductor nanoparticles, specifically comprising:

[0006] Step 1. Weigh copper acetate powder, and then dissolve the copper acetate powder in anhydrous ethanol to obtain a mixed solution A; wherein 1g of copper acetate powder is added to 80mL to 100mL of anhydrous ethanol;

[0007] Step 2: Firstly, the mixed solution A is dispersed by an ultrasonic disperser, and then stirred and degassed in sequence;

[0008] Step 3, weigh TiO2 powder, add the TiO2 powder to the mixed solution A treated in step 2, to obtain a mixed solution B; wherein the particle size of the TiO2 powder is 50nm to 200nm, and 1g of TiO2 powder is added to 4mL to 5mL of the mixed solution A treated in step 2;

[0009] Step 4: First, the mixed solution B is dispersed by an ultrasonic disperser, and then stirred and degassed in sequence to obtain a suspension A, and the suspension A is heated to 60° C. to 80° C. in a water bath;

[0010] Step 5: Add glucose solution to suspension A, and then add NaOH solution to obtain suspension B; wherein the concentration of glucose solution is 0.1mol / L to 1mol / L, which is used to adjust the particle size of Cu2O, the concentration of NaOH solution is 0.1mol / L to 1mol / L, and the volume ratio of suspension A, NaOH solution and glucose solution is 1:1.5 to 3:1 to 2;

[0011] Step 6: Dry the suspension B with a centrifugal dryer to obtain a precipitate, then wash the precipitate with anhydrous ethanol, and finally dry the washed precipitate in a vacuum drying oven at 60°C to 120°C to obtain heterogeneous semiconductor nanoparticles.

[0012] The heterogeneous semiconductor nanoparticles are TiO2@Cu2O heterogeneous semiconductor nanoparticles, and the Cu2O nanoparticles are uniformly loaded on the surface of the TiO2 particles.

[0013] In step 2, the dispersion treatment time is 10 minutes to 30 minutes, the stirring treatment time is 5 minutes to 15 minutes, and the degassing treatment time is 30 seconds to 120 seconds;

[0014] In step 4, the dispersion treatment time is 10 minutes to 30 minutes, the stirring treatment time is 5 minutes to 15 minutes, and the degassing treatment time is 30 seconds to 120 seconds.

[0015] In step 6, the precipitate is washed 5 to 8 times with anhydrous ethanol, and the drying time is 24 to 30 hours.

[0016] A heterogeneous semiconductor nanoparticle prepared by the above preparation method.

[0017] A method for preparing a triboelectric film using the above-mentioned heterogeneous semiconductor nanoparticles, specifically comprising:

[0018] Step a: Weigh liquid polydimethylsiloxane (PDMS) using a balance, add heterogeneous semiconductor nanoparticles to the liquid polydimethylsiloxane at a mass fraction of 0.05% to 5%, and obtain component A after ultrasonic dispersion, planetary stirring, and degassing. Then, component A is mixed with a curing agent, and component B is obtained after secondary stirring and secondary degassing.

[0019] Step b: Use a balance to weigh the liquid polydimethylsiloxane again, then add the curing agent, and obtain component C after ultrasonic dispersion, planetary stirring, and degassing treatment;

[0020] Step c: first use a spin coater to spin-coat component C on the electrode surface, then dry it in an air environment. When component C on the electrode surface is not completely solidified, use a spin coater to spin-coat component B on the surface of component C, and finally dry it in a vacuum environment to make both components B and C completely solidified, thereby obtaining a triboelectric film attached to the electrode surface.

[0021] In step a: the ultrasonic dispersion time is 5 minutes to 10 minutes, the planetary stirring time is 3 minutes to 5 minutes, the degassing time is 30 seconds to 120 seconds, the curing agent is a liquid curing agent, the volume ratio of component A to the curing agent is 8 to 12:1, the secondary stirring time is 5 minutes to 10 minutes, and the secondary degassing time is 30 seconds to 120 seconds.

[0022] In step b: the curing agent is a liquid curing agent, the volume ratio of liquid polydimethylsiloxane to the curing agent is 8 to 12:1, the planetary stirring time is 5 minutes to 10 minutes, and the degassing time is 30 seconds to 120 seconds.

