A passivation process for planar thyristor chip
Through processes such as initial oxidation, selective photolithography, boron diffusion and laser removal, instead of the traditional multi-layer composite oxide film passivation method, the uniformity and cost problems of the semi-insulating oxygen-doped polysilicon film on the planar silicon controlled chip are solved. Achieved higher production efficiency and product reliability.
Patent Information
- Application Number
- CN202111581333.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-22
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-12-22
AI Technical Summary
In the passivation process of traditional planar thyristor chips, the semi-insulating oxygen-doped polysilicon film has uniformity problems during the deposition and removal processes, which leads to increased production costs and cycles, and may damage the wafer surface and affect electrical consistency.
The process of initial oxidation, selective photolithography, boron diffusion, laser removal of oxide film in the electrophoretic area, mixed acid rinsing and electrophoretic deposition of glass powder is used to replace the traditional multi-layer composite oxide film passivation method, simplify the production process and improve product reliability.
It simplifies the production process, reduces production costs, improves product reliability and electrical consistency, and avoids surface damage to the wafer.
Smart Images

Figure CN114267601B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of chip processing, and in particular to a passivation process for a planar thyristor chip. Background Art
[0002] In order to improve the product's withstand voltage and reliability, the passivation layer of traditional planar thyristor chips usually uses semi-insulating oxygen-doped polysilicon, silicon dioxide, phosphorus silicon glass and other materials for terminal passivation, such as Fig.14 The conventional multi-layer silicon oxide passivation structure formed as shown in the figure has the following problems: First, it is necessary to remove the multi-layer passivation film on the metal electrode surface by adding a photolithography process, which increases the production cost and production cycle; second, when the semi-insulating oxygen-doped polysilicon film is deposited, due to its process characteristics, the film thickness is difficult to grow uniformly. When it is removed, the silicon on the surface of the wafer will be damaged due to over-corrosion in some areas, which will destroy the uniformity of the product surface concentration and affect the electrical consistency of the trigger characteristics. Summary of the invention
[0003] In view of the above problems, the present invention provides a passivation process for a planar thyristor chip which is convenient to process, saves time and improves product reliability.
[0004] The technical solution of the present invention is: comprising the following steps:
[0005] (1) Select an N-type silicon substrate wafer;
[0006] (2) Initial oxidation: growing a dense oxide film on the surface of the wafer;
[0007] (3) Selective photolithography and oxide film removal of the P+ isolation area: expose the oxide films of the front and back P+ isolation layers, and protect other areas with photoresist; use BOE to remove the oxide film to expose the P+ isolation area to be diffused;
[0008] (4) Boron pre-deposition in P+ isolation area: use a boron source for diffusion;
[0009] (5) P+ isolation region penetration diffusion: The boron junction is pushed forward in a high-temperature diffusion furnace to make the upper and lower isolation layer junctions deeply connected;
[0010] (6) Removal of back oxide film: Use BOE to completely remove the oxide film on the back of the wafer;
[0011] (7) Back P+ region diffusion: Use a boron source for diffusion and deposit the boron source on the surface of the isolation area;
[0012] (8) Front P+ base region and voltage divider ring lithography: Selective lithography is performed on the front surface of the wafer;
[0013] (9) BOE etching: Use BOE etching to remove the oxide film on the surface of the front P+ base region and the voltage divider ring;
[0014] (10) P+ base region and partial pressure ring boron diffusion: use boron source for diffusion;
[0015] (11) Emission area and cut-off ring lithography: Selective lithography is performed on the front surface of the wafer;
[0016] (12) Diffusion of emitter region and cutoff ring: use POCL3 for diffusion;
[0017] (13) Laser removal of oxide film in electrophoretic area: According to the preset pattern setting, the silicon dioxide area to be removed is burned with laser to expose the silicon on the surface of the electrophoretic area;
[0018] (14) Mixed acid rinsing: Use mixed acid to treat the surface silicon of the electrophoresis area;
[0019] (15) Electrophoresis: A layer of glass powder is deposited on the silicon surface by electrophoresis.
[0020] (16) Glass melting: melting glass powder in a high temperature furnace;
[0021] (17) Removal of back oxide film;
[0022] (18) Metal evaporation;
[0023] (19) Electrode surface lithography: Selective lithography to form the gate and cathode on the front side; (20) Metal etching: Use aluminum etching solution to remove the metal from the chip to complete.
[0024] In step (2), the thickness of the oxide film is 15000-30000 angstroms.
[0025] In step (5), the temperature of the high temperature diffusion furnace is 1260-1280°C.
[0026] In step (14), the temperature of the mixed acid is -6°C to 6°C.
[0027] In step (14), the mixed acid is a mixed aqueous solution containing hydrofluoric acid, nitric acid and glacial acetic acid.
