Laser welding method for chrome-plated stainless steel parts
By using a three-channel protective gas path to protect the welding area during laser welding of chrome-plated parts, the problem of weld blackening was solved, and the wear resistance and corrosion resistance of the welded joint were improved, ensuring welding quality and product life.
Patent Information
- Application Number
- CN202111502577.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-09
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-12-09
AI Technical Summary
In laser welding of chrome-plated parts, the weld and surrounding area are prone to burn-out, resulting in blackening, which affects the appearance and corrosion resistance, and reduces the service life of high-end bathroom products.
The welding process is protected by a three-way protective gas path, including a first protective gas path coaxial with the laser beam, and second and third protective gas paths located on both sides. A mixture of Ar and O2 gas is introduced, and the gas path angle and flow rate are adjusted to prevent the weld from oxidizing and blackening.
Achieving a smooth and clean weld joint improves the wear and corrosion resistance of the weld, prevents weld blackening, and enhances the product's appearance and service life.
Smart Images

Figure CN114260567B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of laser welding, in particular to a laser welding method for stainless steel chrome-plated parts. Background Art
[0002] 304 stainless steel is a kind of chromium-nickel stainless steel with a wide range of applications. Its tensile strength at room temperature is greater than 515MPa. This kind of stainless steel has good corrosion resistance, heat resistance, low-temperature strength and mechanical properties. It is widely used in heat exchangers, bellows, auto parts, household bathroom products, etc. Although 304 stainless steel products have good corrosion resistance, their hardness is relatively low, ≤210HV at room temperature. Therefore, the surface of metal products will still corrode after long-term use in a humid environment, and there will also be varying degrees of wear. In the field of high-end bathrooms, in order to improve the service life and surface brightness of metal products, chrome plating is usually used as a surface treatment method to improve the corrosion resistance and wear resistance of the 304 stainless steel metal surface and extend the service life of the product. The structure of bathroom products is mainly composed of thin-walled round tubes, and laser welding is often used in production to connect the structural parts.
[0003] Laser welding has the characteristics of concentrated energy density, narrow heat-affected zone, and beautiful weld formation, and is widely used in the manufacturing field of stainless steel products. In the conventional welding of 304 stainless steel products, laser welding shows excellent welding processability and welding performance. The surface of the welded joint is smooth, without obvious defects, and has excellent mechanical properties. However, in the welding of chrome-plated parts, the heat input of the weld and its heat-affected zone is high, which causes serious burnout of the chrome plating layer in the weld and the surrounding area of the weld (>500℃), and blackening of the weld and the weld toe, which greatly affects the aesthetics of high-end bathroom products. At the same time, the blackened area is also prone to corrosion, which reduces the service life of high-end bathroom products. Weld blackening has become a key constraint on the application of stainless steel chrome-plated parts in high-end bathroom products.
[0004] Therefore, in view of the above technical problems, it is necessary to provide a laser welding method for stainless steel chrome-plated parts. Summary of the invention
[0005] The object of the present invention is to provide a laser welding method for stainless steel chrome-plated parts, which can prevent the occurrence of weld blackening phenomenon and improve the wear resistance and corrosion resistance of the welded joint.
[0006] To achieve the above purpose, the technical solution provided by the present invention is as follows:
[0007] A laser welding method for stainless steel chrome-plated parts, comprising the following steps:
[0008] S1: Pre-treat the area to be welded of the stainless steel chrome-plated parts;
[0009] S2: Connect the protective gas circuit and perform laser welding on the area to be welded along the welding direction;
[0010] S3: After laser welding is completed, the protective gas circuit is closed;
[0011] Among them, the protective gas circuit includes a first protective gas circuit, a second protective gas circuit and a third protective gas circuit facing the area to be welded, the first protective gas circuit is coaxial with the laser beam used for welding, and the second protective gas circuit and the third protective gas circuit are respectively located on both sides of the first protective gas circuit along the welding direction and form a preset angle with the first protective gas circuit.
[0012] In one or more embodiments, the laser power during laser welding in step S2 is 0.2-0.4 kW, the defocus is 0-2 mm, and the welding speed is 0.18-0.3 m / min.
[0013] In one or more embodiments, in step S2, the shielding gas circuit is connected 2 to 4 seconds before laser welding.
[0014] In one or more embodiments, in step S3, the shielding gas circuit is closed with a delay of 2 to 4 seconds after the laser welding is completed.
[0015] In one or more embodiments, the protective gas introduced into the protective gas circuit is a mixed gas of Ar and O2, wherein the volume fraction of O2 is 1-2%.
[0016] In one or more embodiments, the flow rate of the protective gas introduced into the protective gas circuit is 15 to 30 L / min.
