Coating compositions and methods having multifunctional carbamates
The combination of potential alkali catalyst prepared by Michael addition reaction and crosslinkable resin components solves the problem of both the applicable period and weather resistance of the alkali catalytic coating system during rapid curing, and achieves environmentally friendly catalyst synthesis Efficient coating curing and weather resistance improve.
Patent Information
- Application Number
- CN202080058817.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-09-18
- Filing Date
- 2020-09-09
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2040-09-09
AI Technical Summary
The existing alkali catalytic coating system is difficult to take into account long application periods and excellent weather resistance during rapid curing, and the commonly used potential catalyst synthesis will produce environmentally harmful by-products, affecting performance.
Using a potential base catalyst prepared by Michael addition reaction, the substituted carbamate is used as a catalyst to react with the crosslinkable resin components to form a coating composition with the best applicable life and curing properties, and through hydroxide The reaction of functional components and multifunctional isocyanates prepares catalysts to ensure environmental protection and high efficiency.
The rapid curing and long application period of the coating composition is achieved, and the optimal weather resistance and corrosion resistance are demonstrated, while avoiding environmental pollution and meeting the requirements of low solvent content and high solids systems.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Background Art
[0001] Coatings are often applied to a variety of substrates, including metal and steel substrates, to protect the substrate from corrosion, impact and other damage, while also providing certain appearance or aesthetic features. Typically, these coatings are economical and relatively easy to apply. The coatings dry quickly and have good corrosion and chemical resistance, making the coatings particularly useful for coating metal parts that are to be used for long periods of time and / or in corrosive environments.
[0002] Typically, many coating systems are crosslinkable two-component compositions in which the components are stored separately and mixed prior to use. The two components are highly reactive and begin to crosslink as soon as they are mixed. Catalysts are often included in such primer coating systems to increase the rate of the crosslinking reaction between the two components.
[0003] The crosslinking reaction can be base catalyzed or acid catalyzed. Base catalyzed systems are sometimes preferred because they can cure quickly or rapidly. However, due to the fast cure rate, these compositions can only be used after the components are mixed and for a relatively short period of time, which is defined as the pot life of the coating composition. In some base catalyzed systems, the viscosity increases so quickly that the coating cures before it can be fully applied to the surface, and therefore, these systems have limited practical use.
[0004] Due to regulatory issues regarding the use of volatile organic compounds (VOCs) in solvent-based coatings, high solid systems with low solvent content are preferred. However, high solid systems present several challenges in balancing pot life and cure speed. For example, high solid compositions typically contain less solvent, which can evaporate when the coating is applied, and therefore, the pot life is much lower than is preferred. On the other hand, with less solvent in the system, the increase in reaction rate when the coating is applied is also reduced, resulting in slower curing. Therefore, conventional high solid coating systems are difficult to achieve a combination of fast curing and long pot life.
[0005] One possible solution to the problem of reduced pot life in base catalyzed systems is to use latent catalysts. These catalysts provide a favorable balance between cure speed and pot life. Typically, these catalysts are minimally activated until the coating is applied, and provide a longer pot life without compromising cure speed. For example, the use of substituted carbonates as latent catalysts for base catalyzed systems is described in U.S. Patent No. 8,962,725, which is incorporated herein by reference.
[0006] However, it is unknown whether coating compositions using such latent catalyst systems can be used as primer compositions, particularly where excellent weatherability and durability are desired. In addition, when some currently known base-catalyzed compositions are applied directly to metal substrates, particularly acidic substrates or acid-treated substrates, a loss of corrosion resistance and / or adhesion is observed.
[0007] Other potential catalysts for base catalyzed systems are also known, but their synthesis may include the formation of environmentally harmful byproducts that must be eliminated to meet regulatory requirements. For example, the synthesis of carbamate potential catalysts is described in U.S. Patent Publication No. 20180000720, which is incorporated herein by reference, where volatile amine byproducts are formed and must be removed to purify the product to obtain optimal performance. The presence of amines in the system can lead to undesirable side reactions, such as, for example, rapid crosslinking, which can reduce the pot life. In addition, the waste amine byproducts generated by the purification process can be environmentally harmful.
[0008] Therefore, there is a need for latent base catalysts that can take advantage of the fast cure speeds and optimal pot life exhibited by latent base catalyzed systems that crosslink via Michael addition reactions and also produce coating compositions with optimal corrosion and weathering resistance. Additionally, there is a need for methods of synthesizing latent base catalyst systems that are efficient and do not produce environmentally harmful byproducts. Summary of the invention
[0009] The present description provides compositions and methods involving Michael addition reactions catalyzed by latent base catalysts. The compositions described herein are derived from Michael addition reactions and provide coatings having optimal pot life and optimal cure properties and also exhibiting optimal weatherability.
[0010] In one embodiment, the present specification provides a latent base catalyst of general formula (I). The catalyst is a substituted carbamate capable of reacting with at least one crosslinkable component of the crosslinkable resin composition.
[0011] In another embodiment, this specification provides a coating composition, the coating composition comprises at least one crosslinkable polymer, the at least one crosslinkable polymer comprises at least one crosslinkable resin component. The composition comprises a potential base catalyst of formula (I), wherein the catalyst is a substituted carbamate capable of reacting with at least one crosslinkable resin component. In one aspect, based on the amount of the crosslinkable resin component, the potential catalyst is present in an amount of 0.001 meq to 1.0 meq. The coating composition exhibits an optimum pot life and an optimum curing response.
[0012] In another embodiment, a method for preparing a latent base catalyst is provided. The method comprises the following steps: providing a hydroxide functional component and a component capable of reacting with the hydroxide functional component to prepare a latent base catalyst having the general formula (I).
[0013] In one embodiment, the present specification provides a cured coating. The coating comprises a polymer composition comprising a crosslinkable resin component and a latent catalyst of formula (I). After being applied to a substrate, the polymer coating composition is cured at 150°F (65.5°C) within about 1 minute to 10 minutes to form a cured coating. As described herein, the cured coating exhibits optimal weatherability.
[0014] The above summary of the invention of the present invention is not intended to describe each disclosed embodiment or each implementation mode of the present invention. The following description more specifically illustrates exemplary embodiments. In several places of the full text of this application, guidance is provided by lists of examples, which can be used in various combinations. In each case, the cited lists are only used as representative groups and should not be interpreted as exclusive enumeration.
