Laminated structure and method for producing laminated structure
By atomizing gallium aqueous solution on the lithium tantalate substrate, the β-Ga2O3 film is formed, which solves the problems of low-temperature film formation and thermal instability in the existing technology, and realizes cheap and fast thermally stable film preparation. Semiconductor devices provide efficient solutions.
Patent Information
- Application Number
- CN202080059393.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-06-05
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-06-05
AI Technical Summary
The prior art is difficult to effectively manufacture thermally stable and inexpensive gallium oxide (β-Ga2O3) films under low temperature conditions, resulting in thermal instability and cost and time problems of high-temperature film formation in semiconductor devices.
Lithium tantalate is used as a crystalline substrate, and thermal reaction is carried out by atomizing or dropping gallium aqueous solution to form a crystalline oxide film with a β-gallia structure, and a low-temperature process (250-900°C) is used to produce thermally stable a layered structure.
It is easy and cheap to manufacture β-Ga2O3 films with high thermal stability at low temperatures, and is suitable for semiconductor devices, reducing production costs and time, and improving film quality through subsequent heat treatment.
Smart Images

Figure CN114302982B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a stacked structure and a method for producing the stacked structure. Background Art
[0002] As a semiconductor with a large band gap, gallium oxide (Ga 2 O 3 ) are expected to be used in next-generation switching elements that can achieve high withstand voltage, low loss and high heat resistance.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2014-072463
[0006] Patent Document 2: Japanese Patent Application Publication No. 2014-015366
[0007] Patent Document 3: Japanese Patent Application Publication No. 2015-091740 Summary of the invention
[0008] Technical Problems to be Solved by the Invention
[0009] Patent document 1 discloses a method for producing gallium oxide (α-Ga) with a corundum structure at a relatively low temperature. 2 O 3 ) method, but α-Ga 2 O 3 It is a metastable phase and therefore has the problem of thermal instability.
[0010] In contrast, β-Ga 2 O 3 However, as described in Patent Documents 2 and 3, extremely high temperatures are required for film formation, and thus a simple and inexpensive film formation method at a lower temperature is desired.
[0011] The present invention is made to solve the above-mentioned problems, and its object is to provide an inexpensive stacked structure having a thermally stable crystalline oxide film, and to provide a film forming method capable of forming a stacked structure having a thermally stable crystalline oxide film simply and inexpensively by a low-temperature process.
[0012] Technical means to solve technical problems
[0013] To achieve the above object, the present invention provides a stacked structure having a crystalline substrate and a crystalline oxide film having gallium as a main component and having a β-gallia structure, wherein the crystalline substrate is a crystalline substrate having lithium tantalate as a main component.
[0014] The above-mentioned stacked structure can be obtained easily and inexpensively, is thermally stable, and can be suitably used in semiconductor devices.
[0015] In this case, the crystalline substrate may be a stacked structure in which the crystalline substrate is a lithium tantalate single crystal substrate.
[0016] As a result, a stacked structure including a crystalline oxide film having a β-gallia structure with higher crystallinity is formed.
[0017] In this case, the crystalline oxide film may be formed of β-Ga 2 O 3 A laminated structure as the main component.
[0018] Thus, a stacked structure having a more thermally stable crystalline oxide film is formed.
[0019] In this case, the crystalline oxide film may have a layered structure with a thickness of 1 μm or more.
[0020] Thus, a stacked structure that is more useful for a semiconductor device is formed.
[0021] At this time, the area of the crystalline oxide film can be set to 100 mm 2 The above stacked structure.
[0022] Thus, a large-area stacked structure that is more useful for a semiconductor device is formed.
[0023] At this time, a method for manufacturing a stacked structure can be provided, which is a method for transporting mist generated by atomizing or dropletizing an aqueous solution containing at least gallium to a substrate using a carrier gas, and causing the mist to undergo a thermal reaction on the substrate to form a crystalline oxide film containing gallium as a main component and having a β-gallia structure. In the method for manufacturing the stacked structure, a crystalline substrate containing lithium tantalate as a main component is used as the substrate.
[0024] According to the method for producing a stacked structure, a stacked structure including a crystalline oxide film having a β-gallia structure can be produced simply and inexpensively by a low-temperature process with high productivity.
[0025] In this case, a method for manufacturing a stacked structure using a lithium tantalate single crystal substrate as the crystalline substrate can be used.
[0026] Thus, a stacked structure including a crystalline oxide film having a β-gallia structure with higher crystallinity can be produced.
[0027] In this case, the method for producing a laminated structure can be performed in which the temperature of the thermal reaction is set to 250 to 900°C.
[0028] As a result, since the stacked structure having a β-gallia structure can be produced at a lower temperature, not only the running cost can be reduced, but also the time required for production can be shortened.
[0029] At this time, the crystalline oxide film may be made of β-Ga 2 O 3 A method for producing a laminated structure as a main component.
[0030] Thus, a stacked structure having a more thermally stable crystalline oxide film can be provided.