[0023] In step c: component C is spin-coated on the electrode surface by a coating method, and the coating method adopts a slow coating and high-speed shaping method, specifically: first adjust the spin coater to a rotation speed of 80 r / min to 300 r / min, and spin coat for 100 seconds to 300 seconds, and then adjust the spin coater to a rotation speed of 1000 r / min to 2000 r / min, and spin coat for 10 seconds to 30 seconds; when component B is spin-coated on the surface of component C, the rotation speed of the spin coater is 800 r / min to 2000 r / min; the drying temperature in an air environment is 60°C to 80°C; the drying temperature in a vacuum environment is 70°C to 80°C.

[0024] The triboelectric film prepared by the above method contains two layers: a pure PDMS layer (formed by component C) and a doped PDMS layer (formed by component B). The pure PDMS layer can effectively block the leakage of charge. The doped PDMS layer is located on the upper surface, which can allow the heterogeneous semiconductor nanoparticles to be fully illuminated. The film-forming materials of the pure PDMS layer and the doped PDMS layer are both polydimethylsiloxane (PDMS), and the interface cross-linking degree of the same base material is good.

[0025] Traditional wide bandgap semiconductor TiO2 can only be excited by ultraviolet light to produce hot electron-hole pairs, resulting in low photocatalytic efficiency under sunlight. The present invention uses narrow bandgap semiconductor Cu2O to sensitize wide bandgap semiconductor TiO2, thereby obtaining photogenerated hot electron-hole pairs excited by visible light, which can effectively broaden the wavelength range of photogenerated carriers, improve the utilization rate of sunlight, and ultimately expand the control wavelength of the surface charge density of the triboelectric film. At the same time, the effective transfer of photogenerated hot electrons and holes at the pn junction interface of the heterogeneous semiconductor can inhibit carrier recombination, thereby increasing the carrier (hot electron-hole pair) concentration. Driven by the friction electric field, the hot electron-hole pairs are arranged in a directional manner, thereby forming negative charge traps in the friction layer, thereby achieving the purpose of enhancing the electrification performance of the friction material.

[0026] The friction nanogenerator made of the above-mentioned friction electrification film contains an upper supporting layer, a lower supporting layer, an upper electrode, a lower electrode and a friction electrification film. The upper electrode is attached to the lower surface of the upper supporting layer, the lower electrode is attached to the upper surface of the lower supporting layer, the friction electrification film is attached to the upper surface of the lower electrode, and an air gap is left between the upper electrode and the friction electrification film, thereby forming a parallel capacitor plate structure.

[0027] The upper supporting layer and the lower supporting layer are made of transparent acrylic material; the upper electrode is a silver nanowire transparent electrode or an ITO transparent electrode, and the lower electrode is made of copper foil.

[0028] Beneficial effects of the present invention:

[0029] 1. The Cu2O nanoparticles in the heterogeneous semiconductor nanoparticles of the present invention are uniformly loaded on the surface of the TiO2 particles. This structure can not only effectively increase the contact interface between the Cu2O nanoparticles and the TiO2 particles, but also ensure that the Cu2O nanoparticles and the TiO2 particles are fully exposed to light at the same time.

[0030] 2. The present invention improves the dielectric properties of the triboelectric film by modifying the triboelectric film by doping heterogeneous semiconductor nanoparticles, and uses narrow-bandgap semiconductor Cu2O to sensitize wide-bandgap semiconductor TiO2, thereby obtaining photogenerated hot electron-hole pairs excited by visible light, which can effectively broaden the wavelength range of photogenerated carriers, improve the utilization rate of sunlight, and ultimately expand the control wavelength of the surface charge density of the triboelectric film; at the same time, the effective transfer of photogenerated hot electrons and holes at the pn junction interface of the heterogeneous semiconductor can inhibit carrier recombination, thereby increasing the carrier (hot electron-hole pair) concentration; a reverse electric field is constructed in the triboelectric film by hot electron-hole pairs, thereby improving the output performance of the triboelectric nanogenerator; when the triboelectric film of the present invention is applied to the triboelectric nanogenerator, the output performance of the triboelectric nanogenerator can be controlled in real time by illumination, and the spectral bandwidth can be controlled. It is simple and reliable to use, and the triboelectric nanogenerator can be widely used in outdoor mechanical vibration energy collection, self-powered wireless sensor systems, intelligent buildings, intelligent transportation and other fields. (IV) Description of the drawings:

