Chlorinated graphene material, preparation method and invisible space solar cell

By chlorine doping and subwavelength microstructure processing of graphene, graphene chloride material was prepared, which solved the transparency and surface density of space solar cell arrays, achieved efficient microwave absorption and transparency, and significantly reduced radar reflection The cross-section improves the stealth performance of the solar cell array.

CN114256631BActive Publication Date: 2024-11-12SHANGHAI INST OF SPACE POWER SOURCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111585534.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-22
Publication Date
2024-11-12
Estimated Expiration
2041-12-22

AI Technical Summary

Technical Problem

The existing transparent absorption shielding dielectric materials have low transparency and large surface density on space solar cell arrays, which cannot meet the needs of large-scale use, resulting in reduced battery efficiency and difficult packaging, and cannot effectively adjust specific microwave bands, affecting the stealth of space aircraft. performance.

Method used

Through photochlorine reaction, graphene is chlorodoped, its Fermi energy level is changed, graphene chloride material is prepared, and subwavelength microstructure is processed on the material to form transparent doped graphene for use invisible materials of solar cells. , combined with the silica dielectric layer and the polyvinyl butyral connecting layer, microwave absorption frequency modulation is achieved.

Benefits of technology

It improves the transparency, surface density, wave absorption performance and wave absorption modulation, solves the problem of spectral mismatch of solar cell arrays, reduces the radar reflection cross-section, and improves the efficiency and stealth performance of solar cell arrays.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114256631B_ABST
    Figure CN114256631B_ABST
Patent Text Reader

Abstract

The invention discloses a chlorinated graphene material, a preparation method and a stealth space solar cell. The preparation method comprises: placing a metal film on a target platform of a MOCVD system cavity, evacuating the vacuum to less than 10 ‑4 Torr;Hydrogen and argon are introduced, with a gas flow rate of 50sccm-100sccm and a target stage temperature of 800℃-1100℃;Hydrogen and argon are stopped, methane is introduced, with a gas flow rate of 25sccm-50sccm and a reaction time of 0.5h-3h;Methane is stopped, and chlorine is introduced under visible light irradiation, with a gas flow rate of 30sccm-70sccm, a target stage temperature of 550℃-750℃, and a reaction time of 0.5h-2h;Chlorine is stopped, and the temperature is cooled to room temperature at a rate of 5℃ / s-20℃ / s to obtain the chlorinated graphene material. The material prepared by the method has high wide spectrum transparency, low surface density, good wave absorption performance and strong environmental adaptability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of electromagnetic wave absorbing materials, and specifically relates to graphene chloride materials, preparation methods and stealth space solar cells. Background Art

[0002] With the widespread use of space vehicles including satellites and their huge role in national defense, economy, science and technology, the safety and survivability of space vehicles are facing increasingly severe challenges. Among them, the radar detectability of space vehicles has become one of the important threats to their safety and survival during their on-orbit mission. For example, for a typical satellite, the area occupied by its solar array after deployment accounts for more than 80% of the overall area, becoming the main radar cross section, and the planar structure of the solar array after deployment is also an excellent target for radar detection. Therefore, solar array stealth technology has become an important part of space vehicle stealth technology, and it is also one of the important prerequisites for ensuring the safety of aircraft when facing external threats.

[0003] The existing traditional microwave absorption technology materials are usually opaque materials. Although this material has a high absorption efficiency, it can provide microwave stealth performance for general equipment by effectively reducing the radar scattering cross section. However, due to the opacity of traditional materials, it is impossible to provide wave absorption capabilities for solar cells while maintaining the power supply capacity of the battery array, so it cannot be applied to space solar arrays. The existing light-transmissive microwave shielding material technology usually uses conductive oxide materials or surface structured films based on conductive oxide materials. The more mature application of such films is transparent-microwave reflective shielding films, that is, shielding microwaves by reflection, but reflective shielding materials cannot be applied to radar stealth technology. Transparent-absorbing conductive oxides or similar functional material films modulated by impedance matching or multilayer film structures can usually meet technical requirements such as transparent absorption to a certain extent, but are usually used in fields such as ground communication devices or aircraft cockpit glass.