[0017] In one or more embodiments, the angle between the second shielding gas path and the first shielding gas path is 20-40°, and the angle between the third shielding gas path and the first shielding gas path is 20-40°.
[0018] In one or more embodiments, the pretreatment in step S1 includes: cleaning the area to be welded with alcohol or acetone.
[0019] In one or more embodiments, the chrome-plated stainless steel part is a 304 chrome-plated stainless steel pipe.
[0020] Compared with the prior art, the laser welding method for stainless steel chrome-plated parts provided by the present invention adds a second protective gas path and a third protective gas path on both sides of the laser welding head on the basis of the original first protective gas path being coaxial with the laser, so as to realize the protection of the weld and the high-temperature area around it, and realizes the protection of the weld joint under different laser power and welding speed conditions by adjusting the relative positions of the laser welding head, the second protective gas path and the third protective gas path and the flow rate of the protective gas, so as to prevent the weld from blackening and improve the wear resistance and corrosion resistance of the weld joint. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 is a schematic diagram of a laser welding method for a stainless steel chrome-plated part in one embodiment of the present invention;
[0022] Figure 2 This is a picture of the weld surface morphology formed by the existing conventional laser welding method;
[0023] Figure 3 This is a picture of the weld surface morphology obtained in Example 1 of the present invention. DETAILED DESCRIPTION
[0024] The specific implementation modes of the present invention are described in detail below in conjunction with the accompanying drawings, but it should be understood that the protection scope of the present invention is not limited by the specific implementation modes.
[0025] Unless explicitly stated otherwise, throughout the specification and claims, the term “comprise” or variations such as “include” or “comprising”, etc., will be understood to include the stated elements or components but not to exclude other elements or components.
[0026] A laser welding method for a chrome-plated stainless steel part provided in one embodiment of the present invention comprises the following steps:
[0027] S1: Pre-treat the area to be welded of the stainless steel chrome-plated parts;
[0028] S2: Connect the protective gas circuit and perform laser welding on the area to be welded along the welding direction;
[0029] S3: After laser welding is completed, the protective gas circuit is closed.
[0030] Among them, the protective gas circuit includes a first protective gas circuit, a second protective gas circuit and a third protective gas circuit with the gas outlet facing the area to be welded, the first protective gas circuit is coaxial with the laser beam used for welding, and the second protective gas circuit and the third protective gas circuit are respectively located on both sides of the first protective gas circuit along the welding direction and form a preset angle with the first protective gas circuit.
[0031] The laser welding method for stainless steel chrome-plated parts provided in this embodiment, during welding, by adding a second protective gas path and a third protective gas path on both sides of the laser beam used for welding, the protective gas blown out of the second protective gas path and the third protective gas path can cover the front and rear sides of the area to be welded that the laser head is aimed at in the welding direction, and can effectively prevent the weld from being oxidized and blackened during welding, without the need to apply an anti-oxidation coating on the surface of the area to be welded before and after welding, so as to obtain a welding joint with bright and neat surface quality and excellent wear resistance and corrosion resistance.
[0032] In an exemplary embodiment, the laser power used in laser welding in step S2 is 0.2-0.4 kW, the defocus is 0-2 mm, and the welding speed is 0.18-0.3 m / min. With the above welding process parameters, there will be no phenomenon of too full or lack of flowing molten metal, thereby further ensuring the smoothness and flatness of the weld, which is conducive to increasing the uniformity of the weld and enhancing the welding strength.
[0033] In an exemplary embodiment, in step S2, the shielding gas circuit is connected 2 to 4 seconds in advance before laser welding. By connecting the shielding gas circuit in advance, the air in the area to be welded can be removed before welding to avoid oxidation and blackening during welding.
[0034] In an exemplary embodiment, in step S3, the shielding gas circuit is closed for 2 to 4 seconds after the laser welding is completed. The delayed closing of the shielding gas circuit can play a protective role when the welding point still has a high temperature after the welding is completed, and avoid oxidation and blackening caused by contact with air.
[0035] In an exemplary embodiment, the protective gas introduced into the protective gas circuit is a mixed gas of Ar and O2, wherein the volume fraction of O2 is 1-2%. Argon is easy to prepare, low in cost, has stable chemical properties, is not easy to react with other substances, and can play a better protective role. Other protective gases can also be introduced into the protective gas circuit, such as a mixed gas of other inert gases and O2.
[0036] In an exemplary embodiment, the flow rate of the protective gas introduced into the protective gas circuit is 15 to 30 L / min.