[0031] Figure 1 Schematic diagram of the structure of TiO2@Cu2O heterogeneous semiconductor nanoparticles;

[0032] Figure 2 Schematic diagram of the principle of sensitizing narrow bandgap semiconductor Cu2O to wide bandgap semiconductor TiO2;

[0033] Figure 3 Schematic diagram of the structure of the friction nanogenerator;

[0034] Figure 4 Schematic diagram of the working principle of the friction nanogenerator;

[0035] Figure 5 Schematic diagram of the mechanism of hot electron-hole pairs regulating the output of triboelectric nanogenerator;

[0036] Figure 6 This is the experimental effect diagram of wide-spectrum regulation of friction effect. (V) Specific implementation methods:

[0037] Implementation method 1:

[0038] The preparation method of TiO2@Cu2O heterogeneous semiconductor nanoparticles is as follows:

[0039] Step 1. Weigh copper acetate powder, and then dissolve the copper acetate powder in anhydrous ethanol to obtain a mixed solution A; wherein 1g of copper acetate powder is added to 90mL of anhydrous ethanol;

[0040] Step 2: First, the mixed solution A is dispersed by an ultrasonic disperser for 15 minutes, and then stirred for 10 minutes and degassed for 60 seconds;

[0041] Step 3, weigh TiO2 powder, add the TiO2 powder to the mixed solution A treated in step 2, to obtain a mixed solution B; wherein the particle size of the TiO2 powder is 100 nm, and 1 g of TiO2 powder is added to 4.5 mL of the mixed solution A treated in step 2;

[0042] Step 4: First, the mixed solution B is dispersed by an ultrasonic disperser for 15 minutes, and then stirred for 10 minutes and degassed for 60 seconds to obtain a suspension A, and the suspension A is heated to 70° C. in a water bath;

[0043] Step 5: Add glucose solution to suspension A, and then add NaOH solution to obtain suspension B; wherein the concentration of glucose solution is 0.3 mol / L, which is used to adjust the particle size of Cu2O, the concentration of NaOH solution is 0.3 mol / L, and the volume ratio of suspension A, NaOH solution, and glucose solution is 1:2:1.5;

[0044] Step 6: Dry the suspension B with a centrifugal dryer to obtain a precipitate, then wash the precipitate with anhydrous ethanol for 6 times, and finally dry the washed precipitate in a vacuum drying oven at 70° C. for 26 hours to obtain TiO2@Cu2O heterogeneous semiconductor nanoparticles.

[0045] The structure of TiO2@Cu2O heterogeneous semiconductor nanoparticles is as follows Figure 1 As shown: Cu2O nanoparticles 8 are uniformly loaded on the surface of TiO2 particles 7. This structure can not only effectively increase the contact interface between Cu2O nanoparticles 8 and TiO2 particles 7, but also ensure that Cu2O nanoparticles 8 and TiO2 particles 7 can fully receive light at the same time.

[0046] The method for preparing triboelectric film using TiO2@Cu2O heterogeneous semiconductor nanoparticles is as follows:

[0047] Step a: Weigh liquid polydimethylsiloxane (PDMS) using a balance, add TiO2@Cu2O heterogeneous semiconductor nanoparticles to the liquid polydimethylsiloxane at a mass fraction of 0.1%, and obtain component A after ultrasonic dispersion, planetary stirring, and degassing. Then, component A is mixed with a curing agent, and component B is obtained after secondary stirring and secondary degassing.

[0048] Step b: Use a balance to weigh the liquid polydimethylsiloxane again, then add the curing agent, and obtain component C after ultrasonic dispersion, planetary stirring, and degassing treatment;

[0049] Step c: first use a spin coater to spin-coat component C on the electrode surface, then dry it in an air environment. When component C on the electrode surface is not completely solidified, use a spin coater to spin-coat component B on the surface of component C, and finally dry it in a vacuum environment to make both components B and C completely solidified, thereby obtaining a triboelectric film attached to the electrode surface.