[0004] The technical methods and devices provided by the prior art meet the effects of transparency in the visible light band and absorption and shielding in the microwave band to a certain extent, and have application value. However, for space solar arrays, the above materials still have the problems of relatively low transparency and high surface density. On the one hand, these problems will cause the battery array to mismatch with the space solar spectrum, and the battery efficiency can drop by more than 35%; on the other hand, it is difficult to package it on the solar array, it is heavy, the space reliability is low, and it seriously affects the payload of the spacecraft. In addition, it has problems such as difficulty in adjustment for specific microwave bands and low flexibility.

[0005] Therefore, there is an urgent need to find stealth materials and technologies suitable for space solar arrays that have high wide-spectrum transparency, low surface density, good wave absorption performance, and strong environmental adaptability. Summary of the invention

[0006] The purpose of the present invention is to solve the problems in the existing transparent absorption shielding medium technology that the material transparency is low, the surface density and weight are large, and it cannot meet the use conditions of large-area space solar cells.

[0007] In order to achieve the above object, the present invention provides a method for preparing a chlorinated graphene material, comprising:

[0008] Place the metal film on the target stage of the MOCVD system chamber and evacuate to less than 10 -4 Torr;

[0009] Hydrogen and argon are introduced, the gas flow rate is 50sccm-100sccm, and the target stage temperature is 800℃-1100℃;

[0010] Stop the introduction of hydrogen and argon, and introduce methane with a gas flow rate of 25 sccm-50 sccm and a reaction time of 0.5 h-3 h;

[0011] Stop the introduction of methane, and introduce chlorine gas under visible light irradiation, with a gas flow rate of 30sccm-70sccm, a target stage temperature of 550℃-750℃, and a reaction time of 0.5h-2h;

[0012] Stop introducing chlorine gas, cool to room temperature at a rate of 5°C / s-20°C / s, and obtain the chlorinated graphene material.

[0013] Optionally, before placing the metal film on the target platform, a step of processing a microstructure on the metal film is included.

[0014] Optionally, a post-processing step is included: degumming, pickling and peeling the graphene chloride material.

[0015] The present invention also provides a chlorinated graphene material prepared by the above method.

[0016] A stealth solar cell comprises a first graphene layer, a dielectric layer, a second graphene layer, a connecting layer and a cell structure which are stacked in sequence;

[0017] The first graphene layer and the second graphene layer comprise the chlorinated graphene material of claim 4;

[0018] The dielectric layer comprises silicon dioxide;

[0019] The tie layer comprises polyvinyl butyral.

[0020] Optionally, the first graphene layer comprises a first cross structure, wherein the arm length of the first cross structure is 4mm-8mm, and the arm width is 2mm-5mm.

[0021] Optionally, the second graphene layer comprises a second cross structure, and the arm length of the second cross structure is 1mm-3mm, and the arm width is 1mm-2mm.

[0022] Optionally, the battery structure includes a positive electrode, a space battery and a negative electrode stacked in sequence, and the positive electrode is arranged on one side of the connecting layer.

[0023] Optionally, the space battery is a gallium arsenide battery;

[0024] The positive electrode is a silver positive electrode with a thickness of 4 μm-6 μm;

[0025] The negative electrode is a silver negative electrode with a thickness of 7 μm-9 μm.

[0026] Optionally, the dielectric layer has a thickness of 110 μm-130 μm;

[0027] The thickness of the connecting layer is 140 μm-160 μm.

[0028] The beneficial effects of the present invention are:

[0029] (1) The present invention performs chlorine doping on graphene through a photochlorination reaction, thereby changing the Fermi level of transparent graphene, achieving regulation of the microwave shielding absorption peak position, and realizing the modulation function of the microwave absorption frequency without changing the overall structure of the stealth cover.

[0030] (2) The present invention uses transparent doped graphene as a patterned subwavelength transparent absorbing material. The material has high spectral transparency and low surface density, which solves the problem of spectral mismatch leading to a significant drop in efficiency after packaging the stealth material of space solar cells.

[0031] (3) Compared with the prior art, the present invention has advantages in terms of material transparency, surface density, wave absorption performance, wave absorption modulatability, manufacturing difficulty and cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is a schematic structural diagram of the stealth space solar cell provided by the present invention.