[0028] In step (14), the surface is treated to form micro-corrosion of 3-5 um.
[0029] In step (16), the glass melting temperature is 640-830°C and the time is 15-20 minutes.
[0030] In the working process of the present invention, after the diffusion of the emission area is completed and before the metal layer evaporates, the surface oxide film of the area to be electrophoresed is removed by laser etching method in sequence; the laser etching area is micro-rinsed with mixed acid to remove the surface damage layer; and a layer of glass is grown on the terminal junction by electrophoresis process. In this way, not only the production process is simplified and the production cost is reduced, but also the reliability of the product is improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 is a schematic diagram of the structure in step (2) of the present invention,
[0032] Figure 2 is a schematic diagram of the structure in step (3) of the present invention,
[0033] Figure 3 is a schematic diagram of the structure in step (5) of the present invention,
[0034] Figure 4 is a schematic diagram of the structure in step (7) of the present invention,
[0035] Figure 5 is a schematic diagram of the structure in step (8) of the present invention,
[0036] Figure 6 is a schematic diagram of the structure in step (10) of the present invention,
[0037] Figure 7 is a schematic diagram of the structure in step (11) of the present invention,
[0038] Figure 8 is a schematic diagram of the structure in step (12) of the present invention,
[0039] Fig. 9 is a schematic diagram of the structure in step (13) of the present invention,
[0040] Fig.10 is a schematic diagram of the structure in step (14) of the present invention,
[0041] Fig.11 is a schematic diagram of the structure in steps (15) and (16) of the present invention,
[0042] Fig.12 is a schematic diagram of the structure in step (17) of the present invention,
[0043] Fig.13 is a schematic diagram of the structure in step (20) of the present invention,
[0044] Fig.14 It is a structural schematic diagram of the prior art. DETAILED DESCRIPTION
[0045] The present invention Figure 1-13 , including the following steps:
[0046] (1) Select N-type silicon substrate wafers and choose different resistivities according to the withstand voltage requirements of different products; the thickness is selected according to the different wafer sizes;
[0047] (2) Initial oxidation: A dense oxide film with a thickness of 15,000-30,000 angstroms is grown on the surface of the wafer. Figure 1 .
[0048] (3) Selective photolithography + oxide film removal of P+ isolation area: expose the oxide film of the P+ isolation layer on the front and back sides, protect other areas with photoresist, use BOE to remove the oxide film, and expose the P+ isolation area to be diffused, such as Figure 2 In this way, preparation is made for subsequent penetration diffusion.
[0049] (4) Boron pre-deposition in the P+ isolation area: Use a boron source for diffusion and deposit a certain concentration of boron source on the surface of the isolation area.
[0050] (5) P+ isolation region penetration diffusion: The boron junction is pushed forward in a high-temperature diffusion furnace at 1260-1280℃ to make the upper and lower isolation layer junctions deeply connected, such as Figure 3 .
[0051] (6) Removal of back oxide film: Use BOE to completely remove the oxide film on the back of the wafer.
[0052] (7) Back P+ region diffusion: Use a boron source for diffusion and deposit a certain concentration of boron source on the surface of the isolation area, such as Figure 4 ;
[0053] (8) Front P+ base region and voltage divider ring lithography: Selective lithography is performed on the front surface of the wafer, such as Figure 5 ;
[0054] (9) BOE etching: BOE etching is also used to remove the oxide film on the surface of the front P+ base region and the voltage divider ring;
[0055] (10) P+ base region and voltage divider ring boron diffusion: Use a boron source for diffusion. Select the diffusion temperature and time according to the product voltage level and junction depth, such as Figure 6 ;
[0056] (11) Emission region and cut-off ring lithography: Selective lithography is performed on the front surface of the wafer, such as Figure 7 ;
[0057] (12) Diffusion of emitter region and cut-off ring: Use POCL3 for diffusion. Select the diffusion temperature and time according to the different junction depths of the product, such as Figure 8 ;
[0058] The present invention uses the glass passivation method in steps (13) to (16) to replace the traditional process passivation methods such as multi-layer composite oxide film, which not only simplifies the production process and reduces production costs, but also improves product reliability. The specific steps are as follows:
[0059] (13) Laser removal of oxide film in electrophoretic area: According to the preset pattern setting, the silicon dioxide area to be removed is laser-burned to expose the silicon on the surface of the electrophoretic area. This step uses laser burning to remove the oxide film instead of the traditional selective photolithography to pattern the wafer + BOE etching method, saving production time and cost. Fig. 9 ;
[0060] (14) Mixed acid rinsing: Use a mixed acid (a mixed aqueous solution containing hydrofluoric acid, nitric acid, glacial acetic acid, etc.) at a certain temperature (-6℃-6℃) and proportion to treat the surface silicon of the electrophoresis area, remove the surface micro-damage layer, and micro-corrode 3-5um, such as Fig.10 ;
[0061] (15) Electrophoresis: A layer of glass powder is deposited on the silicon surface by electrophoresis. Fig.11 ; Glass powder is covered on the surface of the silicon wafer through electrophoresis to prepare for the subsequent glass melting.