[0050] In step a: the ultrasonic dispersion time is 7 minutes, the planetary stirring time is 4 minutes, the degassing time is 60 seconds, the curing agent is a liquid curing agent, the volume ratio of component A to the curing agent is 10:1, the secondary stirring time is 7 minutes, and the secondary degassing time is 60 seconds.

[0051] In step b: the curing agent is a liquid curing agent, the volume ratio of liquid polydimethylsiloxane to the curing agent is 10:1, the planetary stirring time is 7 minutes, and the degassing time is 60 seconds.

[0052] In step c: component C is spin-coated on the electrode surface by a coating method, and the coating method adopts a slow coating and high-speed shaping method, specifically: first adjust the spin coater to a speed of 100 r / min, spin coat for 120 seconds, and then adjust the spin coater to a speed of 1500 r / min, and spin coat for 20 seconds; when component B is spin-coated on the surface of component C, the speed of the spin coater is 1000 r / min; the drying temperature in an air environment is 70°C, and the reference drying time can be 5 to 10 minutes; the drying temperature in a vacuum environment is 75°C, and the reference drying time can be 1.5 hours to 2 hours.

[0053] The triboelectric film prepared by the above method contains two layers: a pure PDMS layer (formed by component C) and a doped PDMS layer (formed by component B). The pure PDMS layer can effectively block the leakage of charge. The doped PDMS layer is located on the upper surface, which can allow the heterogeneous semiconductor nanoparticles to be fully illuminated. The film-forming materials of the pure PDMS layer and the doped PDMS layer are both polydimethylsiloxane (PDMS), and the interface cross-linking degree of the same base material is good.

[0054] Traditional wide bandgap semiconductor TiO2 can only be excited by ultraviolet light to produce hot electron-hole pairs, resulting in low photocatalytic efficiency under sunlight. The present invention uses narrow bandgap semiconductor Cu2O to sensitize wide bandgap semiconductor TiO2, thereby obtaining photogenerated hot electron-hole pairs excited by visible light, which can effectively broaden the wavelength range of photogenerated carriers, improve the utilization rate of sunlight, and ultimately expand the control wavelength of the surface charge density of the triboelectric film. At the same time, the effective transfer of photogenerated hot electrons and holes at the pn junction interface of the heterogeneous semiconductor can inhibit carrier recombination, thereby increasing the carrier (hot electron-hole pair) concentration. Driven by the friction electric field, the hot electron-hole pairs are arranged in a directional manner, thereby forming negative charge traps in the friction layer, thereby achieving the purpose of enhancing the electrification performance of the friction material.

[0055] Figure 2 This is a schematic diagram of the principle of sensitizing the narrow-bandgap semiconductor Cu2O to the wide-bandgap semiconductor TiO2. The majority carriers in the p-type semiconductor Cu2O are holes, and the majority carriers in the n-type semiconductor TiO2 are electrons. When the two semiconductors come into contact with each other, a carrier concentration difference will be formed at the contact interface, causing holes to diffuse to the n-type semiconductor TiO2 region and electrons to diffuse to the p-type semiconductor Cu2O region, leaving fixed positive and negative charges at the interface. This space charge region pointing from the n-type semiconductor TiO2 region to the p-type semiconductor Cu2O region is called the built-in electric field. Before the formation of the pn junction, the Fermi level of the n-type semiconductor TiO2 is higher than that of the p-type semiconductor Cu2O. After the two semiconductors come into contact, the energy band of the n-type semiconductor TiO2 moves downward as a whole, while the energy band of the p-type semiconductor Cu2O moves upward, until the Fermi levels of the two semiconductors are leveled. At this time, a pn heterojunction between the two semiconductors is formed. When light shines on a semiconductor, it is excited to generate electrons and holes. Due to the concentration difference, the photogenerated electrons and holes that jump to the space electric field move in a directional manner driven by the built-in electric field, which promotes the separation of photogenerated electron pairs. Hot electrons are injected into the conduction band of TiO2, thereby sensitizing TiO2. On the one hand, it accelerates the separation speed of hot electron-hole pairs and inhibits their recombination, thereby increasing the concentration of carriers. On the other hand, it improves the visible light absorption of TiO2, broadens its spectral range, and improves the utilization rate of solar energy.