[0015] The details of one or more embodiments of the invention are set forth in the description below. Other features, objects, and advantages of the invention will be apparent from the description and from the claims.
[0016] Selected Definition
[0017] Unless otherwise indicated, the following terms as used herein have the meanings provided below.
[0018] As used herein, the term "organic group" means a hydrocarbon group (it has optional elements other than carbon and hydrogen, such as oxygen, nitrogen, sulfur and silicon), which is classified as aliphatic groups, cyclic groups or aliphatic groups and cyclic groups The combination of groups (for example, alkylaryl groups and aralkyl groups). The term "aliphatic group" means a saturated or unsaturated straight or branched hydrocarbon group. For example, the term is used to cover alkyl, alkenyl and alkynyl groups. The term "alkyl group" means a saturated straight or branched hydrocarbon group, including, for example, methyl, ethyl, isopropyl, tetrabutyl (tert-butyl), heptyl, dodecyl, octadecyl, amyl, 2-ethylhexyl, etc. The term "alkenyl group" means an unsaturated, straight or branched hydrocarbon group with one or more carbon-carbon double bonds, such as a vinyl group. The term "alkynyl group" means an unsaturated, straight or branched hydrocarbon group with one or more carbon-carbon triple bonds. The term "cyclic group" means a closed ring hydrocarbon group, which is classified as an alicyclic group or an aromatic group, both of which may contain heteroatoms. The term "alicyclic group" means a cyclic hydrocarbon group whose properties are similar to those of an aliphatic group. The term "Ar" refers to a divalent aryl group (i.e., an arylene group), which refers to a closed aromatic ring or ring system, such as phenylene, naphthylene, biphenylene, fluorenylene and indenyl, and a heteroarylene group (i.e., a closed ring hydrocarbon in which one or more atoms in the ring are elements other than carbon (e.g., nitrogen, oxygen, sulfur, etc.)). Suitable heteroaryl groups include furanyl, thienyl, pyridinyl, quinolyl, isoquinolyl, indolyl, isoindolyl, triazolyl, pyrrolyl, tetrazolyl, imidazolyl, pyrazolyl, oxazolyl, thiazolyl, benzofuranyl, benzothiophenyl, carbazolyl, benzoxazolyl, pyrimidinyl, benzimidazolyl, quinoxalinyl, benzothiazolyl, naphthyridinyl, isoxazolyl, isothiazolyl, purinyl, quinazolinyl, pyrazinyl, 1-oxopyridinyl, pyridazinyl, triazinyl, tetrazinyl, oxadiazolyl, thiadiazolyl, etc. When such groups are divalent, they are often referred to as "heteroarylene" groups (e.g., furanylene, pyridinylene, etc.).
[0019] The group that can be the same or different is referred to as something "independently". It is expected that the organic group of the compounds of the present invention is substituted. As a means of simplifying the discussion and expression of some terms used in the application, the terms "group" and "part" are used to distinguish between chemical species that allow substitution or can be substituted and those chemical species that do not allow or may not be substituted in this way. Therefore, when the term "group" is used to describe a chemical substituent, the chemical substance includes an unsubstituted group, and for example, in a chain (such as in an alkoxy group) there is an O, N, Si or S atom and a carbonyl group or other conventionally substituted group. In the case where the term "part" is used to describe a chemical compound or a substituent, it is only intended to include unsubstituted chemicals. For example, the phrase "alkyl group" is intended to include not only pure open-chain saturated hydrocarbon alkyl substituents, such as methyl, ethyl, propyl, tert-butyl, etc., but also includes alkyl substituents with other substituents known in the art (such as hydroxyl, alkoxy, alkyl sulfonyl, halogen atoms, cyano, nitro, amino, carboxyl, etc.). Thus, "alkyl groups" include ether groups, haloalkyl groups, nitroalkyl groups, carboxyalkyl groups, hydroxyalkyl groups, sulfoalkyl groups, etc. On the other hand, the phrase "alkyl moiety" is restricted to include only pure open-chain saturated hydrocarbon alkyl substituents, such as methyl, ethyl, propyl, tert-butyl, etc.
[0020] The term "component" refers to any compound containing a particular feature or structure. Examples of components include compounds, monomers, oligomers, polymers, and organic groups contained therein.
[0021] The term "double bond" is non-limiting and refers to any type of double bond between any suitable atoms (eg, C, O, N, etc.).
[0022] The term "triple bond" is non-limiting and refers to any type of triple bond between any suitable atoms.
[0023] As used herein, "Michael addition" refers to the nucleophilic addition of a carbanion or other nucleophile to an electron-deficient ethylenically unsaturated compound, such as, for example, an α,β-unsaturated carbonyl compound. The abbreviation "MA" is used interchangeably herein with the term "Michael addition".
[0024] The Michael addition reaction follows the general reaction formula shown here:
[0025]
[0026] In the reaction scheme shown above, B is a latent base catalyst that reacts with a Michael addition (MA) donor by deprotonation to form a carbanion for subsequent addition reaction with a MA acceptor.
[0027] As used herein, the term "resin composition" refers to the resin-containing portion of the composition. The resin composition may include one or more resins or polymer compositions. Suitable examples include, but are not limited to, MA donors, MA acceptors, non-functional resins, and resins having functional groups other than those required for Michael addition. The term is used interchangeably herein with "polymer" or "polymer composition". As used herein, a resin or polymer composition may include one or more resin components.
[0028] "Michael Addition Acceptor" or "MA Acceptor" means a molecule having at least one MA acceptor functional group.
[0029] "Michael addition donor" or "MA donor" means a molecule having at least one MA donor functional group.
[0030] "MA acceptor / donor" means a molecule having at least one Michael addition (MA) acceptor functional group and at least one Michael addition (MA) donor functional group.
[0031] The term "crosslinking agent" refers to a molecule that is capable of forming a covalent bond between polymers or between two different regions of the same polymer. A particular component is said to be "crosslinkable" if it can react with another component via a crosslinking reaction, via a self-crosslinking reaction, or by a reaction of two or more polymers or between two different regions of the same polymer.
[0032] When used in the context of a self-crosslinking polymer, the term "self-crosslinking" refers to the ability of a polymer to enter into a crosslinking reaction with itself and / or with another molecule of the polymer to form covalent bonds therebetween in the absence of an external crosslinking agent. Typically, this crosslinking reaction is carried out by reaction of complementary reactive functional groups present on the self-crosslinking polymer itself or on two separate molecules of the self-crosslinking polymer.