[0031] In this case, the method for manufacturing a stacked structure can be such that the film thickness of the crystalline oxide film is 1 μm or more.
[0032] Thereby, a stacked structure more useful for a semiconductor device can be obtained.
[0033] In this case, the film-forming surface area can be set to 100 mm 2 A method for manufacturing a stacked structure having the above substrate as the substrate.
[0034] Thereby, a large-area stacked structure can be obtained simply and inexpensively.
[0035] At this time, the obtained stacked structure may be heat treated at 600 to 1000°C.
[0036] Thereby, a higher quality laminated structure can be obtained.
[0037] Effects of the Invention
[0038] As described above, the laminated structure of the present invention is thermally stable and can be suitably used in semiconductor devices. In addition, according to the method for producing a laminated structure of the present invention, a laminated structure having a β-gallia structure can be produced simply and inexpensively. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is a schematic cross-sectional view showing an example of the laminated structure of the present invention.
[0040] Figure 2 This is a schematic structural diagram showing an example of a film forming apparatus used in the method for producing a laminated structure of the present invention.
[0041] Figure 3 This is a diagram for explaining an example of an atomizing unit in a film forming apparatus.
[0042] Figure 4The results of evaluating the film obtained in Example 1 using an X-ray diffraction apparatus are shown. DETAILED DESCRIPTION
[0043] Hereinafter, the present invention will be described in detail, but the present invention is not limited thereto.
[0044] As described above, it is desired to provide an inexpensive multilayer structure having a thermally stable crystalline oxide film, and to provide a method for producing a multilayer structure that can form a thermally stable crystalline oxide film simply and inexpensively by a low-temperature process.
[0045] The inventors of the present invention have conducted careful studies on the above-mentioned technical problems and have found that the following stacked structure can be easily and cheaply obtained, is thermally stable, and is suitable for use in semiconductor devices, thereby completing the present invention. The stacked structure comprises a crystalline substrate and a crystalline oxide film having gallium as a main component and having a β-gallia structure, and the crystalline substrate is a crystalline substrate having lithium tantalate as a main component.
[0046] In addition, the inventors of the present invention have discovered that the following method for manufacturing a stacked structure can manufacture a stacked structure including a crystalline oxide film having a β-gallia structure at low temperature, high productivity, simply and inexpensively, thereby completing the present invention. The manufacturing method is a method in which a mist generated by atomizing or dropletizing an aqueous solution containing at least gallium is transported to a substrate using a carrier gas, and the mist is subjected to a thermal reaction on the substrate to form a crystalline oxide film having gallium as a main component and having a β-gallia structure. In the manufacturing method, a crystalline substrate having lithium tantalate as a main component is used as the substrate.
[0047] Hereinafter, description will be given with reference to the drawings.
[0048] (Laminated structure)
[0049] like Figure 1 As shown, one embodiment of the stacked structure 1 of the present invention is a crystalline oxide film 20 having gallium as a main component and having a β-gallia structure stacked on a crystalline substrate 10 having lithium tantalate as a main component. In addition, a buffer layer or the like may be present between the crystalline substrate 10 and the crystalline oxide film 20.
[0050] Here, "crystallinity" means that the crystal state includes a polycrystalline state or a single crystal state. Amorphous substances may be mixed in polycrystalline or single crystal.
[0051] (Crystalline substrate with lithium tantalate as main component)
[0052] First, a crystalline substrate having lithium tantalate as a main component, which is included in the layered structure of the present invention, will be described.
[0053] When manufacturing the stacked structure of the present invention, first, a crystalline substrate containing lithium tantalate as a main component is prepared. Here, "crystalline substrate containing lithium tantalate as a main component" includes a substrate containing 50 to 100% lithium tantalate and the lithium tantalate may be a single crystal or a polycrystalline substrate.
[0054] Lithium tantalate has an ilmenite structure, and its lattice constant is closer to that of α-Ga 2 O 3 α-Ga 2 O 3 (001) plane and β-Ga 2 O 3 The size relationship between the oxygen atoms on the (-201) plane and the (001) plane of lithium tantalate is roughly 2 O 3 <Lithium Tantalate<β-Ga 2 O 3 . with α-Ga 2 O 3 Compared to β-Ga 2 O 3 It is more energetically stable, so it is speculated that β-Ga will preferentially form on the lithium tantalate substrate even at low temperatures. 2 O 3 Instead of forming α-Ga 2 O 3 .
[0055] As the crystalline substrate containing lithium tantalate as a main component, a lithium tantalate single crystal substrate is most preferably used because a crystalline oxide film having the highest film quality can be formed.
[0056] The following description will be made using a lithium tantalate single crystal substrate as an example. The lithium tantalate single crystal substrate can be obtained, for example, by growing a lithium tantalate single crystal by a Czochralski method to obtain a lithium tantalate single crystal ingot, and slicing the ingot to form a substrate shape.