[0056] like Figure 3 As shown: the friction nanogenerator made of the above-mentioned friction electrification film contains an upper support layer 1, a lower support layer 2, an upper electrode 3, a lower electrode 4 and a friction electrification film 5. The friction nanogenerator is a vertically separated friction nanogenerator. The upper electrode 3 is pasted on the lower surface of the upper support layer 1, the lower electrode 4 is pasted on the upper surface of the lower support layer 2, the friction electrification film 5 is attached to the upper surface of the lower electrode 4, and an air gap is left between the upper electrode 3 and the friction electrification film 5, thereby forming a parallel capacitor plate structure.

[0057] The upper support layer 1 and the lower support layer 2 are made of transparent acrylic material; the upper electrode 3 is a silver nanowire transparent electrode, and the lower electrode 4 is made of copper foil.

[0058] Figure 4 The schematic diagram of the working principle of the triboelectric nanogenerator is shown in Figure 1. When the vertical external force F acts on the upper support layer 1, the upper electrode 3 and the triboelectric film 5 will contact each other, so that negative charges accumulate on the triboelectric film 5 and positive charges accumulate on the upper electrode 3. After the vertical force F is removed, the upper electrode 3 and the triboelectric film 5 are separated, and a potential difference is formed between the upper electrode 3 and the lower electrode 4. Electrons flow from the lower electrode 4 to the upper electrode 3, forming a current I1 on the external load R of the triboelectric nanogenerator. When the vertical external force F acts again, the upper electrode 3 and the triboelectric film 5 are contacted again, and electrons flow back, forming a current I2 on the external load R of the triboelectric nanogenerator. When the triboelectric nanogenerator is actually used, the external force F is continuously applied and released, and the upper electrode 3 and the triboelectric film 5 are continuously contacted and separated, thereby forming a continuous current on the external load R of the triboelectric nanogenerator and continuously generating electrical energy.

[0059] Figure 5 The schematic diagram of the mechanism of hot electron-hole pairs regulating the output of triboelectric nanogenerators. Under light irradiation, heterogeneous semiconductor nanoparticles produce photogenerated carrier effects, which will accumulate hot electron-hole pairs inside the triboelectric film. Driven by the electric field from the upper surface of the triboelectric film to the lower electrode (the electric field E1 formed by the friction effect), the hot electron-hole pairs tend to be vertically arranged in the triboelectric film. On the one hand, the vertically arranged hot electron-hole pairs are similar to the polarization of dipoles. In the process of contact electrification, they can act as negative charge traps, enhance the charge capture ability of the triboelectric film, enhance the electrification performance of the triboelectric film, and thus improve the output performance of the triboelectric nanogenerator. On the other hand, the vertically arranged hot electron-hole pairs construct an electric field (E2) in the opposite direction of the electric field E1 inside the triboelectric film. The weakening of the total field strength in the triboelectric film will increase the inherent capacitance C of the triboelectric nanogenerator, thereby achieving the purpose of optimizing the output performance of the triboelectric nanogenerator.

[0060] The short-circuit current (μA) of the above-mentioned friction nanogenerator was tested under different lighting environments (no light, UV light, visible + UV light). The results are as follows: Figure 6 As shown, from Figure 6 It can be seen that under ultraviolet light, the short-circuit current of the friction nanogenerator is greater than that under no light, and the short-circuit current of the friction nanogenerator under + ultraviolet light is greater than that under ultraviolet light, indicating that the heterogeneous semiconductor nanoparticles have realized the wide-spectrum regulation effect of the friction nanogenerator.