[0033] In the context of a dispersible polymer, the term "dispersion" refers to a mixture of the dispersible polymer and the carrier. The term "dispersion" is intended to include the term "solution".
[0034] When used in the context of a coating applied to a surface or substrate, the term "on" includes both coatings applied directly or indirectly to the surface or substrate. Thus, for example, a coating applied to a primer layer covering a substrate constitutes a coating applied to the substrate.
[0035] As used herein, the term "dry to process" refers to the stage of the coating process of a substrate where the applied coating is sufficiently cured to move to the next stage of the manufacturing process.
[0036] Unless otherwise indicated, the term "polymer" includes both homopolymers and copolymers (ie, polymers of two or more different monomers).
[0037] The terms "comprises" and variations thereof do not have a limiting meaning when they appear in the description and claims.
[0038] The terms "preferred" and "preferably" refer to embodiments of the present invention that may provide certain benefits in certain circumstances. However, other embodiments may also be preferred under the same or other circumstances. In addition, the description of one or more preferred embodiments does not imply that other embodiments are unusable, and is not intended to exclude other embodiments from the scope of the present invention.
[0039] As used herein, "a", "an", "the", "at least one", and "one or more" are used interchangeably. Thus, for example, a coating composition comprising "an" additive can be interpreted to mean that the coating composition comprises "one or more" additives.
[0040] Also herein, numerical ranges recited by endpoints include all values contained within that range (e.g., 1 to 5 includes 1, 1.5, 2, 2.75, 3, 3.80, 4, 5, etc.). In addition, disclosure of a range includes disclosure of all subranges included in the broader range (e.g., 1 to 5 discloses 1 to 4, 1.5 to 4.5, 1 to 2, etc.). DETAILED DESCRIPTION
[0041] The present specification provides a latent base catalyst, a method for preparing such a catalyst, and a coating composition for various substrates including metal substrates and steel substrates. In particular, the present specification provides a coating composition for untreated or pretreated substrates, including, for example, steel substrates, wherein the coating is derived from a component that is cured via a latent base-catalyzed Michael addition reaction as described herein.
[0042] The present specification provides a latent base catalyst. In one aspect, the latent base catalyst is a substituted carbamate having a structure of general formula (I):
[0043]
[0044] in:
[0045] Each X + independently a non-acidic cation;
[0046] Each R1 is independently H, C1 to C10 alkyl, aryl, aralkyl, or C1 to C10 substituted alkyl, aryl, aralkyl, or a mixture or combination thereof;
[0047] Each R2 and R3 is independently a C1 to C10 alkyl, aryl, aralkyl, or a C1 to C10 substituted alkyl, aryl, aralkyl, or a mixture or combination thereof;
[0048] and
[0049] n is greater than 1.
[0050] The latent base catalyst having the structure of formula (I) is capable of reacting with at least one crosslinkable component of a crosslinkable polymer or resin composition.
[0051] Without being bound by theory, it is believed that the latent base catalyst of general formula (I) works by releasing carbon dioxide when the carbamate decomposes as a wet film applied to a substrate. In a closed reactor, this reaction occurs slowly, allowing an extended pot life. When the coating is applied and the surface area increases, the base is rapidly regenerated when the carbon dioxide escapes from the surface, allowing faster curing (i.e., drying and hardness development) of the coating. Therefore, the use of the latent base catalyst of general formula (I) allows for the optimal pot life, open time and curing properties of the crosslinkable coating composition described herein.
[0052] In the latent base catalyst having the structure of general formula (I), X + Wherein n in formula (I) is greater than 1, each X in a unit of the potential base catalyst + Can be combined with X in another unit of the same potential base catalyst molecule + Same or different.
[0053] Suitable examples include, but are not limited to, alkali metal ions, alkaline earth metal ions, ammonium ions, phosphonium ions, and the like. + is a lithium ion, a sodium ion or a potassium ion. More preferably, X + is a quaternary ammonium ion NR'4 or a phosphonium ion PR'4, wherein R is H, an unsubstituted C1-C10 alkyl, aryl, aralkyl, a substituted C1-C10 alkyl, aryl, aralkyl, and a mixture or combination thereof. In a preferred aspect, R is an unsubstituted alkyl group having 1 to 4 carbon atoms. If the R group is substituted, the substituent is selected to not substantially interfere with the crosslinking reaction. In one aspect, in order to avoid interfering with the action of the base catalyst, an acidic substituent, such as, for example, a carboxylic acid substituent, is present only in a small amount or is not present at all.
[0054] In the latent base catalyst of general formula (I), R1 is H, C1 to C10 alkyl, aryl, aralkyl, or C1 to C10 substituted alkyl, aryl, aralkyl, or a mixture or combination thereof. In a preferred aspect, R1 is hydrogen.
[0055] In the potential base catalyst of general formula (I), R2 and R3 are each independently C1 to C10 alkyl, aryl, aralkyl, or C1 to C10 substituted alkyl, aryl, aralkyl, or a mixture or combination thereof. In a preferred aspect, R2 and R3 are each independently an unsubstituted alkyl group having 1 to 4 carbon atoms, more preferably 4 carbon atoms.
[0056] The latent catalysts described herein are substituted carbamates synthesized by the reaction of a hydroxide functional component with a component capable of reacting with the hydroxide functional component. In one aspect, the hydroxide functional component is a hydroxide base and the component capable of reacting with the hydroxide base is a polyfunctional isocyanate.
[0057] Suitable hydroxide bases for use in the methods described herein include, but are not limited to, tetrahexylammonium hydroxide, tetradecyl-(i.e., C14)-trihexylammonium hydroxide and tetradecylammonium hydroxide, tetrabutylammonium hydroxide, benzyltrimethylammonium hydroxide, or trihexylmethylammonium hydroxide or trioctylmethylammonium hydroxide, and mixtures or combinations thereof.
