A heating cable for medium-pressure oil pipeline and its preparation process
By using high-strength aluminum alloy conductors, metal shielding layers and cross-linked polyethylene insulation layers, as well as the design of flame-retardant polyethylene outer sheaths, the problem of existing heating cables being unable to provide sufficient heat sources is solved, achieving high-voltage heating under high-voltage conditions. High-temperature heat source supply and safety and reliability of oil pipeline transportation.
Patent Information
- Application Number
- CN202111561147.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-20
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-12-20
AI Technical Summary
Existing heating cables cannot provide sufficient heat sources under high-temperature oil pipeline conditions, resulting in increased viscosity and potential safety hazards.
The cable conductor is made of 6201 aluminum-magnesium-silicon high-strength aluminum alloy, with a metal shielding layer and a cross-linked polyethylene insulation layer, plus a flame-retardant polyethylene outer sheath to ensure that high-temperature heat sources are provided under high-pressure conditions, and through a specific material ratio Improve insulation and thermal conductivity properties.
It provides a high-temperature heat source under high-pressure conditions to ensure the smooth transportation of oil, improves the voltage resistance and safety of the cable, reduces the influence of external electromagnetic interference and short-circuit current, and has a simple structure, light weight and easy installation.
Smart Images

Figure CN114286463B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of high-voltage power cables, and in particular to a heating cable for a medium-pressure oil pipeline and a preparation process thereof. Background Art
[0002] The pipeline system currently used to transport oil and petroleum products is mainly composed of oil pipelines, oil stations and other auxiliary related equipment. It is one of the main equipment in the oil storage and transportation industry, and it is also the most important transportation equipment for crude oil and petroleum products. Compared with railway and road oil transportation, which are also land transportation methods, pipeline oil transportation has the characteristics of large transportation volume, good airtightness, low cost and high safety factor.
[0003] The pipes of oil pipelines are generally steel pipes, and a heating system is also provided. There are two main methods: isothermal transportation and heated transportation. When the medium being transported is easy to solidify and has high viscosity (such as the oil produced by Daqing Oilfield with a high wax content), if its solidification point is higher than the ambient temperature around the pipeline or the viscosity is very high at the ambient temperature, it is impossible to directly use the isothermal method for transportation, because too high viscosity will greatly increase the pressure drop of the pipeline, which will not only consume a lot of power but also pose a safety hazard. Therefore, the method of heated transportation must be used to achieve the effect of reducing viscosity and reducing friction. The heating system is attached to the outer wall of the pipeline to keep the temperature of the pipeline to meet the needs of transportation. At present, countries around the world, especially major countries that produce waxy and viscous crude oil, are using long-distance pipeline heating and transportation technology for transportation. The heating cable used on the oil pipeline is the main heat source of the heating and transportation technology, and it still has considerable development potential in the future.
[0004] At present, the general heating product in China is heating cable belt. This kind of cable is mostly produced by extruding a layer of sheath on the outside of aluminum single wire. The process is simple. The heat dissipation of the single wire is low under the condition of low voltage power supply. Under the condition of oil pipelines that require high temperature transmission, it cannot provide sufficient heat source. Summary of the invention
[0005] The purpose of the present invention is to solve the problem that the current cables cannot provide sufficient heat source for the pipelines, to provide a heating cable for medium-pressure oil pipelines, and to provide a corresponding preparation process.
[0006] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:
[0007] A heating cable for a medium-pressure oil pipeline comprises a cable conductor made of 6201 aluminum-magnesium-silicon high-strength aluminum alloy, a conductor shielding layer is arranged outside the cable conductor, an insulating layer is arranged outside the conductor shielding layer, an insulating shielding layer is arranged outside the insulating layer, a metal shielding layer is arranged outside the insulating shielding layer, and a flame-retardant polyethylene outer sheath is arranged outside the metal shielding layer.
[0008] Taking into full consideration the short-circuit current conducting capability of the cable, the metal shielding layer of the cable is added. The metal shielding layer can effectively shield the external electromagnetic interference and can also conduct the metal shielding short-circuit current. Considering the high heat demand, the cable should be able to be used at a higher voltage level without breakdown, so the cross-linked polyethylene insulation layer is specially considered to increase the overall voltage resistance level of the cable.
[0009] During the production process of aluminum alloy conductors, metal burrs will be generated on the conductor surface. Under high voltage, the conductor burrs will cause insulation breakdown. In addition, the insulation layer should not contact the metal shielding layer.
[0010] The metal shielding layer will also cause mechanical damage to the insulation layer during cable bending, so a semi-conductive shielding layer should be extruded on the inner and outer layers of the insulation layer to increase the smoothness of the insulation interface and homogenize the field strength. The inner layer of the insulation layer is the conductor shielding layer, and the outer layer of the insulation layer is the insulation shielding layer.