[0037] In an exemplary embodiment, the angle between the second protective gas circuit and the first protective gas circuit is 20-40°, for example, it can be 20°, 22.6°, 30°, 40°, etc. The angle between the third protective gas circuit and the first protective gas circuit is 20-40°, for example, it can be 20°, 22.6°, 30°, 40°, etc. The angle between the second protective gas circuit and the third protective gas circuit and the first protective gas circuit, and the spacing between the second protective gas circuit and the third protective gas circuit and the first protective gas circuit outlet can be adjusted according to actual needs, as long as it can ensure that the protective gas blown out of the entire protective gas circuit can cover the corresponding laser head corresponding to the area to be welded, that is, the front and back sides of the area.
[0038] In an exemplary embodiment, the pretreatment in step S1 includes: cleaning and wiping the area to be welded with alcohol or acetone to ensure that the area to be welded is clean and free of oil stains, thereby reducing the generation of welding pores.
[0039] In an exemplary embodiment, the chrome-plated stainless steel part is a 304 chrome-plated stainless steel pipe.
[0040] Figure 1 Schematic diagram of a laser welding method for chrome-plated stainless steel parts in one embodiment of the present invention, wherein 1 is a first protective gas circuit, 2 is a second protective gas circuit, 3 is a third protective gas circuit, 4 is a laser beam, 5 is a welding specimen, 6 is a workbench, 7 is a protective gas, α is an angle between the third protective gas circuit and the first protective gas circuit, and β is an angle between the third protective gas circuit and the first protective gas circuit.
[0041] The present invention will be further described below in conjunction with specific embodiments.
[0042] Example 1
[0043] A 304 stainless steel chrome-plated pipe fitting with a wall thickness of 1 mm, a coating thickness of 4 to 6 μm, a diameter of 10 mm, and a pipe length of 600 mm was prepared as a welding test piece.
[0044] The welding area of the welding specimen is cleaned with alcohol or acetone until the welding area is bright and free of obvious dust. After cleaning, the welding specimen is clamped on the workbench by a fixture.
[0045] The protective gas line is connected, and the protective gas is a mixed gas of Ar and O2, in which the volume fraction of O2 is about 1-2%, and the protective gas flow rate is 20L / min.
[0046] The laser head was made perpendicular to the surface of the welding area of the welding specimen for laser welding. The ambient temperature was 25°C, gas was supplied 3s in advance, and the laser head was kept stationary at the starting position for 3s. Welding parameters: laser power was 0.4kW, welding speed was 4mm / s, defocus was 2mm, the first shielding gas path was coaxial with the laser beam, and the angle between the second and third shielding gas paths and the first shielding gas path was 30°.
[0047] After welding is completed, keep the laser head still at the end position for 3 seconds, and close the protective gas circuit after a delay of 3 seconds.
[0048] The laser welding welds obtained by the above welding process method were visually inspected and X-rayed. The weld surface was smooth and tidy, with good brightness, no surface and internal cracks, no undercut and other defects, and met the performance requirements. Figure 3 This is a picture of the weld surface morphology obtained in Example 1 of the present invention.
[0049] Example 2
[0050] Two 304 stainless steel chrome-plated pipes with a wall thickness of 1 mm, a coating thickness of 4 to 6 μm, a diameter of 10 mm, and a tube length of 600 mm were prepared as welding specimens; a 10 mm hole was processed in the geometric center of one of the pipes, and the two pipes were T-welded.
[0051] Welding is performed at the joint of two pipes. The weld shape is saddle-shaped. The area to be welded is cleaned with alcohol or acetone until the area to be welded is bright and free of obvious dust. After cleaning, the welding specimen is limited on the welding positioner by a fixture.
[0052] The protective gas line is connected, and the protective gas is a mixed gas of Ar and O2, in which the volume fraction of O2 is about 1-2%, and the protective gas flow rate is 20L / min.
[0053] The laser head was made perpendicular to the surface of the welding area of the welding specimen for laser welding. The ambient temperature was 25°C, gas was supplied 3s in advance, and the laser head was kept stationary at the starting position for 3s. Welding parameters: laser power was 0.4kW, welding speed was 4mm / s, defocus was 2mm, the first shielding gas path was coaxial with the laser beam, and the angle between the second and third shielding gas paths and the first shielding gas path was 30°.
[0054] After welding is completed, keep the laser head still at the end position for 3 seconds, and close the protective gas circuit after a delay of 3 seconds.
[0055] The laser welding welds obtained by the above welding process method were visually inspected and X-rayed. The weld surface was smooth and tidy, with good brightness, no surface and internal cracks, no undercut and other defects, and met the performance requirements.
[0056] Example 3
[0057] Two 304 stainless steel chrome-plated test plates with a size of 150*300*1mm were prepared as welding specimens; the assembly gap of the specimens was 0mm.