[0058] In order to prepare a potential base catalyst as described herein, a hydroxide functional component is reacted with a polyfunctional isocyanate. Suitable polyfunctional isocyanate compounds include, but are not limited to, 2,4-toluene diisocyanate, hexamethylene diisocyanate (HDI), polymethylene-polyphenyl diisocyanate, methylene diphenyl diisocyanate, cyclic trimers, cocyclic trimers, their homopolymers, copolymers or mixtures. In a preferred embodiment, polyfunctional isocyanate is a trimer. The example of a suitable trimer includes, but is not limited to, a trimer product prepared by an average of three diisocyanate molecules, or a trimer prepared by reacting an average of three moles of diisocyanate (e.g., HDI) with one mole of another compound (such as, for example, triol (e.g., trimethylolpropane)). In a preferred aspect, polyfunctional isocyanate is an HDI trimer.
[0059] The reaction of the hydroxide functional component with the polyfunctional isocyanate can be carried out in the presence of an alcohol such as, for example, methanol. Without being bound by theory, when the reaction is carried out in the presence of an alcohol, it is believed that any isocyanate that does not react with the hydroxide has reacted with excess methanol in solution. However, it is not necessary to react in the presence of an alcohol, and the alcohol can be added at the end of the synthesis, i.e., after the hydroxide functional component has reacted with the polyfunctional isocyanate.
[0060] The potential catalyst described herein is a carbamate made by reacting a hydroxide base (preferably tetrabutylammonium hydroxide) with a multifunctional isocyanate (preferably a trimer of HDI). In one aspect, the potential catalyst described herein comprises more than one carbamate moiety, preferably two or more carbamate moieties. In one aspect, the ratio of hydroxide groups to isocyanate groups in the potential catalyst is 0.60:1.0 to 0.99:1.0, preferably 0.7:1.0 to 0.99:1.0. More preferably, the potential catalyst has a ratio of hydroxide groups to isocyanate groups of 0.9:1.0, i.e., the index of the catalyst relative to the amount of isocyanate groups present is 0.9. Any excess isocyanate in the system that does not react with the hydroxide will react with excess methanol, water or other solvents present in the solution.
[0061] In a preferred aspect, the latent base catalyst is prepared by reacting tetrabutylammonium hydroxide (TBAH) with hexamethylene diisocyanate. The latent base catalyst has a structure shown in formula (II).
[0062]
[0063] In one embodiment, the latent catalyst described herein is a carbamate prepared by reacting a hydroxide base with a polyfunctional isocyanate, wherein the reaction is super-exponential with respect to the polyfunctional isocyanate. That is, the reaction includes an excess of isocyanate to ensure complete conversion of the hydroxide to the carbamate. Any excess isocyanate remaining after the reaction is consumed by excess methanol, water or other solvent present in the solution.
[0064] In another embodiment, the latent catalyst described herein is a carbamate made by reacting a hydroxide base with a multifunctional isocyanate, wherein the reaction is super-exponential in terms of the hydroxide. That is, the reaction includes excess hydroxide to ensure complete conversion to the carbamate. Any excess hydroxide remaining after the reaction can be titrated with acid addition to remove excess base from the system. In one embodiment, the excess hydroxide is present in an amount of up to about 10%, preferably less than 10%, and more preferably the minimum excess that actually consumes all of the isocyanate.
[0065] The latent catalysts described herein are used to prepare coating compositions, including two-component coating compositions. In one aspect, the coating composition is prepared by reacting the latent catalyst with a crosslinkable polymer composition via a Michael addition reaction. The polymer composition comprises at least one crosslinkable resin component, but may also comprise non-functional resins, resins having functional groups other than those required for Michael addition, and the like.
[0066] The Michael addition reaction involves the nucleophilic addition of a carbanion or other nucleophile to an electron-deficient olefinic compound. The nucleophile is called a Michael addition (MA) donor and can be any organic compound containing at least one active hydrogen and at least one electron withdrawing group such as, for example, -CN, -COOR, -COR, etc. The Michael addition (MA) acceptor is typically an ethylenically unsaturated compound having a double bond that can be activated by a carbonyl group at the alpha position.
[0067] Suitable examples of MA donors include, but are not limited to, dialkyl malonates (e.g., dimethyl malonate, diethyl malonate, etc.), cyanoacetates (e.g., methyl cyanoacetate, ethyl cyanoacetate, etc.), chloroacetates, acetoacetates, propionylacetates, malononitrile, acetonitrile, acetylacetone, dipropionylmethane, etc., and mixtures or combinations thereof. Preferred examples of MA donors include, but are not limited to, oligomeric and polymeric compounds containing malonate or acetoacetate groups, such as, for example, polyesters, polyurethanes, polyacrylates, epoxy resins, polyamides, and polyvinyl resins containing malonate or acetoacetate functional groups in the main chain, side chains, or both.
[0068] Suitable examples of MA acceptors include, but are not limited to, esters of (meth)acrylic acid, i.e., (meth)acrylate functional compounds derived from the reaction of a hydroxyl functional compound (i) with (meth)acrylic acid or its ester derivative (ii), wherein the hydroxyl functional compound may be monofunctional, difunctional or polyfunctional and have as a backbone containing an aliphatic, alicyclic or aromatic chain: (poly)epoxies, (poly)ethers, (poly)esters (e.g. (poly)caprolactones), (poly)alkyds, (poly)urethanes, (poly)amines, (poly)amides, (poly)carbonates, (poly)olefins, (poly)siloxanes, (poly)acrylates, halogens (e.g. fluorine), melamine-derivatives, copolymers of any of them, etc., and mixtures and combinations thereof.
[0069] The crosslinkable polymer composition may include one or more MA donor components and one or more MA acceptor components. In a preferred aspect, the crosslinkable polymer composition includes at least one malonate functional MA donor component and at least one acrylate functional MA acceptor component. Exemplary crosslinkable compositions are described in the applicant's co-pending patent application PCT / US2019 / 031069 filed on May 7, 2019, which is incorporated herein by reference.
[0070] Without being bound by theory, it is believed that the MA acceptor and MA donor components will react via a Michael addition reaction and thereby contribute to improved cure speed, crosslink density and hardness development of the coating compositions described herein. Improved cure and increased crosslink density will lead to improved performance properties.
[0071] The MA donor and MA acceptor are present in a crosslinkable polymer composition that reacts with the latent base catalyst described herein to produce a coating composition having optimal curing properties and optimal weathering properties. In one aspect, the crosslinkable polymer composition is one part (e.g., part A) of a two-component coating composition, wherein the latent base catalyst described herein is the other part (e.g., part B).