[0011] In the selection and design of the cable outer sheath material, it is considered that the material should have a high voltage resistance level and high insulation. The material should be flame retardant and light in weight so as not to cause a high weight load on the oil pipeline. It should be light and easy to construct. After comprehensive consideration, the outer sheath material is determined to be flame retardant polyethylene material. This material has excellent properties such as low density, high volume resistivity, good insulation performance and flame retardancy.
[0012] The specific material configuration is as follows.
[0013] As a further preferred embodiment: the material of the insulating layer is prepared by the following components in parts by weight: 60 to 80 parts of linear low-density polyethylene, 30 to 40 parts of ethylene-octene copolymer, 20 to 30 parts of epoxy resin, 10 to 15 parts of aluminum hydroxide, 10 to 15 parts of magnesium oxide, 10-15 parts of hexagonal boron nitride, 10 to 30 parts of compatibilizer, 1 to 3 parts of antioxidant, 0.5 to 2 parts of coupling agent, and 1 to 5 parts of lubricant.
[0014] Since the cable in this case is mainly used for heating oil, the insulation layer is not only required to have better insulation properties, but also to be light in weight, have a certain flame retardant effect, and be able to effectively transfer heat.
[0015] Therefore, in this case, the above-mentioned ratio is adopted, and linear low-density polyethylene, ethylene-octene copolymer, and epoxy resin are used to make the insulation layer have a good thermal conductivity. In particular, the aluminum hydroxide, magnesium oxide, and hexagonal boron nitride in the auxiliary agent clinic can provide a certain flame retardant effect while also promoting the system to have good thermal conductivity, so that heat can be transferred out in a timely and effective manner, facilitating the heating of the oil. At the same time, the overall light weight can make the cable semi-suspended in the oil, avoiding sinking to the bottom and causing the heating effect to deteriorate.
[0016] As a further preferred embodiment: the material of the flame-retardant polyethylene outer sheath is prepared by the following components in parts by weight: 70 to 80 parts of low-density polyethylene, 20 to 40 parts of ethylene and vinyl acetate copolymer resin, 30 to 50 parts of silicone rubber, 15 to 30 parts of melamine polyphosphate, 10 to 30 parts of tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer, 20 to 30 parts of polyphenylene ether, 10 to 20 parts of aluminum hypophosphite, 10 to 30 parts of compatibilizer, 1 to 3 parts of antioxidant, 0.5 to 2 parts of coupling agent, and 1 to 5 parts of lubricant.
[0017] The main functions of the flame retardant polyethylene outer sheath are flame retardancy and heat conduction, and it must also have good interdependence with oil. This case uses a compound of silicone rubber, melamine polyphosphate, polyphenylene ether, and aluminum hypophosphite to provide good insulation and thermal conductivity. At the same time, tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer can ensure that the outer sheath has a smooth contact surface with the oil, thereby avoiding negative impact on the flow of the oil.
[0018] As a further preferred embodiment: the antioxidant is at least one of antioxidant 1010, antioxidant 1076, and antioxidant 168.
[0019] As a further preferred embodiment: the coupling agent is a silane coupling agent.
[0020] As a further preferred embodiment: the compatibilizer is at least one of maleic anhydride grafted ethylene-vinyl acetate, maleic anhydride grafted metallocene linear low-density polyethylene, and maleic anhydride grafted polyolefin elastomer.
[0021] As a further preferred embodiment: comprising the following steps:
[0022] Extrusion granulation is carried out according to the material ratio distribution of the insulation layer and the flame-retardant polyethylene outer sheath;
[0023] The temperature of each section of the twin-screw extruder is configured as follows: zone 1 100-120°C, zone 2 110-130°C, zone 3 130-145°C, zone 4 145-160°C, zone 5 160-180°C, zone 6 160-180°C, zone 7 150-180°C, zone 8 150-170°C, zone 9 140-160°C, and die head temperature 140-160°C;
[0024] Then, a heating cable for medium-pressure oil pipeline is prepared by multi-layer co-extrusion.
[0025] The above-mentioned medium-pressure oil pipeline heating cable provided in this solution has a conductor made of aluminum alloy, can be used under high-voltage power-on conditions, has high heat dissipation, can provide high temperature, and can provide a sustainable heat source above 65°C at the place where it is attached to the oil pipeline. The cable has a higher voltage resistance level than conventional heating cable belts, the insulation is made of cross-linked polyethylene material, and the sheath is made of flame-retardant polyethylene material, which increases the safety and reliability of the cable.