[0057] The lithium tantalate single crystal substrate that can be used in the present invention is preferably cut in such a way that the lattice constant of its surface is close to the lattice constant of the crystalline oxide film that is subsequently deposited. 2 O 3 In the case of a crystalline oxide film as a main component, it is preferable to cut so that the crystal orientation is within Z±10°, and more preferably, it is cut so that the crystal orientation is within Z±5°.
[0058] In addition, for the lithium tantalate single crystal substrate that can be used in the present invention, it is preferred that the polarization state of the substrate be homogenized, since this promotes uniform growth of the oxide single crystal film. That is, it is preferred that the lithium tantalate substrate be subjected to single polarization treatment or multi-polarization treatment.
[0059] For the obtained substrate that has undergone a single polarization treatment, for example, a lithium tantalate single crystal ingot produced by the pulling method can be heated to 700°C, and a voltage of 200V is applied in the crystal orientation Z direction to perform a polarization treatment for 10 hours, and then the ingot is sliced and processed into a substrate shape. Alternatively, the substrate processed into a substrate shape can be heated to 700°C, and a voltage of 200V is applied in the crystal orientation Z direction to perform a polarization treatment for 10 hours.
[0060] When using a substrate that has been subjected to a single polarization treatment, if a pyroelectricity suppression treatment is further performed on the substrate surface, it is preferred that the substrate be charged when a crystalline oxide film is deposited on the heated substrate. For the pyroelectricity suppression treatment, for example, a lithium tantalate single crystal substrate that has been subjected to a single polarization treatment is buried in lithium carbonate powder and heat treated at a temperature above 350°C and below the Curie temperature (about 610°C) in a reducing gas atmosphere. At this time, if the volume resistivity of the substrate in the thickness direction is set to 1.0×10 11 Ω·cm or more and 2.0×10 13 If the substrate is treated so that the ratio of the maximum value to the minimum value of the volume resistivity in the substrate is 4.0 or less, it is possible to effectively suppress the charging of the substrate when a crystalline oxide film is deposited on the substrate.
[0061] On the other hand, in order to obtain a substrate that has been subjected to multi-polarization treatment, for example, a single crystal (ingot or substrate) that has been subjected to single polarization in advance, or a single crystal (ingot or substrate) that has not been subjected to single polarization treatment, can be heated to above 700°C and annealed for several hours (preferably above 1000°C, preferably above 5 hours, and more preferably above 10 hours) to perform a deformation relaxation treatment. In the case of an ingot, it is sliced and processed into a substrate shape. If a substrate that has been subjected to multi-polarization treatment is used, it is possible to suppress the charging of the substrate when a crystalline oxide film is deposited on the heated substrate, which is preferred. In particular, if the average domain size of the polarization on the surface of the substrate is made less than 5 μm, the charging can be effectively suppressed. If the charging effect of the lithium tantalate substrate is suppressed, the crystalline oxide film can be stably deposited, which is more preferred. In addition, if the composition of the lithium tantalate single crystal (at least on the surface of the substrate) is made to be a congruent composition, the average ferroelectric domain of the polarization on the surface of the substrate is likely to become smaller, which is preferred. In the case of lithium tantalate, the isocratic composition means that the ratio of Li to Ta is Li:Ta=48.5-α:51.5+α, where α is in the range of -0.5≤α≤0.5.
[0062] If the surface of a crystalline substrate mainly composed of lithium tantalate is polished to be smooth so as to reduce the unevenness, a flat crystalline oxide film can be obtained as a laminated film. Ra is preferably 10 nm or less. More preferably, Ra is 5 nm or less.
[0063] In addition, ions selected from hydrogen, helium, argon, and other rare gases may be pre-implanted into the surface of the crystalline substrate with lithium tantalate as the main component on which the crystalline oxide film is deposited, so as to form a fragile layer 50 nm to 3 μm below the deposited surface. Thus, after the crystalline oxide film is deposited, the deposited crystalline oxide film can be easily peeled off from the lithium tantalate single crystal substrate by giving an impact to the fragile layer.
[0064] The thickness of the crystalline substrate is not particularly limited, but is preferably 10 to 2000 μm, more preferably 50 to 800 μm. In addition, the area of the substrate is preferably 100 mm 2 More preferably, the diameter is 2 inches (50 mm) or more.
[0065] (Crystalline oxide film)
[0066] The crystalline oxide film in the stacked structure of the present invention is a crystalline oxide film having gallium as a main component and a β-gallia structure. Crystalline oxide films are usually composed of metals and oxygen. In the present invention, gallium can be used as the main component of the metal. In the present invention, when "gallium is used as the main component", it means that 50 to 100% of the metal component is gallium. As metal components other than gallium, for example, one or more metals selected from iron, indium, aluminum, vanadium, titanium, chromium, rhodium, iridium, nickel and cobalt may be contained. In addition, as long as the crystalline oxide film has a β-gallia structure, it can be either single crystal or polycrystalline.