[0072] The coating compositions described herein are prepared by reacting a latent base catalyst (part B) with a crosslinkable polymer composition (part A), wherein the ratio of A:B may vary depending on the reaction conditions and the desired end use. In one embodiment, the amount of the latent base catalyst used herein may vary depending on the characteristics of the coating composition. Preferably, the composition comprises from about 0.001 meq to 1 meq, more preferably from 0.02 meq to 0.07 meq, based on the amount of resin solids in the composition.
[0073] In one embodiment, a non-latent base catalyst may be used alone or in combination with a latent base catalyst as described herein to accelerate the Michael addition reaction. Examples of suitable non-latent catalysts include, but are not limited to, tetrabutylammonium hydroxide, ammonium hydroxide, DBU (8-diazabicyclo [5.4.0] undec-7-ene), DBN (1,5-diazabicyclo [4.3.0] non-5-ene), and TMG (1,1,3,3-tetramethylguanidine).
[0074] Suitable additional examples of non-latent catalysts include, but are not limited to, reactions with basic anions X from compounds containing acidic XH groups. - Paired non-acidic cations (such as K + 、Na + , Li + ) or a salt of a weakly acidic cation such as, for example, a protonated species of a strong organic base such as, for example, DBU, DBN, etc., or TMG, etc., wherein X is N, P, O, S or C, and the anion X - is a MA donor capable of reacting with a MA acceptor (e.g., acrylate), and the anion X - The pKa of the corresponding acid XH is more than two units lower than the pKa of most donor components (e.g., acetoacetate functional resins). Suitable examples of such salts include, but are not limited to, salts formed by the reaction of KOH and benzotriazole, TBAH and benzotriazole, or KOH and 1,2,4-triazole, which are contained in a content between 0.001 meq / g solid resin and 1 meq / g solid resin. The above mixture or combination can be used. A preferred non-latent catalyst is a solution of potassium benzotriazole, which is formed by reaction of KOH and benzotriazole in ethanol in an equimolar ratio.
[0075] Optionally, to extend the open time and pot life, one or more additional components may be included, such as, for example, one or more acidic X'-H groups, where X' is N, P, O, S or C, where the X' anion is a MA donor capable of reacting with a MA acceptor, and the pKa of the X'-H group is lower than the pKa of most MA donors (e.g., acetoacetate functional resins), preferably more than 2 units lower. Suitable examples include, but are not limited to, ethyl acetoacetate, benzotriazole, succinimide, acetylacetone or 1,2,4-triazole, and mixtures or combinations thereof. In a preferred aspect, the component is benzotriazole, which is present in an amount between about 0.5% and 5%, more preferably between about 0.5% and 1.5%, based on the total weight of the resin solids.
[0076] In one embodiment, the coating composition described herein comprises an acid scavenging component or a pH buffering component. Suitable examples include, but are not limited to, metal oxides (e.g., zinc oxide, nanoparticulate zinc oxide, magnesium oxide, calcium oxide, strontium oxide, barium oxide, lanthanum oxide, ytterbium oxide, zirconium oxide, etc.), mixed metal oxides (e.g., MgO-TiO2, etc.), zeolites (e.g., cesium exchanged zeolites, X, Y-Cs intercalated zeolites, etc.), modified mesoporous materials (e.g., MgO-coated mesoporous silica (SBA-15), amino-functionalized mesoporous silica (MCM-41), mesoporous silicon oxynitrides, etc.), metal hydroxides (e.g., calcium hydroxide, Na / NaOH / Al2O3, Na / MgO, etc.), metal nitrides, metal oxides, etc. Nitrides (e.g., silicon oxynitride, aluminum oxynitride phosphate, zirconium oxynitride phosphate, calcined NaNO3, etc.), metal carbonates (e.g., calcium carbonate, sodium carbonate, potassium carbonate, etc.), metal silicates (e.g., calcium silicate, calcium borosilicate, magnesium silicate, Mg-Al hydrotalcite, chrysotile, etc.), metal carboxylates (e.g., titanium acetoacetate, etc.), organometallic compounds (e.g., organic zirconates, weakly basic titanates, tetraalkyl titanates, etc.), amines (e.g., guanidine, aziridine, amidine, triethanolamine, DMP30, etc.), imides (e.g., carbodiimide, etc.), diazabicyclic compounds (e.g., DABCO, etc.), and mixtures or combinations thereof.
[0077] Thus, the coating compositions described herein can be applied over an acidic substrate such as, for example, a metal substrate having a pretreatment applied thereto. Suitable examples of pretreatments include, but are not limited to, iron phosphate, zinc phosphate, silane, zirconium, and the like. Many other pretreatments are known in the metal pretreatment industry. In a preferred aspect, the metal substrate has an iron phosphate treatment applied thereto.
[0078] The coating composition described herein may also include other optional ingredients that do not adversely affect the coating composition or the cured coating composition produced therefrom. Such optional ingredients are generally included in the coating composition to enhance the coating aesthetics; promote the manufacture, processing, treatment and application of the composition; and further improve the specific functional properties of the coating composition or the cured coating composition produced therefrom. For example, the composition described herein may optionally include adhesion promoters, fillers, catalysts, lubricants, pigments, surfactants, dyes, colorants, toners, coalescing agents, extenders, preservatives, flow control agents, thixotropic agents, dispersants, antioxidants, adhesion promoters, light stabilizers, and mixtures thereof, such as those required to provide the desired film properties. Each optional ingredient is preferably included in an amount sufficient for its intended purpose, but not in an amount that adversely affects the coating composition or the cured coating composition produced therefrom.
[0079] In one embodiment, in addition to the MA donors and MA acceptors described herein, the compositions described herein may also include resin components that do not undergo Michael addition reactions. These additional resin components may have no reactive functional groups or have reactive functional groups that undergo reactions other than Michael addition reactions.
[0080] In one embodiment, coating composition as described herein may include solvent. Suitable solvent can be aqueous, organic or their mixture. Suitable examples of organic solvents include but are not limited to aliphatic solvents, aromatic solvents and / or alkylated aromatic solvents (e.g., toluene, xylene, etc.), alcohols (e.g., isopropanol), esters (e.g., methoxypropanol acetate, butyl acetate, isobutyl acetate, etc.), ketones (e.g., methyl ethyl ketone, methyl amyl ketone, etc.), glycol ethers, glycyl ether esters, and mixtures or combinations thereof. In one aspect, coating composition as described herein has low volatile organic compound (VOC) content, preferably less than 400g / L, more preferably less than 300g / L, and most preferably less than 250g / L.