[0061] Implementation method 2:

[0062] The preparation method of TiO2@Cu2O heterogeneous semiconductor nanoparticles is as follows:

[0063] Step 1. Weigh copper acetate powder, and then dissolve the copper acetate powder in anhydrous ethanol to obtain a mixed solution A; wherein 1g of copper acetate powder is added to 80mL of anhydrous ethanol;

[0064] Step 2: First, the mixed solution A is dispersed by an ultrasonic disperser for 10 minutes, and then stirred for 5 minutes and degassed for 30 seconds;

[0065] Step 3, weigh TiO2 powder, add the TiO2 powder to the mixed solution A treated in step 2, to obtain a mixed solution B; wherein the particle size of the TiO2 powder is 50nm, and 1g of TiO2 powder is added to 4mL of the mixed solution A treated in step 2;

[0066] Step 4: First, the mixed solution B is dispersed by an ultrasonic disperser for 10 minutes, and then stirred for 5 minutes and degassed for 30 seconds to obtain a suspension A, and the suspension A is heated to 60° C. in a water bath;

[0067] Step 5: Add glucose solution to suspension A, and then add NaOH solution to obtain suspension B; wherein the concentration of glucose solution is 0.1 mol / L, which is used to adjust the particle size of Cu2O, the concentration of NaOH solution is 0.1 mol / L, and the volume ratio of suspension A, NaOH solution, and glucose solution is 1:1.5:1;

[0068] Step 6: Dry the suspension B with a centrifugal dryer to obtain a precipitate, then wash the precipitate with anhydrous ethanol for 5 times, and finally dry the washed precipitate in a vacuum drying oven at 60° C. for 24 hours to obtain TiO2@Cu2O heterogeneous semiconductor nanoparticles.

[0069] The method for preparing triboelectric film using TiO2@Cu2O heterogeneous semiconductor nanoparticles is as follows:

[0070] Step a: Weigh liquid polydimethylsiloxane (PDMS) using a balance, add TiO2@Cu2O heterogeneous semiconductor nanoparticles to the liquid polydimethylsiloxane at a mass fraction of 0.05%, and obtain component A after ultrasonic dispersion, planetary stirring, and degassing. Then, component A is mixed with a curing agent, and component B is obtained after secondary stirring and secondary degassing.

[0071] Step b: Use a balance to weigh the liquid polydimethylsiloxane again, then add the curing agent, and obtain component C after ultrasonic dispersion, planetary stirring, and degassing treatment;

[0072] Step c: first use a spin coater to spin-coat component C on the electrode surface, then dry it in an air environment. When component C on the electrode surface is not completely solidified, use a spin coater to spin-coat component B on the surface of component C, and finally dry it in a vacuum environment to make both components B and C completely solidified, thereby obtaining a triboelectric film attached to the electrode surface.

[0073] In step a: the ultrasonic dispersion time is 5 minutes, the planetary stirring time is 3 minutes, the degassing time is 30 seconds, the curing agent is a liquid curing agent, the volume ratio of component A to the curing agent is 8:1, the secondary stirring time is 5 minutes, and the secondary degassing time is 30 seconds.

[0074] In step b: the curing agent is a liquid curing agent, the volume ratio of liquid polydimethylsiloxane to the curing agent is 8:1, the planetary stirring time is 5 minutes, and the degassing time is 30 seconds.

[0075] In step c: component C is spin-coated on the electrode surface by a coating method, and the coating method adopts a slow coating and high-speed shaping method, specifically: first adjust the spin coater to a speed of 80 r / min, spin coat for 100 seconds, and then adjust the spin coater to a speed of 1000 r / min, and spin coat for 10 seconds; when component B is spin-coated on the surface of component C, the speed of the spin coater is 800 r / min; the drying temperature in an air environment is 60°C, and the reference drying time can be 5 to 10 minutes; the drying temperature in a vacuum environment is 70°C, and the reference drying time can be 1.5 hours to 2 hours.

[0076] Implementation method three:

[0077] The preparation method of TiO2@Cu2O heterogeneous semiconductor nanoparticles is as follows:

[0078] Step 1. Weigh copper acetate powder, and then dissolve the copper acetate powder in anhydrous ethanol to obtain a mixed solution A; wherein 1g of copper acetate powder is added to 100mL of anhydrous ethanol;

[0079] Step 2: First, the mixed solution A is dispersed by an ultrasonic disperser for 30 minutes, and then stirred for 15 minutes and degassed for 120 seconds;