[0026] Compared with the prior art, the present invention has the following beneficial effects: it can provide sufficient heat source for oil when it is transported through the oil pipeline, so as to ensure the smooth transportation of oil in the oil pipeline. At the same time, the designed cable has a simple structure, high reliability, and a larger heat dissipation than conventional heating cables. The added cross-linked polyethylene insulation layer can be used under high voltage conditions. The cable itself can shield external electromagnetic interference and effectively conduct shielded short-circuit current. The cable is safe and environmentally friendly, light in weight, will not cause high weight load on the oil pipeline, and is light and easy to lay and install. The provided preparation process is easy to implement. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a schematic diagram of the structure of the cable of the present invention.
[0028] In the figure: 1 cable conductor, 2 conductor shielding layer, 3 insulation layer, 4 insulation shielding layer, 5 metal shielding layer, 6 flame retardant polyethylene outer sheath. DETAILED DESCRIPTION
[0029] The technical solution of the present invention is further described below through specific embodiments.
[0030] Unless otherwise specified, the raw materials used in the embodiments of the present invention are all commonly used raw materials in the art, and the methods used in the embodiments are all conventional methods in the art.
[0031] Embodiment 1: A heating cable for medium pressure oil pipeline, such as Figure 1 As shown, it includes a cable conductor made of 6201 aluminum-magnesium-silicon high-strength aluminum alloy, a conductor shielding layer is arranged outside the cable conductor, an insulating layer is arranged outside the conductor shielding layer, an insulating shielding layer is arranged outside the insulating layer, a metal shielding layer is arranged outside the insulating shielding layer, and a flame-retardant polyethylene outer sheath is arranged outside the metal shielding layer.
[0032] The material of the insulating layer is prepared from the following components in parts by weight: 60 parts of linear low-density polyethylene, 40 parts of ethylene-octene copolymer, 20 parts of epoxy resin, 15 parts of aluminum hydroxide, 10 parts of magnesium oxide, 15 parts of hexagonal boron nitride, 10 parts of compatibilizer, 3 parts of antioxidant, 0.5 parts of coupling agent, and 5 parts of lubricant. The antioxidant is antioxidant 168. The coupling agent is a silane coupling agent, and the compatibilizer is maleic anhydride grafted ethylene-vinyl acetate.
[0033] The material of the flame-retardant polyethylene outer sheath is prepared from the following components in parts by weight: 70 parts of low-density polyethylene, 40 parts of ethylene and vinyl acetate copolymer resin, 30 parts of silicone rubber, 30 parts of melamine polyphosphate, 10 parts of tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer, 30 parts of polyphenylene ether, 10 parts of aluminum hypophosphite, 30 parts of compatibilizer, 1 part of antioxidant, 2 parts of coupling agent, and 1 part of lubricant. The antioxidant is antioxidant 1010. The coupling agent is a silane coupling agent, and the compatibilizer is a maleic anhydride grafted polyolefin elastomer.
[0034] Then, the insulation layer and the flame-retardant polyethylene outer sheath are extruded and granulated according to the material ratio distribution;
[0035] A twin-screw extruder is used to configure the temperatures of each section, which are: zone one 100-120°C, zone two 110-130°C, zone three 130-145°C, zone four 145-160°C, zone five 160-180°C, zone six 160-180°C, zone seven 150-180°C, zone eight 150-170°C, zone nine 140-160°C, and a die head temperature of 140-160°C; then multi-layer co-extrusion is used to prepare a heating cable for a medium-pressure oil pipeline.
[0036] Example 2: The difference between Example 1 and Example 1 is that the material of the insulating layer is prepared by the following components in parts by weight: 80 parts of linear low-density polyethylene, 30 parts of ethylene-octene copolymer, 30 parts of epoxy resin, 10 parts of aluminum hydroxide, 15 parts of magnesium oxide, 10 parts of hexagonal boron nitride, 30 parts of compatibilizer, 1 part of antioxidant, 2 parts of coupling agent, and 1 part of lubricant. The coupling agent is a silane coupling agent, and the compatibilizer is maleic anhydride grafted ethylene-vinyl acetate. The antioxidant is antioxidant 1010.
[0037] The material of the flame retardant polyethylene outer sheath is prepared from the following components in parts by weight: 80 parts of low-density polyethylene, 20 parts of ethylene and vinyl acetate copolymer resin, 50 parts of silicone rubber, 15 parts of melamine polyphosphate, 30 parts of tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer, 20 parts of polyphenylene ether, 20 parts of aluminum hypophosphite, 10 parts of compatibilizer, 3 parts of antioxidant, 0.5 parts of coupling agent, and 5 parts of lubricant. The coupling agent is a silane coupling agent, and the compatibilizer is maleic anhydride grafted metallocene linear low-density polyethylene. The antioxidant is antioxidant 1010.