[0081] The compositions described herein also show comparable shelf life and an optimal balance of pot life and drying time relative to conventional polyurethane coatings and knowledge of such coatings in the art. In one aspect, the compositions described herein have an optimal shelf life and do not exhibit a loss of cure response or any viscosity increase after storage at a temperature of about 120F (48.8°C) for at least one week. In another aspect, the coating compositions described herein also exhibit an optimal pot life, wherein the composition takes preferably longer than 60 minutes, more preferably longer than 120 minutes, after mixing, to double in viscosity.
[0082] In one embodiment, the coating compositions described herein exhibit an improved curing response relative to systems without a latent base catalyst. In one aspect, the coating compositions described herein have an optimal curing response, as assessed by a pencil hardness test after the coating is applied to a substrate and cured. The optimal curing response means that after drying at ambient temperature (including, for example, at room temperature of 75F to 77F (approximately 24°C to 25°C)), the coating composition dries within about 1 minute to 30 minutes, preferably about 1 minute to 10 minutes for processing. Optimal curing can also be affected by baking at elevated temperatures, including at about 100F (37.7°C), 200F (93.3°C), 300F (148.9°C) and even higher temperatures. In a preferred aspect, the optimal curing response is observed when the coating composition is baked at a temperature of about 150F (65.5°C).
[0083] The coating compositions described herein can be used as primers or can be part of primer formulations. When used as primers or in primer formulations, the compositions described herein can be applied to untreated substrates, pretreated substrates, substrates having a temporary coating applied thereon, and the like.
[0084] The coating compositions described herein exhibit optimal corrosion resistance when used as primers.Best corrosion resistance means that after salt spray exposure, the cured coating derived from the compositions described herein shows a scratch creep of less than 3 mm, preferably less than 2 mm.
[0085] Coating composition as herein described can be used as topcoat.In one aspect, first coating (such as, primer) is applied to untreated substrate, pretreated substrate, substrate with temporary coating applied thereon etc. above.Then, if necessary, second coating (such as, topcoat) is applied above primer.In one aspect, second coating is applied only after first coating is completely dried or solidified.In alternative aspect, before first coating is completely dried or solidified, second coating is applied above first coating.
[0086] Composition as herein described can be used as both primer and finish paint, as a part of the coating system applied to substrate. In one aspect, the first coating (i.e. coating composition as herein described) is applied as primer to untreated substrate, pretreated substrate, substrate with temporary coating applied thereon etc. above. Then, if necessary, the second coating (i.e. coating composition as herein described) is applied to the primer top. In one aspect, the second coating is applied only after the first coating has been completely dried or solidified. In alternative aspect, before the first coating has been completely dried or solidified, the second coating is applied to the first coating top.
[0087] The coating compositions described herein are intended for exterior use and / or intended as weatherable coatings, e.g., applied as a topcoat or directly in contact with metal (single coat), i.e., the cured coatings formed from the compositions described herein exhibit optimal weatherability. Optimal weatherability means that the coating exhibits at least 60%, preferably at least 70%, 20° gloss retention, and at least 70%, preferably at least 80% 60° gloss retention after 2000 hours of accelerated weathering in a xenon arc weathering chamber. Alternatively, if the measured color shift (ΔE 00 ) is less than 1.0 unit, preferably less than 0.5 unit, the coating has optimal weather resistance.
[0088] In one embodiment, the coating composition as described herein can be used as a primer, and any topcoat can be applied above the primer. In one aspect, the topcoat composition is also obtained by Michael addition reaction. The topcoat derived from the Michael addition can be the same or different from the primer composition derived from the Michael addition as described herein. On the other hand, the topcoat composition can be a component that is not derived from the Michael addition reaction, but is known in the art as a suitable topcoat material (such as, for example, a polyurethane topcoat).
[0089] In general, Michael addition derived coating compositions have demonstrated improved cure response relative to conventional primers made with polyurethanes, epoxies, non-isocyanate systems, etc. However, the use of such Michael addition derived coatings has been limited due to poor adhesion to various substrates, and due to lack of corrosion resistance, particularly when applied as a primer or as a direct to metal (DTM) coating on metal substrates, particularly pretreated steel substrates. Surprisingly, the Michael addition derived coating compositions described herein can be used as primers or DTM coatings with optimal corrosion resistance.
[0090] The coating composition of the present invention can be applied to the substrate before or after the substrate is formed into an article. In one aspect, the coating composition described herein can be applied on various substrates. Suitable examples include but are not limited to natural and engineered buildings and building materials, freight containers, floor materials, walls, furniture, other building materials, motor vehicles, motor vehicle parts, aircraft parts, trucks, rail vehicles and engines, bridges, water towers, telephone towers, wind towers, radio towers, lighting devices, statues, signboard brackets, fences, guardrails, tunnels, pipelines, ship parts, mechanical parts, laminates, equipment parts, electrical appliances and packaging. Exemplary substrate materials include but are not limited to wood, plastics, thermosetting materials, metals, metal alloys, intermetallic compositions, metal-containing composite materials and these combinations. Exemplary metal substrates include but are not limited to aluminum, steel, weathering steel and stainless steel. In a preferred aspect, the substrate is steel, preferably pretreated steel is applied thereon.
[0091] The coating compositions described herein can be applied by any method known in the art. Standard application methods include, but are not limited to, such as by brushing, spraying, spin coating, roller coating, curtain coating, dipping, gravure coating, bell coating, etc. In the case of a two-component thermosetting substrate, the coating can be applied via an in-mold process. When the coating composition is applied by a spraying method, conventional air or air-assisted spray equipment or airless spray equipment can be used. Both electrostatic equipment and non-electrostatic equipment can be used.
[0092] The coating thickness of the specific layer and the entire coating system will vary depending on the coating material used, the substrate, the coating application method and the end use of the coated article. When used as a primer applied over an untreated or pretreated metal substrate, the thickness of the applied coating film is preferably about 0.05 mil to 20 mils (1.27 microns to 500 microns), more preferably 0.4 mil to 40 mils (10 microns to 100 microns), and even more preferably 1.0 mil to 2.5 mils (25 microns to 70 microns).