[0080] Step 3, weigh TiO2 powder, add the TiO2 powder to the mixed solution A treated in step 2, to obtain a mixed solution B; wherein the particle size of the TiO2 powder is 200nm, and 1g of TiO2 powder is added to 5mL of the mixed solution A treated in step 2;

[0081] Step 4: First, the mixed solution B is dispersed by an ultrasonic disperser for 30 minutes, and then stirred for 15 minutes and degassed for 120 seconds to obtain a suspension A, and the suspension A is heated to 80° C. in a water bath;

[0082] Step 5: Add glucose solution to suspension A, and then add NaOH solution to obtain suspension B; wherein the concentration of glucose solution is 1 mol / L, which is used to adjust the particle size of Cu2O, the concentration of NaOH solution is 1 mol / L, and the volume ratio of suspension A, NaOH solution, and glucose solution is 1:3:2;

[0083] Step 6: Dry the suspension B with a centrifugal dryer to obtain a precipitate, then wash the precipitate with anhydrous ethanol for 8 times, and finally dry the washed precipitate in a vacuum drying oven at 120° C. for 30 hours to obtain TiO2@Cu2O heterogeneous semiconductor nanoparticles.

[0084] The method for preparing triboelectric film using TiO2@Cu2O heterogeneous semiconductor nanoparticles is as follows:

[0085] Step a: Weigh liquid polydimethylsiloxane (PDMS) using a balance, add TiO2@Cu2O heterogeneous semiconductor nanoparticles to the liquid polydimethylsiloxane at a ratio of 5% by mass, and obtain component A after ultrasonic dispersion, planetary stirring, and degassing treatment. Then, component A is mixed with a curing agent, and component B is obtained after secondary stirring and secondary degassing treatment.

[0086] Step b: Use a balance to weigh the liquid polydimethylsiloxane again, then add the curing agent, and obtain component C after ultrasonic dispersion, planetary stirring, and degassing treatment;

[0087] Step c: first use a spin coater to spin-coat component C on the electrode surface, then dry it in an air environment. When component C on the electrode surface is not completely solidified, use a spin coater to spin-coat component B on the surface of component C, and finally dry it in a vacuum environment to make both components B and C completely solidified, thereby obtaining a triboelectric film attached to the electrode surface.

[0088] In step a: the ultrasonic dispersion time is 10 minutes, the planetary stirring time is 5 minutes, the degassing time is 120 seconds, the curing agent is a liquid curing agent, the volume ratio of component A to the curing agent is 12:1, the secondary stirring time is 10 minutes, and the secondary degassing time is 120 seconds.

[0089] In step b: the curing agent is a liquid curing agent, the volume ratio of liquid polydimethylsiloxane to the curing agent is 12:1, the planetary stirring time is 10 minutes, and the degassing time is 120 seconds.

[0090] In step c: component C is spin-coated on the electrode surface by a coating method, and the coating method adopts a slow coating and high-speed shaping method, specifically: first adjust the spin coater to a speed of 300 r / min, spin coat for 300 seconds, and then adjust the spin coater to a speed of 2000 r / min, and spin coat for 30 seconds; when component B is spin-coated on the surface of component C, the speed of the spin coater is 2000 r / min; the drying temperature in an air environment is 80°C, and the reference drying time can be 5 to 10 minutes; the drying temperature in a vacuum environment is 80°C, and the reference drying time can be 1.5 hours to 2 hours.

Claims

1. A method for preparing heterogeneous semiconductor nanoparticles, characterized in that: Step 1. Weigh copper acetate powder, and then dissolve the copper acetate powder in anhydrous ethanol to obtain a mixed solution A; wherein 1g of copper acetate powder is added to 80mL to 100mL of anhydrous ethanol; Step 2: Firstly, the mixed solution A is dispersed by an ultrasonic disperser, and then stirred and degassed in sequence; Step 3, weigh TiO2 powder, add the TiO2 powder to the mixed solution A treated in step 2, to obtain a mixed solution B; wherein the particle size of the TiO2 powder is 50nm to 200nm, and 1g of TiO2 powder is added to 4mL to 5mL of the mixed solution A treated in step 2; Step 4: First, the mixed solution B is dispersed by an ultrasonic disperser, and then stirred and degassed in sequence to obtain a suspension A, and the suspension A is heated to 60° C. to 80° C. in a water bath; Step 5: Add glucose solution to suspension A, and then add NaOH solution to obtain suspension B; wherein the concentration of glucose solution is 0.1 mol / L to 1 mol / L, the concentration of NaOH solution is 0.1 mol / L to 1 mol / L, and the volume ratio of suspension A, NaOH solution and glucose solution is 1:1.5 to 3:1 to 2; Step 6: Dry the suspension B with a centrifugal dryer to obtain a precipitate, then wash the precipitate with anhydrous ethanol, and finally dry the washed precipitate in a vacuum drying oven at 60°C to 120°C to obtain heterogeneous semiconductor nanoparticles.