[0033] Figure 2 Schematic diagram of the minimum repeating unit of the sub-wavelength microstructure of the stealth space solar cell provided by the present invention.

[0034] Figure 3 The present invention provides an average transmittance curve of the invisible space solar cell in the 380-780nm band.

[0035] Figure 4 The present invention provides an average transmittance curve of the invisible space solar cell in the 780-2000nm band.

[0036] Figure 5a This is a cross-sectional view of the radar cross section (RCS) (phi=0) of the stealth space solar cell provided by the present invention.

[0037] Figure 5b The cross-sectional view of the radar cross section (RCS) (phi=0) of a space solar cell covered with the chlorinated graphene material provided by the present invention.

[0038] Figure 6 The wave absorbing and shielding efficiency curve of the stealth space solar cell provided by the present invention.

[0039] Figure 7 A comparison diagram of microwave absorption peak changes of stealth space solar cells covered with materials with different Cl doping concentrations provided by the present invention.

[0040] In the figure, 1-first graphene layer, 10-first cross structure, 2-medium layer, 20-second cross structure, 3-second graphene layer, 4-connecting layer, 5-battery structure, 51-positive electrode, 52-space battery, 53-negative electrode. DETAILED DESCRIPTION

[0041] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] In the description of the present invention, it should be noted that the terms "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and "third" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.

[0043] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected" and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0044] Under light conditions, Cl2 can generate high-energy free radicals that hit the graphene π-π bond and add to the graphene carbon atoms, converting the sp 2 The hybrid structure changes to sp 3 Hybrid structure. The bottom of the conduction band and the top of the valence band of the intrinsic graphene in the present invention intersect at the Fermi level, and the band structure is approximately linearly distributed, and its band gap is zero. 2 The change of hybrid orbitals leads to the change of Fermi level, and the bottom of the conduction band and the top of the valence band are no longer distributed approximately linearly. By adjusting the band gap of the material, the corresponding central wavelength of the microwave of the material can be adjusted.

[0045] Based on the above principle, the present invention utilizes the photochlorination reaction of graphene to chlorinate the graphene material to obtain chlorinated graphene material, which can be used as a stealth material for space solar cells. The method for preparing the chlorinated graphene material includes:

[0046] S1: preparing a patterned microstructure on the metal copper film by photolithography reaction. Preferably, the patterned microstructure is a millimeter-scale cross structure.

[0047] S2: Place the copper film on the target stage of the MOCVD system chamber and evacuate to less than 10 -4 Torr.

[0048] S3: hydrogen and argon are introduced at a gas flow rate of 50sccm-100sccm, and the target stage temperature is heated to 800°C-1100°C. Hydrogen and argon are used as protective gases to prevent the substrate material from being oxidized during the heating process.

[0049] S4: Stop the introduction of hydrogen and argon, introduce methane, the gas flow rate is 25sccm-50sccm, and the reaction time is 0.5h-3h. Methane is used as a carbon source, and methane is decomposed at high temperature to deposit graphene on the patterned metal copper film to prepare intrinsic graphene material.

[0050] S5: Stop the introduction of methane and cool down to room temperature at a rate of 5°C / s-20°C / s. In actual preparation, after the intrinsic graphene material is prepared, it is usually necessary to take it out first to observe the morphology and quality of the graphene before proceeding to the next step of the experiment.

[0051] S6: Evacuate the chamber to less than 10 -4 Torr, the target temperature is raised to 550℃-750℃.

[0052] S7: Under visible light irradiation, chlorine gas is introduced with a gas flow rate of 30 sccm-70 sccm and a reaction time of 0.5h-2h.

[0053] S8: Stop introducing chlorine gas, and cool to room temperature at a rate of 5°C / s-20°C / s to obtain a chloride graphene material.

[0054] S9: Post-processing, degumming, pickling and peeling of the graphene chloride material.