[0093] Example
[0094] The present invention is illustrated by the following examples. It should be understood that the specific embodiments, materials, amounts and procedures are broadly interpreted according to the scope and essence of the present invention as described herein. Unless otherwise indicated, all parts and percentages are by weight, and all molecular weights are weight average molecular weights. Unless otherwise indicated, all chemicals used are commercially available from, for example, Sigma-Aldrich (St.Louis, Missouri).
[0095] Unless otherwise indicated, the following test methods were utilized in the following examples.
[0096] Corrosion resistance (salt spray)
[0097] The corrosion resistance of the cured coatings prepared using the compositions and methods described herein was tested using a salt spray method, as described in ASTM B117 (standard practice for operating salt spray equipment). The results are represented by the degree of blistering (ASTM D714), rusting (ASTMD610), and scratch creep (ASTM D1654-08). Scratch creep is represented on a scale of 0 to 10, where 0 indicates extensive corrosion at the scratch, and 10 indicates that the coating does not change due to exposure to a corrosive environment. Rust ratings for coatings subjected to salt spray exposure in a humid environment are also represented on a scale of 0 to 10, where 0 indicates complete surface rusting, and 10 indicates no surface rusting. The blistering rating is represented on a scale of 0 to 10, where 0 is excessive blistering, and 10 is no blistering.
[0098] Corrosion resistance (creep)
[0099] The corrosion resistance of the cured coating formed by the composition described herein is also tested by measuring creep after exposure to a corrosive environment, as described in ASTM D1654-08 (Standard Test Method for Evaluating Painted or Coated Specimens Subjected to Corrosive Environments). The coating is applied to a panel and then cured. The panel is then scratched to metal and exposed to salt spray for a given period of time. The paint loss due to the scratch is measured and the results are expressed as the amount of scratch creep (in mm). For commercially viable coatings, the scratch creep is expected to be 2 mm or less.
[0100] Application period evaluation
[0101] The pot life of the coating compositions described herein is determined by measuring the viscosity of the composition over a given period of time under a given set of conditions (such as, for example, at room temperature, or after storage in a hot box, etc.). In the examples herein, viscosity is determined as follows. A Zahn cup is dipped into a sample of the coating composition and completely filled with the sample. The cup is then raised and the flow time of the sample is measured in seconds and reported along with the specific Zahn cup number. The pot life is reported as the time it takes for a sample of the coating composition to double in viscosity.
[0102] Effective curing (hardness)
[0103] The curing effectiveness of the coating can be evaluated by measuring the hardness of the cured coating using the pencil hardness method, as described in ASTM D3363 (Standard Test Method for Obtaining Film Hardness by Pencil Test). Pencils with different hardnesses ranging from 6B (softest) to 6H (hardest) are applied to the surface of the cured coating. The results are expressed as the hardest pencil that does not scratch or scratch the surface of the cured coating applied to the test panel. Thus, for example, if the coating does not break with a 2H pencil but breaks when a 3H pencil is used, the pencil hardness of the coating is 2H.
[0104] Curing speed (Konig)
[0105] The hardness of the cured coating can also be evaluated by the Konig pendulum hardness method as described in ASTM D4366 (Standard Test Method for Hardness of Organic Coatings by Pendulum Damping Test). A pendulum is allowed to oscillate above the cured coating, and the hardness of the cured coating is expressed as the damping time (in seconds) for the pendulum deflection to slow to a specific value.
[0106] Catalyst stability
[0107] Hardness measurements can also be used to evaluate the stability of potential catalysts described herein. The catalysts are stored in a hot box for a given period of time, after which the hardness of the cured coatings prepared with the catalysts and baked at a given temperature for a given period of time is tested using both the pencil hardness method and the Konig pendulum hardness method.
[0108] Example 1: Synthesis of Catalyst and Coating Compositions
[0109] 6.59 g of OXSOL 100 was added to a 10% methanol solution of 3.68 g of tetrabutylammonium hydroxide (TBAH) and mixed. Then, 1.32 g of a solution of hexamethylene diisocyanate trimer (HDI trimer) was added dropwise with sufficient mixing. The ratio of hydroxyl groups to isocyanate functional groups was maintained at 0.9:1.0, resulting in excess isocyanate. It is believed that any isocyanate that did not react with the hydroxide has reacted with excess methanol in the solution.
[0110] The 0.9 index catalyst prepared above (Part B) was mixed with a batch of finished paint (Part A) containing a malonate functional Michael addition donor component and an acrylate functional Michael addition acceptor component. Parts A and B were mixed in a 10:1 (A:B) ratio to form a coating composition of the present invention. As a control, a composition was prepared using the same Part A described above in combination with a 6% solution (i.e., a diluted solution) of a latent catalyst as Part B (commercially available as ACURE 500 from Allnex).
[0111] Example 2: Curing performance
[0112] The control and inventive coating compositions prepared in Example 1 were applied to pretreated metal test panels at a dry film thickness of about 2 mils (50.8 μm). The curing properties of the coatings were then evaluated by curing the coatings at a given temperature as indicated in Table 1 below and baking the coatings for a given period of time, and then testing the pencil hardness and Konig pendulum hardness of the cured coatings. The results are shown in Table 1.
[0113] Table 1. Curing properties of coating compositions
[0114]
[0115] Example 3: Stability of Catalyst
[0116] To evaluate the stability of the latent base catalysts described herein, the 0.9 index catalyst prepared in Example 1 was placed in a hot box at 120°F (48.8°C) for one week. The curing properties of the coatings were then evaluated as in Example 2. For comparison, a control sample as in Example 2 was used. The results of the curing properties are shown in Table 2.
[0117] Table 2. Curing properties of coating compositions after hot box
[0118]
[0119] Example 4: Pot life
[0120] To determine the effect of the potential catalysts described herein on the pot life of the coating compositions, the 0.9 index catalyst (Part B) of Example 1 was mixed with a batch of the finished paint (Part A) of Example 1 at a 10:1 (A:B) ratio. The initial viscosity was measured with a #3 marked Zahn cup and again after 180 minutes. In addition, the coating composition was placed in a hot box at 120°F (48.8°C) for one week and the initial viscosity was measured, followed by the viscosity after 180 minutes. The results are shown in Table 3A.