[0038] Example 3: The difference from Example 1 is that the material of the insulating layer is prepared by the following components in parts by weight: 60 parts of linear low-density polyethylene, 30 parts of ethylene-octene copolymer, 30 parts of epoxy resin, 15 parts of aluminum hydroxide, 10 parts of magnesium oxide, 10 parts of hexagonal boron nitride, 30 parts of compatibilizer, 3 parts of antioxidant, 0.5 parts of coupling agent, and 1 part of lubricant. The coupling agent is a silane coupling agent, and the compatibilizer is maleic anhydride grafted metallocene linear low-density polyethylene. The antioxidant is antioxidant 1010.
[0039] The material of the flame-retardant polyethylene outer sheath is prepared from the following components in parts by weight: 80 parts of low-density polyethylene, 40 parts of ethylene and vinyl acetate copolymer resin, 30 parts of silicone rubber, 15 parts of melamine polyphosphate, 30 parts of tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer, 30 parts of polyphenylene ether, 10 parts of aluminum hypophosphite, 10 parts of compatibilizer, 3 parts of antioxidant, 2 parts of coupling agent, and 1 part of lubricant. The coupling agent is a silane coupling agent, the compatibilizer is maleic anhydride grafted ethylene-vinyl acetate, and the antioxidant is antioxidant 1010.
[0040] The above are only preferred embodiments of the present invention and the technical principles used. Those skilled in the art will understand that the present invention is not limited to the specific embodiments described herein, and that various obvious changes, readjustments and substitutions can be made by those skilled in the art without departing from the scope of protection of the present invention. Therefore, although the present invention has been described in more detail through the above embodiments, the present invention is not limited to the above embodiments, and may include more other equivalent embodiments without departing from the concept of the present invention, and the scope of the present invention is determined by the scope of the appended claims.
Claims
1. A heating cable for medium pressure oil pipeline, characterized in that: It comprises a cable conductor made of 6201 aluminum-magnesium-silicon high-strength aluminum alloy, wherein a conductor shielding layer is arranged outside the cable conductor, an insulating layer is arranged outside the conductor shielding layer, an insulating shielding layer is arranged outside the insulating layer, a metal shielding layer is arranged outside the insulating shielding layer, and a flame-retardant polyethylene outer sheath is arranged outside the metal shielding layer; The material of the insulating layer is prepared by the following components in parts by weight: 60-80 parts of linear low-density polyethylene, 30-40 parts of ethylene-octene copolymer, 20-30 parts of epoxy resin, 10-15 parts of aluminum hydroxide, 10-15 parts of magnesium oxide, 10-15 parts of hexagonal boron nitride, 10-30 parts of compatibilizer, 1-3 parts of antioxidant, 0.5-2 parts of coupling agent, and 1-5 parts of lubricant; The material of the flame-retardant polyethylene outer sheath is prepared by the following components in parts by weight: 70-80 parts of low-density polyethylene, 20-40 parts of ethylene and vinyl acetate copolymer resin, 30-50 parts of silicone rubber, 15-30 parts of melamine polyphosphate, 10-30 parts of tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer, 20-30 parts of polyphenylene ether, 10-20 parts of aluminum hypophosphite, 10-30 parts of compatibilizer, 1-3 parts of antioxidant, 0.5-2 parts of coupling agent, and 1-5 parts of lubricant; The antioxidant is at least one of antioxidant 1010, antioxidant 1076, and antioxidant 168; the coupling agent is a silane coupling agent; and the compatibilizer is at least one of maleic anhydride grafted ethylene-vinyl acetate, maleic anhydride grafted metallocene linear low-density polyethylene, and maleic anhydride grafted polyolefin elastomer.
2. The preparation process of a heating cable for medium-pressure oil pipeline according to claim 1, characterized in that: The following steps are involved: Extrusion granulation is carried out according to the material ratio distribution of the insulation layer and the flame-retardant polyethylene outer sheath; The temperature of each section of the twin-screw extruder is configured as follows: zone 1 100-120°C, zone 2 110-130°C, zone 3 130-145°C, zone 4 145-160°C, zone 5 160-180°C, zone 6 160-180°C, zone 7 150-180°C, zone 8 150-170°C, zone 9 140-160°C, and die head temperature 140-160°C; Then, a heating cable for medium-pressure oil pipeline is prepared by multi-layer co-extrusion.
Citation Information
Patent Citations
Heat-conducting wire cable electric-insulation material or sheath material
CN104017267A
High-strength high-temperature-resistant cable sheath material
CN105949596A
Long-distance-pipeline electric heat tracing system and laying method thereof
CN108980504A
Double-layer coextruded insulation LED ultraviolet crosslinking colored low-smoke halogen-free flame-retardant cable material and preparation method thereof
CN110951141A
Manufacturing method of intelligent power cable based on double-frequency RFID technology and cable
CN112435811A
Cited By
High-strength aluminum alloy medium-voltage power cable
CN122266859A