[0055] In the present invention, the above-mentioned preparation method is used to make the chloride graphene material obtain a specific doping concentration and change the Fermi level of the graphene material. By adjusting the Fermi level, the absorption shielding center wavelength can be modulated without changing the overall structure of the stealth cover to adapt to space radar detection with different characteristic wavelengths. In this embodiment, the Fermi level of the chloride graphene material after the reaction is measured to be 0.25eV. The material is used in the stealth cover of the solar cell, and the microwave absorption peak of the stealth cover can be adjusted in the range of 8.5GHz to 12.0GHz. In this embodiment, the volume density of the chloride graphene material ρ0=1.06g / cm 3 , the mass is M = 1.68 × 10 -2 g, so the total surface density of graphene chloride material is ρ A =168g / m 2 , and its density has certain advantages over existing materials. By changing the Fermi level of graphene materials through doping, the central wavelength of the material's wave absorption and shielding can be effectively changed to achieve different performances required in different application scenarios.

[0056] like Figure 1 As shown, the present invention also provides a stealth solar cell, comprising a first graphene layer 1, a dielectric layer 2, a second graphene layer 3, a connecting layer 4 and a battery structure 5 stacked in sequence. The first graphene layer 1, the dielectric layer 2, the second graphene layer 3 and the transparent connecting layer 4 are all transparent structural layers. The first graphene layer 1 and the second graphene layer 3 contain the chlorinated graphene material prepared by the present invention. The dielectric layer 2 contains silicon dioxide with a thickness of 120 μm. The connecting layer 4 contains polyvinyl butyral with a thickness of 150 μm. The battery structure 5 includes a positive electrode 51, a space battery 52 and a negative electrode 53 stacked in sequence, and the positive electrode 51 is connected to the connecting layer 4. Preferably, the space battery 52 is a gallium arsenide battery; the positive electrode 51 is a silver positive electrode with a thickness of 5 μm; and the negative electrode 53 is a silver negative electrode with a thickness of 5 μm.

[0057] Traditional thin film absorbing materials cannot break through the thickness limit of one quarter of the central wavelength. By processing the material obtained by patterning the structure on the surface of the metal film, an electromagnetic wave resonator can be formed in the plane. Adjusting the shape and size of the microstructure pattern can make the size effect of the microwave wavelength at the millimeter scale significant. Strong mutual coupling of multiple energy carriers (electrons, phonons, photons) will occur in the composite interface of the metamaterial microstructure (metal and dielectric material), such as surface plasmons, surface phonon polaritons, high-order electromagnetic modes, etc. These strong interactions can also compress the microwave absorption energy into a specific band. Therefore, metamaterials can efficiently change the amplitude, phase, polarization and propagation direction of the incident electromagnetic wave on a subwavelength scale. Based on the above principles, the present invention designs a surface microstructure of corresponding size on the graphene chloride material for the commonly used microwave detection wavelength band (2 to 18 GHz), so that the material's absorbing center wavelength is within the commonly used microwave detection wavelength band, which can more effectively dissipate and absorb microwave frequency band radiation.

[0058] like Figure 2 As shown, the patterned microstructure on the first graphene layer 1 is a first cross structure 10, the arm length of the first cross structure 10 is 4mm-8mm, and the arm width is 2mm-5mm; the patterned microstructure on the second graphene layer 3 is a second cross structure 20, the arm length of the second cross structure 20 is 1mm-3mm, and the arm width is 1mm-2mm. Figure 3 The patterned structure shown is a repetitive minimum unit, including a first cross structure 10 and four second cross structures 20, and the four second cross structures 20 are evenly placed in the four spaces divided by the first cross structure 10. The side length of the minimum unit is 10 mm, and the minimum unit can be periodically arranged horizontally and vertically to expand the coverage area to meet the needs of solar cell use.