[0058] The welding area of the welding specimen is cleaned with alcohol or acetone until the welding area is bright and free of obvious dust. After the cleaning is completed, the welding specimen is confined on a workbench with a back-shielding gas device by a clamp.
[0059] The protective gas line is connected, and the protective gas is a mixed gas of Ar and O2, in which the volume fraction of O2 is about 1-2%, and the protective gas flow rate is 20L / min.
[0060] The laser head was made perpendicular to the surface of the welding area of the welding specimen for laser welding. The ambient temperature was 25°C, gas was supplied 3s in advance, and the laser head was kept stationary at the starting position for 3s. Welding parameters: laser power was 0.4kW, welding speed was 8mm / s, defocus was 2mm, the first protective gas path was coaxial with the laser beam, and the angle between the second and third protective gas paths and the first protective gas path was 30°.
[0061] After welding is completed, keep the laser head still at the end position for 3 seconds, and close the protective gas circuit after a delay of 3 seconds.
[0062] The laser welding welds obtained by the above welding process method were visually inspected and X-rayed. The weld surface was smooth and tidy, with good brightness, no surface and internal cracks, no undercut and other defects, and met the performance requirements.
[0063] In summary, the present invention adds a second protective gas path and a third protective gas path on both sides of the laser welding head on the basis of the original first protective gas path being coaxial with the laser, so as to realize the protection of the weld and the high-temperature area around it, and realizes the protection of the weld joint under different laser power and welding speed conditions by adjusting the relative positions of the laser welding head, the second protective gas path and the third protective gas path and the flow rate of the protective gas, thereby preventing the weld from blackening and improving the wear resistance and corrosion resistance of the weld joint.
[0064] The laser welding method for stainless steel chrome-plated parts provided by the present invention can replace the existing method of applying an anti-oxidation layer on the surface of the chrome-plated parts, save research and development and production costs, reduce the pollution of the anti-oxidation layer to the environment, and obtain a laser welded joint with a smooth and beautiful weld surface and excellent wear resistance and corrosion resistance; and the method has the advantages of simple operation, excellent welding process performance, high production efficiency, etc., and is easy to promote and apply the industrialization of high-quality welding of stainless steel chrome-plated parts.
[0065] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the exact form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.
Claims
1. A laser welding method for chrome-plated stainless steel parts, characterized in that: The following steps are involved: S1: Pre-treat the area to be welded of the stainless steel chrome-plated parts; S2: Connect the protective gas circuit and perform laser welding on the area to be welded along the welding direction; S3: After laser welding is completed, the protective gas circuit is closed; Among them, the protective gas circuit includes a first protective gas circuit, a second protective gas circuit and a third protective gas circuit facing the area to be welded, the first protective gas circuit is coaxial with the laser beam used for welding, the second protective gas circuit and the third protective gas circuit are respectively located on both sides of the first protective gas circuit along the welding direction and form a preset angle with the first protective gas circuit, and the protective gas blown out of the protective gas circuit can cover the area to be welded to which the laser head is aligned and the front and back sides of the area to be welded.
2. The laser welding method for chrome-plated stainless steel parts according to claim 1, characterized in that: The laser power during laser welding in step S2 is 0.2-0.4 kW, the defocusing amount is 0-2 mm, and the welding speed is 0.18-0.3 m / min.
3. The laser welding method for chrome-plated stainless steel parts according to claim 1, characterized in that: In the step S2, the shielding gas circuit is connected 2 to 4 seconds before laser welding.
4. The laser welding method for chrome-plated stainless steel parts according to claim 3, characterized in that: In the step S3, the protective gas circuit is closed after the laser welding is completed for 2 to 4 seconds.
5. The laser welding method for chrome-plated stainless steel parts according to claim 4, characterized in that: The protective gas introduced into the protective gas path is a mixed gas of Ar and O2, wherein the volume fraction of O2 is 1-2%.
6. The laser welding method for chrome-plated stainless steel parts according to claim 5, characterized in that: The flow rate of the protective gas introduced into the protective gas circuit is 15 to 30 L / min.
7. The laser welding method for chrome-plated stainless steel parts according to claim 1, characterized in that: The included angle between the second protection gas path and the first protection gas path is 20-40°, and the included angle between the third protection gas path and the first protection gas path is 20-40°.
8. The laser welding method for chrome-plated stainless steel parts according to claim 1, characterized in that: The pretreatment in step S1 includes: cleaning the area to be welded with alcohol or acetone.
9. The laser welding method for chrome-plated stainless steel parts according to any one of claims 1 to 8, characterized in that: The stainless steel chrome-plated parts are 304 stainless steel chrome-plated pipe fittings.