[0067] Among the crystalline oxide films containing gallium as a main component and having a β-gallia structure, β-Ga is particularly preferred. 2 O 3 A crystalline oxide film as the main component. β-Ga 2 O 3 It is a more thermally stable crystalline oxide film. When evaluated by X-ray diffraction, α-Ga 2 O 3 There is a peak near 2θ = 40.3°, while β-Ga 2 O 3 Since there is a peak near 2θ=38.4°, the two can be easily distinguished.
[0068] The crystalline oxide film may contain a dopant, for example, an n-type dopant such as tin, germanium, silicon, titanium, zirconium, vanadium or niobium, or a p-type dopant such as copper, silver, tin, iridium, rhodium, etc. The dopant is not particularly limited, but tin is preferred. The concentration of the dopant can be, for example, about 1×10 16 / cm 3 ~1×10 22 / cm 3 , which can be set to about 1×10 17 / cm 3 The following low concentrations can also be set to about 1×10 20 / cm 3 Above high concentration.
[0069] In the present invention, the film thickness of the crystalline oxide film is not particularly limited and may be greater than 1 μm. For example, it may be 1 to 100 μm, preferably 5 to 50 μm, and more preferably 10 to 20 μm. In addition, other layers may be provided between the substrate and the crystalline oxide film. Other layers are layers having different compositions from the substrate and the crystalline oxide film as the outermost layer, and may be, for example, any one of a crystalline oxide film, an insulating film, a metal film, and the like.
[0070] The stacked structure of the present invention or the crystalline oxide film obtained from the stacked structure can be used in semiconductor devices by appropriately designing the structure. For example, the semiconductor layers of Schottky barrier diodes (SBDs), metal-semiconductor field effect transistors (MESFETs), high electron mobility transistors (HEMTs), metal-oxide semiconductor field effect transistors (MOSFETs), static induction transistors (SITs), junction field effect transistors (JFETs), insulated gate bipolar transistors (IGBTs), light emitting diodes (LEDs), etc. can be formed.
[0071] (Film forming device)
[0072] One embodiment of the stacked structure of the present invention is a method for forming a crystalline oxide film, which comprises using a carrier gas to transport a mist generated by atomizing or dropletizing an aqueous solution containing at least gallium to a substrate, and then causing the mist to undergo a thermal reaction on the substrate to form a crystalline oxide film. The method is characterized in that the substrate is a crystalline substrate having lithium tantalate as a main component, and the crystalline oxide film has gallium as a main component and has a β-gallia structure.
[0073] Figure 2 An example of a film forming apparatus 101 that can be used in the method for manufacturing a laminated structure of the present invention is shown. The film forming apparatus 101 includes an atomizing unit 120 that atomizes a raw material solution to generate mist, a carrier gas supply unit 130 that supplies a carrier gas for transporting the mist, a film forming unit 140 that performs a heat treatment on the mist to form a film on a substrate, and a transport unit 109 that connects the atomizing unit 120 and the film forming unit 140 and transports the mist through the carrier gas. In addition, the film forming apparatus 101 can be controlled by having a control unit (not shown) that controls the entire or a part of the film forming apparatus 101.
[0074] In addition, here, mist in the present invention is a general term for liquid particles dispersed in gas, and includes substances called mist, liquid droplets, etc.
[0075] (Raw material solution)
[0076] The raw material solution 104a is not particularly limited as long as it contains at least gallium. That is, in addition to gallium, it may also contain one or more metals selected from, for example, iron, indium, aluminum, vanadium, titanium, chromium, rhodium, iridium, nickel and cobalt. A solution in which the metal is dissolved or dispersed in water in the form of a complex or a salt can be appropriately used. As the form of the complex, for example, acetylacetone complexes, carbonyl complexes, amine complexes, hydride complexes, etc. can be listed. As the form of the salt, for example, metal chloride salts, metal bromide salts, metal iodide salts, etc. can be listed. In addition, a solution in which the above-mentioned metal is dissolved in hydrobromic acid, hydrochloric acid, hydroiodic acid, etc. can also be used in the form of an aqueous solution of the salt. The solute concentration is preferably 0.01 to 1 mol / L.
[0077] The raw material solution 104a may contain a dopant element. For example, n-type dopants such as tin, germanium, silicon, titanium, zirconium, vanadium or niobium, or p-type dopants such as copper, silver, tin, iridium, rhodium, etc. can be listed. The dopant is not particularly limited, and tin is preferred. In addition, it is preferred that the dopant element is ionized. Therefore, an acid can be mixed in the raw material solution 104a to promote the dissolution of the dopant element. As the acid, for example, hydrogen halides such as hydrobromic acid, hydrochloric acid, and hydroiodic acid, halogen oxoacids such as hypochlorous acid, chlorous acid, hypobromous acid, bromous acid, hypoiodous acid, iodic acid, etc., carboxylic acids such as formic acid, nitric acid, etc. can be listed. In addition, heating or applying ultrasound is also effective in promoting dissolution.
[0078] (Atomization part)
[0079] In the atomizing unit 120, the raw material solution 104a is prepared and atomized to generate mist. The atomizing means is not particularly limited as long as the raw material solution 104a can be atomized, and can be a known atomizing means, but an atomizing means based on ultrasonic vibration is preferably used. The reason is that atomization can be performed more stably.