[0059] By modifying graphene with chlorine doping and processing subwavelength structures on the material, the two wave-absorbing characteristics are coupled, which can maintain the material's high transmittance in the infrared and visible light bands while achieving high shielding efficiency in the microwave band. Figure 3 As shown, the average transmittance of the invisible space solar cell provided by the present invention in the 380-780nm band is greater than 87%, and the minimum value is ≥86%. Figure 4 As shown, the stealth space solar cell provided by the present invention achieves a transmittance of ≥86% in the infrared band of 780nm to 1000nm and a transmittance of ≥70% in the infrared band of 1000nm to 2000nm. The present invention couples the double-layer graphene chloride material to improve the microwave shielding effect and shielding bandwidth. Figure 5a and Figure 5bAs shown, the solar cell array not covered with the chlorinated graphene material has a scattering cross section of 0.9058dB at 0° and -13.71dB at 30° under radar detection at a center frequency of 9GHz; after being covered with the chlorinated graphene material provided by the present invention, the radar scattering cross section of the solar cell array is -10.06dB at 0° and -23.82dB at 30°. Compared with the two, the radar scattering cross section reduction ratio of the solar cell array is ≥90%. The shielding efficiency of the solar cell array covered with the chlorinated graphene material provided by the present invention is as follows: Figure 6 As shown in Figure 2, the cell efficiency of the solar array drops by less than 10%. Figure 7 As shown, the Fermi level of the material can be adjusted in the range of 0.25eV-0.6eV, and the corresponding absorption peak of the solar cell array can be moved from 9.0GHz to 10.6GHz.

[0060] In summary, the material provided by the present invention is chlorinated and doped with subwavelength microstructures, and has the advantages of wide spectrum, high transparency, low surface density, good wave absorption performance, and strong environmental adaptability. It provides technical support for the development of new satellite platforms in my country in the future. The application of this material to satellite solar arrays can effectively reduce the RCS of solar arrays, realize the stealth of solar arrays, enhance their concealment in space, and improve the safety threshold of spacecraft.

[0061] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as a limitation of the present invention. After reading the above content, it will be apparent to those skilled in the art that various modifications and substitutions of the present invention will occur. Therefore, the protection scope of the present invention should be limited by the appended claims.

Claims

1. A method for preparing a chlorinated graphene material, characterized in that: include: Using photolithography to prepare patterned microstructures on metal films; The metal film is placed on the target stage of the MOCVD system chamber and vacuumed to less than 10 -4 Torr; Introducing hydrogen and argon with a gas flow rate of 50sccm-100sccm and a target stage temperature of 800°C-1100°C; stopping the introduction of hydrogen and argon, introducing methane with a gas flow rate of 25sccm-50sccm, and a reaction time of 0.5h-3h, using methane as a carbon source and utilizing high-temperature decomposition of methane to deposit graphene on the metal film to prepare an intrinsic graphene material; Stop the introduction of methane, and introduce chlorine gas under visible light irradiation, with a gas flow rate of 30sccm-70sccm, a target stage temperature of 550℃-750℃, and a reaction time of 0.5h-2h; Stop introducing chlorine gas, and cool to room temperature at a rate of 5°C / s-20°C / s to obtain the chlorinated graphene material; Post-processing: degumming, pickling and peeling the graphene chloride material.

2. A chlorinated graphene material prepared by the method according to claim 1.

3. A stealth space solar cell, characterized in that: It includes a first graphene layer, a dielectric layer, a second graphene layer, a connecting layer and a battery structure which are stacked in sequence; The first graphene layer and the second graphene layer comprise the chlorinated graphene material of claim 2; The dielectric layer comprises silicon dioxide; The tie layer comprises polyvinyl butyral.

4. The invisible space solar cell according to claim 3, characterized in that: The first graphene layer includes a first cross structure, wherein the arm length of the first cross structure is 4mm-8mm and the arm width is 2mm-5mm.

5. The invisible space solar cell according to claim 3, characterized in that: The second graphene layer includes a second cross structure, wherein the arm length of the second cross structure is 1mm-3mm, and the arm width is 1mm-2mm.

6. The invisible space solar cell according to claim 3, characterized in that: The battery structure comprises a positive electrode, a space battery and a negative electrode stacked in sequence, wherein the positive electrode is arranged on one side of the connecting layer.

7. The invisible space solar cell according to claim 6, characterized in that: The space battery is a gallium arsenide battery; The positive electrode is a silver positive electrode with a thickness of 4 μm-6 μm; The negative electrode is a silver negative electrode with a thickness of 7 μm-9 μm.

8. The invisible space solar cell according to claim 3, characterized in that: The thickness of the dielectric layer is 110 μm-130 μm; The thickness of the connecting layer is 140 μm-160 μm.