A method for testing the conductivity of a lithium-ion battery conductive paste
By replacing lithium iron phosphate with calcium carbonate, the fluctuations, low accuracy and high cost in the resistance measurement of conductive paste of lithium-ion batteries are solved, and more accurate and economical resistivity testing is achieved, reducing environmental pollution.
Patent Information
- Application Number
- CN202111619882.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-27
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2041-12-27
AI Technical Summary
In the prior art, the resistivity measurement of conductive paste of lithium-ion batteries has problems such as large fluctuations, low accuracy and high cost. In particular, the resistivity fluctuations of lithium iron phosphate materials affect the accuracy of the conductivity test, and the market price is high and Severe environmental pollution.
Calcium carbonate instead of lithium iron phosphate as the intermediate material. By formulating calcium carbonate, PVDF and conductive paste into a mixed slurry with solvent in a specific proportion, coated on the PET film and dried and sliced to test the resistivity, reducing the resistivity volatility affects and reduces testing costs and environmental pollution.
It effectively eliminates the impact of resistivity fluctuations in lithium iron phosphate on the test results, reduces resistivity testing costs, reduces environmental pollution, and improves the accuracy and economicality of the test.
Smart Images

Figure CN114324490B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium ion batteries, and in particular to a method for testing the conductivity of a lithium ion battery conductive paste. Background Art
[0002] The electrodes of lithium-ion batteries are mainly composed of current collector aluminum foil and electrode slurry coated on the aluminum foil, and the conductivity of the electrode slurry is an important indicator for evaluating electrode performance. Conductivity refers to the ability of an object to conduct electric current. The conductivity of each part of the material in the battery will affect the performance of the battery in different aspects, such as the internal resistance and discharge heat of the battery. Among them, the conductivity of the battery slurry is directly related to the battery capacity and the size of the rate performance. Generally speaking, the higher the conductivity of the electrode slurry, the better its conductivity, the more conducive it is to reducing the polarization of the electrode, and accordingly, the better the large current charge and discharge capacity of the electrode. The conductivity of the electrode slurry is generally evaluated by measuring the conductivity of the slurry.
[0003] At present, the resistivity test of the conductive paste of battery materials basically adopts 96% positive electrode material lithium iron phosphate LFP, 3% polyvinylidene fluoride PVDF, 1% conductive paste and a small amount of N-methylpyrrolidone to mix evenly into battery paste, and the coated aluminum foil or PET film is dried to test the resistivity. China's public patent CN108519407A discloses a method for evaluating the dispersibility of lithium-ion battery conductive paste, the conductive paste is mixed with active material, conductive agent and binder according to the weight ratio of 90:6:6; the positive electrode active material includes: lithium iron phosphate, lithium manganese iron phosphate, nickel cobalt manganese ternary material and lithium cobalt oxide material, and the negative electrode active material includes graphite, lithium titanate and silicon-based negative electrode. China's public patent CN108303592A discloses a method for testing the conductivity of the electrode layer of a lithium-ion battery, wherein the positive electrode slurry of different proportions of lithium iron phosphate, conductive agent, binder, and solvent is evenly coated on a clean polypropylene film; China's public patent CN108226641A discloses a method for testing the conductivity of positive electrode materials of lithium-ion batteries, wherein the positive electrode active material, conductive agent, binder, and solvent are mixed in a stirring tank, stirred, and mixed to obtain positive electrode slurry; the above method has the disadvantage that the resistivity of positive electrode materials such as lithium iron phosphate fluctuates greatly, which affects the accuracy of the resistivity value of the conductive slurry. The resistivity of lithium iron phosphate LFP on the market is currently 20 to 200Ω.cm; the testing cost is high, the market value of lithium iron phosphate LFP materials is 50,000 to 150,000 yuan / ton, and the environmental pollution is large. Summary of the invention
[0004] The invention provides a method for testing the conductivity of a lithium ion battery conductive paste, which solves the problems of large resistivity measurement fluctuation, low resistivity value accuracy and high cost in the prior art.
[0005] In order to solve this technical problem, the present invention provides the following technical solution:
[0006] A method for testing the conductivity of a lithium-ion battery conductive paste comprises the following steps:
[0007] S1, preparing a mixed slurry with a solvent at a ratio of 94-96:3-5:1 of calcium carbonate, PVDF and conductive slurry;
[0008] S2, evenly coating the mixed slurry onto the PET film;
[0009] S3, drying the PET film coated with the mixed slurry, slicing it and testing its resistivity.