[0080] An example of the atomizing unit 120 is shown in FIG. Figure 3 . It may include a mist generating source 104 containing a raw material solution 104a, a container 105 containing a medium that can transmit ultrasonic vibrations, such as water 105a, and an ultrasonic vibrator 106 installed on the bottom surface of the container 105. In detail, the mist generating source 104 composed of a container containing the raw material solution 104a is stored in the container 105 containing water 105a using a support body (not shown). The ultrasonic vibrator 106 is arranged at the bottom of the container 105, and the ultrasonic vibrator 106 and the oscillator 116 are connected. Moreover, it is configured in the following manner: when the oscillator 116 is operated, the ultrasonic vibrator 106 vibrates, and the ultrasonic wave is transmitted to the mist generating source 104 through the water 105a, and the raw material solution 104a is atomized.
[0081] (Transportation Department)
[0082] The transport unit 109 connects the atomizing unit 120 and the film forming unit 140. The mist is transported from the mist generating source 104 of the atomizing unit 120 to the film forming chamber 107 of the film forming unit 140 by the carrier gas through the transport unit 109. The transport unit 109 can be, for example, a supply pipe 109a. As the supply pipe 109a, for example, a quartz pipe or a resin pipe can be used.
[0083] (Film Forming Department)
[0084] In the film forming unit 140, the mist is heated to cause a thermal reaction, thereby forming a film on a part or all of the surface of the substrate (crystalline substrate) 110. The film forming unit 140 includes, for example, a film forming chamber 107, in which the substrate (crystalline substrate) 110 is disposed, and may include a heating plate 108 for heating the substrate (crystalline substrate) 110. The heating plate 108 may be as follows: Figure 2 Although shown as being provided outside the film forming chamber 107, it may be provided inside the film forming chamber 107. In addition, in the film forming chamber 107, an exhaust port 112 for exhaust gas may be provided at a position that does not affect the supply of mist to the substrate (crystalline substrate) 110.
[0085] In the present invention, the substrate (crystalline substrate) 110 may be disposed on the upper surface of the film forming chamber 107 so as to face downward, or may be disposed on the bottom surface of the film forming chamber 107 so as to face upward.
[0086] Regarding the thermal reaction, as long as the mist can react by heating, the reaction conditions are not particularly limited. It can be appropriately set according to the raw materials or the film-forming material. For example, the heating temperature can be in the range of 250 to 900° C., preferably in the range of 300 to 800° C., and more preferably in the range of 350 to 700° C.
[0087] The thermal reaction can be carried out in any atmosphere of vacuum, non-oxygen atmosphere, reducing gas atmosphere, air atmosphere and oxygen atmosphere, and can be appropriately set according to the film to be formed. In addition, the reaction pressure can be carried out under any conditions of atmospheric pressure, pressurized or reduced pressure, but if the film is formed under atmospheric pressure, the device structure can be simplified, so it is preferred.
[0088] (Carrier gas supply unit)
[0089] The carrier gas supply unit 130 may include a carrier gas source 102a for supplying a carrier gas, and a flow rate regulating valve 103a for regulating the flow rate of the carrier gas (hereinafter referred to as "main carrier gas") delivered from the carrier gas source 102a. In addition, a dilution carrier gas source 102b for supplying a dilution carrier gas and a flow rate regulating valve 103b for regulating the flow rate of the dilution carrier gas delivered from the dilution carrier gas source 102b may also be provided as needed.
[0090] The type of carrier gas is not particularly limited and can be appropriately selected according to the film-forming material. For example, inert gases such as oxygen, ozone, nitrogen or argon, or reducing gases such as hydrogen and forming gas can be listed. In addition, the type of carrier gas can be one or more than two. For example, a dilution gas obtained by diluting the same gas as the first carrier gas (for example, diluting 10 times) with a gas other than the first carrier gas can be used as the second carrier gas, or air can be used.
[0091] In the present invention, the carrier gas flow rate Q refers to the total flow rate of the carrier gas. In the above example, the carrier gas flow rate Q is the total of the flow rate of the main carrier gas sent from the carrier gas source 102a and the flow rate of the dilution carrier gas sent from the dilution carrier gas source 102b.
[0092] The flow rate Q of the carrier gas can be appropriately determined according to the size of the film formation chamber or the substrate, but is usually 1 to 60 L / min, preferably 2 to 40 L / min.
[0093] (Film Forming Method)
[0094] Then, refer to the following Figure 2 , an example of the film forming method of the present invention is described. First, the raw material solution 104a is stored in the mist generation source 104 of the atomizing unit 120, and the substrate (crystalline substrate) 110 is directly placed on the electric hot plate 108 or placed on the electric hot plate 108 via the wall of the film forming chamber 107, and the electric hot plate 108 is operated. Since the thermal expansion coefficient of lithium tantalate is large, it is preferred to slowly increase the temperature from a low temperature.