[0121] Table 3A. Pot life measurements after hot box
[0122]
[0123] For the coating compositions described herein, the effect of water on pot life was also evaluated. A sample of the finished paint of Example 1 (Part A) was mixed with the 0.9 index catalyst of Example 1 (Part B) at 10:1 by weight to prepare a coating composition. Half was used as a control, while the other half was mixed with a 1:1 solution of 2 wt % water and acetone. The initial viscosity was measured using a #3 marked Zahn cup and is expressed as the effluent time (in minutes), with additional viscosity measurements made at specific time points thereafter. The results are shown in Table 3B.
[0124] Table 3B. Pot life measurements using water
[0125] sample Initial viscosity Viscosity: 60min Viscosity: 120min Viscosity: 180min Comparison 14.62 17.57 24.60 33.97 1% Water 13.72 14.72 17.40 19.40
[0126] Example 5: Performance Characteristics (Cure Response and Corrosion Resistance)
[0127] To determine the performance of the coatings described herein, primer compositions A, B, C, and D were prepared, which contained a resin component that can be crosslinked by Michael addition. Compositions A, B, and C were prepared using a 0.9 index catalyst at the levels shown in Table 4. Composition D was a control prepared using a commercially available latent base catalyst (ACURE 500, Allnex) at the levels shown in Table 4.
[0128] Each composition was sprayed onto a metal test panel at a dry film thickness of approximately 2.0 mils (50 μm). Each panel was then cured at 150F (65.5°C) for 10 minutes. The curing response of each sample was evaluated using the Konig pendulum hardness test (3-4 replicates for each composition).
[0129] To determine the corrosion resistance of the coating compositions, samples A, B, C, and D were sprayed onto phosphate treated cold rolled steel test panels (ACT B1000 P99X) at a dry film thickness of about 1.5 to 2.0 mils (38 μ to 50 μ) and force cured at 150F (65.5°C) for 30 minutes. The panels were then placed in a salt spray cabinet for 500 hours as described in ASTM B117. Corrosion resistance was evaluated by evaluating blistering, rusting, and scratch creep for each sample. The results are shown in Table 4.
[0130] Table 4. Properties of coating compositions
[0131]
[0132] Comparison of the cure performance and salt spray results for the composition of the invention (Sample B) and the control composition (Sample D) showed similar performance.
[0133] The complete disclosures of all patents, patent applications and publications cited herein and electronically available materials are incorporated by reference. The aforementioned detailed description and examples are given only for the purpose of clear understanding. It should be understood that there are no unnecessary restrictions. The present invention is not limited to the exact details shown and described, and changes obvious to those skilled in the art will be included in the present invention defined by the claims. In some embodiments, in the absence of any element not specifically disclosed herein, the illustrative disclosed invention of this paper can be appropriately practiced.
Claims
1. A method for preparing a latent catalyst, the method comprising: providing a hydroxide functional component; Providing a multifunctional component capable of reacting with the hydroxide functional component: The hydroxide functional component is reacted with the component capable of reacting with the hydroxide functional component to prepare a substituted carbamate latent catalyst having the structure of formula (I): in: Each X + independently a non-acidic cation; Each R1 is independently H, C1 to C10 alkyl, aryl, aralkyl, or C1 to C10 substituted alkyl, aryl, aralkyl, or a mixture or combination thereof; Each R2 and R3 is independently C1 to C10 alkyl, aryl, aralkyl, or C1 to C10 substituted alkyl, aryl, aralkyl, or a mixture or combination thereof; and n is greater than 1.
2. The method according to claim 1, wherein X + Selected from alkali metal ions, alkaline earth metal ions, ammonium ions, phosphonium ions, or combinations thereof.
3. The method according to claim 1, wherein X + It is a quaternary ammonium cation or a phosphonium ion.
4. The method according to claim 1, wherein X + is a quaternary ammonium cation having the general formula NR'4, Wherein R' is H, unsubstituted C1-C10 alkyl, substituted C1-C10 alkyl, aryl, aralkyl, or a mixture or combination thereof.
5. The method according to claim 1, wherein X + is a quaternary ammonium cation having the general formula NR'4, wherein R' is a C1-C4 unsubstituted alkyl group.
6. The process according to any one of the preceding claims 1 to 5, wherein the latent catalyst is present in an amount of 0.1 meq to 1.0 meq.
7. The process according to any one of the preceding claims 1 to 5, wherein the latent catalyst is present in an amount of 0.01 meq to 0.5 meq.
8. The method of claim 1, wherein the hydroxide functional compound is selected from C1-C10 alkylammonium hydroxides, arylammonium hydroxides, aralkylammonium hydroxides, or combinations thereof.
9. The method of claim 1, wherein the hydroxide functional component is a C1-C10 alkylammonium hydroxide.
10. The method according to claim 9, wherein the C1-C10 alkylammonium hydroxide is tetrabutylammonium hydroxide.
11. The method of claim 1 wherein the component capable of reacting with the hydroxide functional component is a polyfunctional isocyanate.
12. The method according to claim 11, wherein the polyfunctional isocyanate is selected from 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 4,4'-methylene diphenyl diisocyanate, hexamethylene diisocyanate, polymethylene-polyphenyl isocyanate, homopolymers thereof, cyclic trimers thereof, cocyclic trimers thereof, and mixtures thereof.
13. The method of claim 12, wherein the polyfunctional isocyanate is a hexamethylene diisocyanate trimer, a hexamethylene diisocyanate homopolymer, or a combination thereof.
14. The method of claim 12, wherein any polyfunctional isocyanate that does not react with the hydroxide functional component is reacted with excess solvent in the solution.
15. The method according to any one of the preceding claims 1 to 5, optionally comprising a pot life or open time extending component, the pot life or open time extending component comprising: one or more compounds containing an acidic X'-H group, wherein X' is N, P, O, S or C, and wherein the pKa of X'H is at least one unit less than the Michael addition donor component present in the composition.
16. The method according to any one of the preceding claims 1 to 5, wherein: The substituted carbamate latent catalyst is prepared by the reaction of tetrabutylammonium hydroxide (TBAH) and hexamethylene diisocyanate and has a structure shown in formula (II):
17. A cured coating, comprising: A polymer coating composition comprising a cross-linkable resin component; and Latent catalyst, the latent catalyst is prepared according to the method of claim 1 in, After being applied to the substrate, the polymer coating composition is cured at 150°F in 1 minute to 10 minutes to form the cured coating, and The cured coating exhibits the best curing properties.
18. The cured coating of claim 17, wherein the substrate is selected from pretreated metal, wood, polymeric material, ceramic material, glass, or combinations thereof.