[0010] As one of the main materials of positive electrode materials, lithium iron phosphate needs to add a small amount of conductive slurry to enhance its conductivity due to its poor conductivity. The addition amount is generally between 0.5 and 2%. If the addition amount is too small, the conductivity is poor, and if the addition amount is large, the battery energy density is low. Compared with the prior art that uses lithium iron phosphate and other electrode materials as test materials, this scheme uses calcium carbonate as an intermediate material to replace lithium iron phosphate to test the resistivity of the conductive slurry. The calcium carbonate used in this scheme is not conductive, eliminating the influence of the resistivity fluctuation of the auxiliary material on the sample test results. At the same time, the market value of lithium iron phosphate LFP material is 50,000 to 150,000 yuan / ton, and the cost of calcium carbonate is 2,000 to 3,000 yuan / ton. The method of this scheme can reduce the cost of resistivity testing and reduce environmental pollution. The amount of calcium carbonate added when testing the resistivity of the conductive slurry can refer to the approximate proportion of battery production. This scheme can adjust the proportion of conductive agent addition.
[0011] Preferably, the solvent is N-methylpyrrolidone.
[0012] Preferably, the solid content of the mixed slurry is 40-50%.
[0013] Preferably, the conductive paste includes any one of conductive carbon black SP, carbon nanotubes or KS-6, or a combination of at least two of them.
[0014] Preferably, the calcium carbonate is preferably 2000 mesh calcium carbonate.
[0015] Preferably, the ratio of calcium carbonate, PVDF and conductive agent is 95:4:1.
[0016] Preferably, the solid content of the mixed slurry is 45%.
[0017] Compared with the prior art, the present invention has the following advantages:
[0018] The 2000 mesh calcium carbonate in this solution replaces lithium iron phosphate to eliminate the influence of resistivity fluctuation of the positive electrode material lithium iron phosphate LFP on the sample test results; at the same time, it reduces the resistivity test cost and reduces environmental pollution. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The drawings described herein are used to provide a further understanding of the embodiments of the present invention, constitute a part of this application, and do not constitute a limitation of the embodiments of the present invention. In the drawings:
[0020] Figure 1 This is a schematic diagram of the preparation of the conductive slurry for lithium-ion batteries of the present invention. DETAILED DESCRIPTION
[0021] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments. The illustrative embodiments of the present invention and their description are only used to explain the present invention and are not intended to limit the present invention.
[0022] Example 1
[0023] Add 1% conductive slurry (calculated according to the content of conductive agent SP) to a clean 200ml beaker, then add 4% PVDF solution, stir with a stirrer at 500rpm for 30min, slowly add 95% 2000 mesh calcium carbonate, and then add an appropriate amount of NMP to prepare a mixture with a total weight of 80g and a total solid content of about 45%, and stir with a stirrer at 900rpm for another 120min. After stirring, apply the mixed slurry on a PET film, dry, slice, and test with a resistivity meter. The test results are shown in Table 1.
[0024] Example 2
[0025] Add 1% conductive slurry (calculated according to the content of conductive agent SP) to a clean 200ml beaker, then add 3% PVDF solution, stir with a stirrer at 500rpm for 30min, slowly add 96% 2000 mesh calcium carbonate, and then add an appropriate amount of NMP to prepare a mixture with a total weight of 80g and a total solid content of about 40%, and stir with a stirrer at 900rpm for another 120min. After stirring, apply the mixed slurry on a PET film, dry, slice, and test with a resistivity meter. The test results are shown in Table 1.
[0026] Example 3
[0027] Add 1% conductive slurry (calculated according to the content of conductive agent SP) to a clean 200ml beaker, then add 6% PVDF solution, stir with a stirrer at 500rpm for 30min, slowly add 93% 2000 mesh calcium carbonate, and then add an appropriate amount of NMP to prepare a mixture with a total weight of 80g and a total solid content of about 50%, and stir with a stirrer at 900rpm for another 120min. After stirring, apply the mixed slurry on a PET film, dry, slice, and test with a resistivity meter. The test results are shown in Table 1.
[0028] Comparative Example 1
[0029] Add 1% conductive slurry (calculated according to the content of conductive agent SP) to a clean 200ml beaker, then add 4% PVDF solution, stir with a stirrer at 500rpm for 30min, slowly add 95% lithium iron phosphate LFP, and then add an appropriate amount of NMP to prepare a mixture with a total weight of 80g and a total solid content of about 45%, and stir with a stirrer at 900rpm for another 120min. After stirring, apply the mixed slurry on a PET film, dry, slice, and test with a resistivity meter. The test results are shown in Table 1.