[0095] Then, open the flow regulating valves 103a and 103b, and supply the carrier gas from the carrier gas sources 102a and 102b to the film forming chamber 107, and use the carrier gas to fully replace the atmosphere of the film forming chamber 107. At the same time, adjust the flow rate of the main carrier gas and the flow rate of the dilution carrier gas respectively, so as to control the carrier gas flow rate Q.
[0096] In the step of generating mist, the ultrasonic vibrator 106 is vibrated, and the vibration is propagated to the raw material solution 104a through the water 105a, thereby atomizing the raw material solution 104a to generate mist. Next, in the step of transporting the mist using a carrier gas, the mist is transported from the atomizing unit 120 to the film forming unit 140 through the transport unit 109 using a carrier gas, and introduced into the film forming chamber 107. In the step of forming a film, the mist introduced into the film forming chamber 107 is heat-treated and thermally reacted by the heat of the electric hot plate 108 in the film forming chamber 107, thereby forming a film on the substrate (crystalline substrate) 110.
[0097] Before forming the crystalline oxide film containing gallium as the main component, a buffer layer may be formed. As the material of the buffer layer, Al may be used appropriately. 2 O 3 , Ga 2 O 3 Cr 2 O 3 , Fe 2 O 3 、In 2 O 3 , Rh 2 O 3 、V 2 O 3 、Ti 2 O 3 , Ir 2 O 3 Etc. The buffer layer can be formed by known methods such as sputtering and evaporation, but it is preferably formed by the atomized CVD method of the present invention. Specifically, a solution in which one or more metals selected from aluminum, gallium, chromium, iron, indium, rhodium, vanadium, titanium, and iridium are dissolved or dispersed in water in the form of a complex or salt can be appropriately used as a raw material aqueous solution. As the form of the complex, for example, acetylacetone complexes, carbonyl complexes, amine complexes, hydride complexes, etc. can be listed. As the form of the salt, for example, chloride metal salts, bromide metal salts, iodide metal salts, etc. can be listed. In addition, a solution obtained by dissolving the above metals in hydrobromic acid, hydrochloric acid, hydroiodic acid, etc. can also be used in the form of an aqueous solution of the salt. The solute concentration is preferably 0.01 to 1 mol / L. Regarding other conditions, the buffer layer can be formed under the same conditions as above. After the buffer layer is formed into a film with a specified thickness, a crystalline oxide film with gallium as the main component is prepared by the above method. The thickness of the buffer layer is preferably 0.1 μm to 2 μm.
[0098] (Heat Treatment)
[0099] The obtained stacked structure can be heat treated at 600 to 1000° C. Thus, unreacted species in the film can be removed, and a higher quality stacked structure can be obtained. The heat treatment can be carried out in air or oxygen atmosphere, or in an inert gas atmosphere such as nitrogen or argon. The heat treatment time can be appropriately determined, for example, it can be set to 5 to 240 minutes.
[0100] (Evaluation of film quality)
[0101] The composition of the obtained film can be evaluated by elemental analysis based on energy dispersive X-ray analysis (EDS). In addition, the crystallinity can be evaluated by X-ray diffraction. The peak near 2θ=38.4° (β-Ga 2 O 3peak) and the peak near 2θ=40.3° (α-Ga 2 O 3 The crystallinity of the film was evaluated by the presence or absence of peaks) and the half-width of the rocking curves of these peaks.
[0102] (peel off)
[0103] The crystalline substrate can be peeled off from the crystalline oxide film. The peeling means is not particularly limited and can be a known means. For example, a means of peeling by applying mechanical impact, a means of peeling by applying heat and utilizing thermal stress, a means of peeling by applying vibration such as ultrasound, a means of peeling by etching, laser peeling, etc. can be cited. By the peeling, a crystalline oxide film as an independent film can be obtained.
[0104] (electrode)
[0105] The electrodes necessary for forming a semiconductor device can be formed using conventional methods. That is, any one of methods such as evaporation, sputtering, CVD, electroplating, and printing methods that make resins and the like bond together can be used. As electrode materials, in addition to metals such as Al, Ag, Ti, Pd, Au, Cu, Cr, Fe, W, Ta, Nb, Mn, Mo, Hf, Co, Zr, Sn, Pt, V, Ni, Ir, Zn, In, and Nd, metal oxide conductive films such as tin oxide, zinc oxide, indium oxide, indium tin oxide (ITO), indium zinc oxide (IZO), and organic conductive compounds such as polyaniline, polythiophene, or polypyrrole can also be used, and alloys or mixtures of two or more of these components can also be used. The thickness of the electrode is preferably 1 to 1000 nm, and more preferably 10 to 500 nm.
[0106] Example
[0107] Hereinafter, the present invention will be described in detail with reference to Examples, but these Examples do not limit the present invention.
[0108] (Example 1)
[0109] According to the method for producing the stacked structure, gallium oxide (β-Ga) having a β-gallia structure is produced. 2 O 3 ) is formed into a film to obtain a stacked structure.