[0062] (16) Glass melting: Melt the glass powder in a high temperature furnace at a temperature of 640-830°C for 15-20 minutes. Fig.11 ;
[0063] (17) Removal of back oxide film, such as Fig.12 :
[0064] (18) Metal evaporation: AL on the front, Ag on the back;
[0065] (19) Electrode surface photolithography: selective photolithography to form the gate and cathode on the front side; (20) Metal etching: use aluminum etching solution to remove metal from the chip, such as Fig.13 .
[0066] After the diffusion of the emission area is completed and before the metal layer evaporates, the present invention ① uses a laser etching method to remove the surface oxide film of the area to be electrophoresed; ② uses a mixed acid to micro-rinse the laser etching area to remove the surface damage layer; ③ grows a layer of glass on the terminal junction by electrophoresis, and the glass covers the following areas: a. Part of the front edge isolation area (P+), the cutoff ring, the voltage divider ring and the connecting area of the edge position of the P+ short base area, and b. The passivation process at the connection between the N+ cathode edge area and the gate edge area.
[0067] Regarding the contents disclosed in this case, there are a few points that need to be explained:
[0068] (1) The drawings of the embodiments disclosed in this case only involve the structures involved in the embodiments disclosed in this case. Other structures can refer to the general design;
[0069] (2) In the absence of conflict, the embodiments and features of the embodiments disclosed in this case may be combined with each other to obtain new embodiments;
[0070] The above are only specific implementation methods disclosed in this case, but the protection scope of the present disclosure is not limited thereto. The protection scope disclosed in this case should be based on the protection scope of the claims.
Claims
1. A passivation process for a planar thyristor chip, characterized in that: The following steps are involved: (1) Select an N-type silicon substrate wafer; (2) Initial oxidation: growing a dense oxide film on the surface of the wafer; (3) Selective photolithography and oxide film removal of the P+ isolation area: expose the oxide films of the P+ isolation layer on the front and back sides, and protect other areas with photoresist; Use BOE to remove the oxide film to expose the P+ isolation area to be diffused; (4) Boron pre-deposition in P+ isolation area: use a boron source for diffusion; (5) P+ isolation region penetration diffusion: The boron junction is pushed forward in a high-temperature diffusion furnace to make the upper and lower isolation layer junctions deeply connected; (6) Removal of back oxide film: Use BOE to completely remove the oxide film on the back of the wafer; (7) Back P+ region diffusion: Use a boron source for diffusion and deposit the boron source on the surface of the isolation area; (8) Front P+ base region and voltage divider ring lithography: Selective lithography is performed on the front surface of the wafer; (9) BOE etching: Use BOE etching to remove the oxide film on the surface of the front P+ base region and the voltage divider ring; (10) P+ base region and partial pressure ring boron diffusion: use boron source for diffusion; (11) Emission area and cut-off ring lithography: Selective lithography is performed on the front surface of the wafer; (12) Diffusion of emitter region and cutoff ring: use POCL3 for diffusion; (13) Laser removal of oxide film in electrophoretic area: According to the preset pattern setting, the silicon dioxide area to be removed is burned with laser to expose the silicon on the surface of the electrophoretic area; (14) Mixed acid rinsing: Use mixed acid to treat the surface silicon of the electrophoresis area; (15) Electrophoresis: A layer of glass powder is deposited on the silicon surface by electrophoresis. (16) Glass melting: melting glass powder in a high temperature furnace; (17) Removal of back oxide film; (18) Metal evaporation; (19) Electrode surface lithography: Selective lithography to form the gate and cathode on the front side; (20) Metal etching: Use aluminum etching solution to remove metal from the wafer; In step (14), the temperature of the mixed acid is -6°C to 6°C; In step (14), the surface is treated to form micro-corrosion of 3-5 um; In step (16), the glass melting temperature is 640-830°C and the time is 15-20 minutes.
2. A passivation process for a planar thyristor chip according to claim 1, characterized in that: In step (2), the thickness of the oxide film is 15000-30000 angstroms.
3. The passivation process of a planar thyristor chip according to claim 1, characterized in that: In step (5), the temperature of the high temperature diffusion furnace is 1260-1280°C.
4. The passivation process of a planar thyristor chip according to claim 1, characterized in that: In step (14), the mixed acid is a mixed aqueous solution containing hydrofluoric acid, nitric acid and glacial acetic acid.