2. The method for preparing heterogeneous semiconductor nanoparticles according to claim 1, characterized in that: The heterogeneous semiconductor nanoparticles are TiO2@Cu2O heterogeneous semiconductor nanoparticles.

3. The method for preparing heterogeneous semiconductor nanoparticles according to claim 1, characterized in that: In step 2, the dispersion treatment time is 10 minutes to 30 minutes, the stirring treatment time is 5 minutes to 15 minutes, and the degassing treatment time is 30 seconds to 120 seconds; In step 4, the dispersion treatment time is 10 minutes to 30 minutes, the stirring treatment time is 5 minutes to 15 minutes, and the degassing treatment time is 30 seconds to 120 seconds.

4. The method for preparing heterogeneous semiconductor nanoparticles according to claim 1, characterized in that: In step 6, the precipitate is washed with anhydrous ethanol for 5 to 8 times, and the drying time is 24 to 30 hours.

5. A heterogeneous semiconductor nanoparticle obtained by the preparation method according to any one of claims 1 to 4.

6. A method for preparing a triboelectric film using the heterogeneous semiconductor nanoparticles according to claim 5, characterized in that: Step a: Weigh liquid polydimethylsiloxane, add heterogeneous semiconductor nanoparticles to the liquid polydimethylsiloxane at a mass fraction of 0.05% to 5%, and obtain component A after ultrasonic dispersion, planetary stirring, and degassing. Then, component A is mixed with a curing agent, and component B is obtained after secondary stirring and secondary degassing. Step b: Weigh the liquid polydimethylsiloxane again, then add the curing agent, and obtain component C after ultrasonic dispersion, planetary stirring and degassing treatment; Step c: first use a spin coater to spin-coat component C on the electrode surface, then dry it in an air environment. When component C on the electrode surface is not completely solidified, use a spin coater to spin-coat component B on the surface of component C, and finally dry it in a vacuum environment to make both components B and C completely solidified, thereby obtaining a triboelectric film attached to the electrode surface.

7. The method for preparing a triboelectric film according to claim 6, characterized in that: In the step a, the ultrasonic dispersion time is 5 to 10 minutes, the planetary stirring time is 3 to 5 minutes, the degassing time is 30 to 120 seconds, the curing agent is a liquid curing agent, the volume ratio of component A to the curing agent is 8 to 12:1, the secondary stirring time is 5 to 10 minutes, and the secondary degassing time is 30 to 120 seconds.

8. The method for preparing a triboelectric film according to claim 6, wherein: In the step b, the curing agent is a liquid curing agent, the volume ratio of liquid polydimethylsiloxane to the curing agent is 8 to 12:1, the planetary stirring time is 5 to 10 minutes, and the degassing time is 30 to 120 seconds.

9. The method for preparing a triboelectric film according to claim 6, characterized in that: In the step c: the C component is spin-coated on the electrode surface by a coating method, and the coating method is specifically as follows: firstly, the spin coater is adjusted to a rotation speed of 80 r / min to 300 r / min, and the coating is performed for 100 seconds to 300 seconds, and then the spin coater is adjusted to a rotation speed of 1000 r / min to 2000 r / min, and the coating is performed for 10 seconds to 30 seconds; when the B component is spin-coated on the surface of the C component, the rotation speed of the spin coater is 800 r / min to 2000 r / min; the drying temperature in an air environment is 60°C to 80°C; and the drying temperature in a vacuum environment is 70°C to 80°C.