[0110] Specifically, first, a lithium tantalate single crystal substrate of the same composition (Li / (Li+Ta) value is 0.485) is prepared as a crystalline substrate. The lithium tantalate single crystal prepared by the pulling method is Z-cut and processed into a C-surface substrate, and multipolarized by heating at 700°C for 10 hours, and the surface is polished to a surface roughness of Ra = 0.5 nm. Then, as a raw material aqueous solution, a 0.1 mol / L gallium bromide aqueous solution is prepared, and further a 48% hydrobromic acid solution is added in a manner that the volume ratio is 10% so that it contains a 48% hydrobromic acid solution, and this is used as a raw material solution 104a.
[0111] The raw material solution 104a obtained in the above manner is contained in the mist generation source 104. Then, in the film forming chamber 107, a 4-inch (diameter 100 mm) c-plane lithium tantalate substrate as a substrate (crystalline substrate) 110 is placed on a hot plate 108, and the hot plate 108 is operated to raise the temperature to 400°C.
[0112] Then, the flow regulating valves 103a and 103b are opened, and nitrogen gas as a carrier gas is supplied from the carrier gas sources 102a and 102b into the film forming chamber 107, and the atmosphere of the film forming chamber 107 is fully replaced by the carrier gas, and at the same time, the flow rate of the main carrier gas is adjusted to 4 L / min, and the flow rate of the dilution carrier gas is adjusted to 20 L / min. That is, the carrier gas flow rate Q = 24 L / min.
[0113] Then, the ultrasonic vibrator 106 is vibrated at 2.4 MHz, and the vibration is propagated to the raw material solution 104a through the water 105a, thereby atomizing the raw material solution 104a to generate mist. The mist is introduced into the film forming chamber 107 through the supply pipe 109a using a carrier gas. Then, the mist is thermally reacted in the film forming chamber 107 under the conditions of atmospheric pressure and 400°C, thereby forming gallium oxide (β-Ga) having a β-gallia structure on the substrate (crystalline substrate) 110. 2 O 3 The film forming time was set to 15 minutes.
[0114] The obtained film was subjected to elemental analysis by EDS, and it was confirmed that Ga 2 O 3 In addition, the results evaluated by the X-ray diffraction device are shown in Figure 4 When the X-ray source is set to CuKα line, β-Ga is confirmed near 2θ=38.4°. 2 O 3 The rocking curve of this peak was measured and the half-peak width was calculated, which was 45 seconds. In addition, the obtained gallium oxide film was annealed at 600°C for 3 hours, but the crystallinity of the film did not change.
[0115] (Example 2)
[0116] Film formation and evaluation were performed under the same conditions as in Example 1 except that the film formation temperature was set to 350°C. 2 O 3 The half-value width of the peak was 40 seconds. In addition, the obtained gallium oxide film was annealed at 600° C. for 3 hours, but the crystallinity of the film did not change.
[0117] (Example 3)
[0118] Film formation and evaluation were performed under the same conditions as in Example 1 except that the film formation temperature was set to 550°C. 2 O 3 The half-value width of the peak was 53 seconds. The obtained gallium oxide film was annealed at 600° C. for 3 hours, but the crystallinity of the film did not change.
[0119] (Example 4)
[0120] As the raw material aqueous solution, a 48% hydrobromic acid solution was contained and dissolved in 0.1 mol / L gallium acetylacetonate at a volume ratio of 10%, and this was used as the raw material solution 104a. Film formation and evaluation were performed under the same conditions as in Example 1 except for this. β-Ga 2 O 3 The half-value width of the peak was 43 seconds. In addition, the obtained gallium oxide film was annealed at 600° C. for 3 hours, but the crystallinity of the film did not change.
[0121] (Example 5)
[0122] Film formation and evaluation were performed under the same conditions as in Example 1 except that 0.1 mol / L of gallium iodide was used as the raw material solution 104a. 2 O 3 The half-value width of the peak was 33 seconds. The obtained gallium oxide film was annealed at 600° C. for 3 hours, but the crystallinity of the film did not change.
[0123] (Example 6)
[0124] In addition to the raw material aqueous solution of Example 1, 5×10 -4 The film formation and evaluation were carried out under the same conditions as in Example 1 except that 1 mol / L of tin(II) chloride was mixed. 2 O 3 The half-value width of the peak was 37 seconds. The obtained gallium oxide film was annealed at 600° C. for 3 hours, but the crystallinity of the film did not change.
[0125] (Example 7)
[0126] The film formation and evaluation were performed under the same conditions as in Example 1 except that the lithium tantalate single crystal substrate was polarized. 2 O 3 The half-value width of the peak was 52 seconds. The obtained gallium oxide film was annealed at 600° C. for 3 hours, but the crystallinity of the film did not change.