[0030] Comparative Example 2
[0031] Add 1% conductive slurry (calculated according to the content of conductive agent SP) to a clean 200ml beaker, then add 3% PVDF solution, stir with a stirrer at 500rpm for 30min, slowly add 96% lithium iron phosphate LFP, and then add an appropriate amount of NMP to prepare a mixture with a total weight of 80g and a total solid content of about 40%, and stir with a stirrer at 900rpm for another 120min. After stirring, apply the mixed slurry on a PET film, dry, slice, and test with a resistivity meter. The test results are shown in Table 1.
[0032] Comparative Example 3
[0033] Add 1% conductive slurry (calculated according to the content of conductive agent SP) to a clean 200ml beaker, then add 6% PVDF solution, stir with a stirrer at 500rpm for 30min, slowly add 93% lithium iron phosphate LFP, and then add an appropriate amount of NMP to prepare a mixture with a total weight of 80g and a total solid content of about 50%, and stir with a stirrer at 900rpm for another 120min. After stirring, apply the mixed slurry on a PET film, dry, slice, and test with a resistivity meter. The test results are shown in Table 1.
[0034] The resistivity (Ω.cm) of the mixed slurry obtained by testing calcium carbonate and lithium iron phosphate in Example 1-3 and Comparative Example 1-3 was measured using the enterprise standard and RTS-8 four-probe tester. The specific operation steps are:
[0035] 1. Cutting: Put the sample to be tested into the cutting machine, press the cutting machine to cut out a disc with a diameter of 40mm, hold the disc with tweezers and measure the thickness of the disc on the micrometer;
[0036] 2. Place the sample: Place the disc in the center of the test bench and unscrew the probe head to press the disc tightly;
[0037] 3. Input sample information: input temperature and humidity, wafer identification, thickness, diameter in the upper left corner of the software main interface, select the appropriate current range (usually 100uA), the average probe spacing is 3.8mm, and the probe spacing correction factor is 1mm;
[0038] 4. Measure: Click "Measure" in the upper right corner, adjust the current value of the instrument host according to the current value on the pop-up interface until the two are consistent, click "OK", and the instrument starts testing;
[0039] 5. Record: After the test is completed, record the resistivity value in the test data.
[0040] The measurement data are shown in Table 1 below.
[0041] Table 1
[0042]
[0043] Compared with the prior art using lithium iron phosphate electrode material as the test material, the resistivity of the conductive paste tested using calcium carbonate as the intermediate material is significantly increased; after conversion, the influence of resistivity fluctuations of the auxiliary material lithium iron phosphate on the sample test results can be eliminated.
[0044] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for testing the conductivity of a lithium-ion battery conductive paste, characterized in that: The steps include: S1, preparing a mixed slurry with a solvent at a ratio of 94-96:3-5:1 of calcium carbonate, PVDF and conductive slurry; S2, evenly coating the mixed slurry onto the PET film; S3, drying the PET film coated with the mixed slurry, slicing and testing the resistivity; The solvent is N-methylpyrrolidone; The solid content of the mixed slurry is 40-50%.
2. The method for testing the conductivity of a lithium-ion battery conductive paste according to claim 1, characterized in that: The conductive paste includes any one of conductive carbon black SP, carbon nanotubes or KS-6 or a combination of at least two thereof.
3. The method for testing the conductivity of a lithium-ion battery conductive paste according to claim 1, characterized in that: The calcium carbonate is 2000 mesh calcium carbonate.
4. The method for testing the conductivity of a lithium-ion battery conductive paste according to claim 1, characterized in that: The ratio of calcium carbonate, PVDF and conductive paste is 95:4:
1.
5. The method for testing the conductivity of a lithium-ion battery conductive paste according to claim 1, characterized in that: The solid content of the mixed slurry is 45%.
Citation Information
Patent Citations
Method for testing electrical conductivity of cathode material used for lithium ion battery
CN108226641A
Method for testing conductivity of pole piece dressing layer of lithium ion battery
CN108303592A
Method for evaluating dispersibility of conductive paste of lithium ion battery
CN108519407A
Cited By
Electrode slurry evaluation method and system based on DRT analysis, and memory
CN120668735A