[0127] (Example 8)
[0128] A buffer layer was provided on a lithium tantalate single crystal substrate. Specifically, as a raw material aqueous solution, a 48% hydrobromic acid solution in 0.1 mol / L chromium acetylacetonate was contained and dissolved in the chromium acetylacetonate in a manner of 10% by volume, and this was used as a raw material solution. Otherwise, the film was formed under the same conditions as in Example 1. Elemental analysis was performed by energy dispersive X-ray analysis (EDS), and the result confirmed that it was Cr 2 O 3 Then, a gallium oxide film was formed on the obtained film under the same conditions as in Example 1. Elemental analysis by EDS confirmed that Ga 2 O 3 .
[0129] (Comparative Example)
[0130] The film formation and evaluation were performed under the same conditions as in Example 1 except that c-plane sapphire was used as the crystalline substrate. 2 O 3 The peak of α-Ga 2 O 3 After annealing the obtained gallium oxide film at 600°C for 3 hours, the crystal structure of the film changed and β-Ga 2 O 3 The peak.
[0131] Examples 1 to 7 not only have low film formation temperatures, but also produce β-Ga films with good crystallinity. 2 O 3 membrane. β-Ga 2 O 3 It is thermally stable and can be used in semiconductor devices.
[0132] (Example 9)
[0133] The gallium oxide film obtained by the same method as in Example 1 was annealed in air at 600°C for 3 hours, and the film density before and after the annealing was compared. 3 The film density after annealing is 5.89 g / cm 3, and the film density was confirmed to have increased. In addition, the film density was estimated by X-ray reflectivity method. Further, annealing treatment was performed at 1000°C for 1 hour, and the result confirmed that the film density further increased to 6.02 g / cm 3 This is considered to be the result of obtaining a higher quality film by removing unreacted species in the film. As a result, a higher quality semiconductor device can be manufactured.
[0134] The present invention is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any technical solution having substantially the same structure and having the same function and effect as the technical concept described in the claims of the present invention is included in the protection scope of the present invention.
Claims
1. A stacked structure comprising a crystalline substrate and a crystalline oxide film having gallium as a main component and having a β-gallia structure, wherein: The crystalline substrate is a crystalline substrate containing lithium tantalate as a main component.
2. The laminated structure according to claim 1, characterized in that The crystalline substrate is a lithium tantalate single crystal substrate.
3. The laminated structure according to claim 1, characterized in that The crystalline oxide film contains β-Ga2O3 as a main component.
4. The laminated structure according to claim 2, characterized in that The crystalline oxide film contains β-Ga2O3 as a main component.
5. The laminated structure according to any one of claims 1 to 4, characterized in that The crystalline oxide film has a thickness of 1 μm or more.
6. The laminated structure according to any one of claims 1 to 4, characterized in that The area of the crystalline oxide film is 100 mm 2 above.
7. The laminated structure according to claim 5, characterized in that The area of the crystalline oxide film is 100 mm 2 above.
8. A method for producing a laminated structure, comprising: conveying a mist generated by atomizing or dropletizing an aqueous solution containing at least gallium to a substrate using a carrier gas, and causing the mist to undergo a thermal reaction on the substrate to produce a crystalline oxide film having gallium as a main component and having a β-gallia structure, wherein the method for producing a laminated structure is characterized in that: As the substrate, a crystalline substrate containing lithium tantalate as a main component is used.
9. The method for producing a laminated structure according to claim 8, characterized in that: A lithium tantalate single crystal substrate was used as the crystalline substrate.
10. The method for producing a laminated structure according to claim 8, wherein: The temperature of the thermal reaction is set to 250 to 900°C.
11. The method for producing a laminated structure according to claim 9, wherein: The temperature of the thermal reaction is set to 250 to 900°C.
12. The method for manufacturing a laminated structure according to claim 8, characterized in that: The crystalline oxide film contains β-Ga2O3 as a main component.
13. The method for manufacturing a laminated structure according to claim 9, characterized in that: The crystalline oxide film contains β-Ga2O3 as a main component.
14. The method for producing a laminated structure according to claim 10, wherein: The crystalline oxide film contains β-Ga2O3 as a main component.
15. The method for producing a laminated structure according to claim 11, wherein: The crystalline oxide film contains β-Ga2O3 as a main component.
16. The method for producing a laminated structure according to any one of claims 8 to 15, characterized in that: The crystalline oxide film has a thickness of 1 μm or more.
17. The method for producing a laminated structure according to any one of claims 8 to 15, characterized in that: The film-forming surface area is 100mm 2 The above substrate is used as the substrate.
18. A method for manufacturing a laminated structure, characterized in that: The laminated structure produced by the method according to any one of claims 8 to 15 is heat treated at 600 to 1000°C.
Citation Information
Patent Citations
SUBSTRATE WITH ??-Ga2O3 SINGLE CRYSTAL FILM AND ITS MANUFACTURING METHOD
JP2014015366A
Semiconductor device and crystal
JP2014072463A
GROWTH METHOD OF &bgr;-Ga2O3-BASED SINGLE CRYSTAL FILM AND CRYSTAL LAMINATE STRUCTURE
JP2015091740A
Method of manufacturing crystalline laminate structure, and semiconductor device
JP2016064961A
Crystalline semiconductor film, lamination structure, and semiconductor device