Modified aromatic hydrocarbon formaldehyde resin, waterborne epoxy resin composition and cured product thereof
By reacting the aromatic hydrocarbon formaldehyde resin with polyether monohydric alcohol or polyether polyol to form a modified resin, the shortcomings of the use of aromatic hydrocarbon formaldehyde resin in water system in terms of water resistance and adhesion are solved, and emulsification stability is achieved and Excellent properties of cured substances.
Patent Information
- Application Number
- CN202080059897.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-08-27
- Filing Date
- 2020-08-19
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-08-19
AI Technical Summary
The aromatic hydrocarbon formaldehyde resins used in existing water systems have shortcomings in water resistance, adhesion and emulsification stability, and the addition of commercially available surfactants will impair these characteristics.
By reacting the aromatic hydrocarbon formaldehyde resin with polyether monohydric alcohol or polyether polyhydric alcohol, a modified aromatic hydrocarbon formaldehyde resin is formed, and the use of commercially available surfactants is avoided, and emulsification stability and water resistance are improved.
The modified aromatic hydrocarbon formaldehyde resin has been achieved with excellent emulsification effect, and the water resistance, corrosion resistance and adhesion of the aqueous epoxy resin composition and cured substances contained therein are significantly improved.
Smart Images

Figure BDA0003517976290000131 
Figure BDA0003517976290000171 
Figure BDA0003517976290000181
Abstract
Description
Technical Field
[0001] The invention relates to a modified aromatic hydrocarbon formaldehyde resin, a waterborne epoxy resin composition and a cured product thereof. Background Art
[0002] In order to improve the water resistance, corrosion resistance, adhesion and other properties of resins such as acrylic resins, polyurethane resins and epoxy resins, aromatic hydrocarbon formaldehyde resins are widely used as non-reactive modifiers and reactive modifiers (Patent Document 1). In recent years, due to the danger of fire and the impact on the human body, the use of solvents has been increasingly strictly regulated. Therefore, it is desired to develop aromatic hydrocarbon formaldehyde resins that can be used in water (Patent Document 2).
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Laid-Open No. 61-228013
[0006] Patent Document 2: Japanese Patent Application Publication No. 2001-261815 Summary of the invention
[0007] Problem that the invention aims to solve
[0008] For aromatic hydrocarbon formaldehyde resins that can be used in water systems, it is necessary to further improve water resistance and adhesion. In addition, when a commercially available surfactant is added to improve emulsion stability, there is a concern that water resistance, corrosion resistance and adhesion are impaired. In view of this concern, it is desired to have a modified aromatic hydrocarbon formaldehyde resin with emulsification performance without using a commercially available surfactant.
[0009] Solutions for solving problems
[0010] The present inventors have conducted intensive studies and have found that the above-mentioned problems can be solved by modifying an aromatic hydrocarbon formaldehyde resin with a polyether monool or a polyether polyol, thereby completing the present invention.
[0011] [1] A modified aromatic hydrocarbon formaldehyde resin obtained by reacting an aromatic hydrocarbon formaldehyde resin with a polyether monool or a polyether polyol.
[0012] [2] The modified aromatic hydrocarbon formaldehyde resin according to [1] above, wherein the aromatic hydrocarbon is at least one selected from the group consisting of toluene, xylene, mesitylene and pseudocumene.
[0013] [3] The modified aromatic hydrocarbon formaldehyde resin according to [1] or [2], wherein the polyether monool or polyether polyol is an ethylene oxide adduct or an oxetane adduct of a monool or polyol having 1 to 20 carbon atoms.
[0014] [4] The modified aromatic hydrocarbon formaldehyde resin according to any one of [1] to [3] above, wherein the polyether monool or polyether polyol is at least one selected from the group consisting of polyoxyethylene monomethyl ether, polyethylene glycol, polyoxyethylene glycerol ether, polyoxyethylene trimethylolpropane ether, polyoxyethylene neopentyl glycol ether and polyoxyethylene pentaerythritol ether.
[0015] [5] The modified aromatic hydrocarbon formaldehyde resin according to any one of [1] to [4] above, wherein the weight average molecular weight of the polyether monool or polyether polyol is 450 to 50,000.
[0016] [6] The modified aromatic hydrocarbon formaldehyde resin according to any one of [1] to [5] above, wherein the weight average molecular weight of the polyether monool or polyether polyol is 750 to 25,000.
[0017] [7] The modified aromatic hydrocarbon formaldehyde resin according to any one of [1] to [6] above, wherein the weight average molecular weight of the polyether monool or polyether polyol is 1,100 to 14,000.
[0018] [8] The modified aromatic hydrocarbon formaldehyde resin according to any one of [1] to [7] above, which is obtained by reacting 100 parts by mass of the aromatic hydrocarbon formaldehyde resin with 10 to 990 parts by mass of a polyether monool or a polyether polyol.
[0019] [9] The modified aromatic hydrocarbon formaldehyde resin according to [8] above, which is obtained by reacting 30 to 900 parts by mass of a polyether monool or a polyether polyol with 100 parts by mass of the aromatic hydrocarbon formaldehyde resin.
[0020]
[10] The modified aromatic hydrocarbon formaldehyde resin according to any one of [1] to [9] above, wherein the weight average molecular weight of the modified aromatic hydrocarbon formaldehyde resin is 300 to 100,000.
[0021]
[11] An aqueous epoxy resin composition comprising the modified aromatic hydrocarbon formaldehyde resin (A) according to any one of [1] to
[10] above, an epoxy resin (B), and an aqueous medium (C).
[0022]
[12] The water-based epoxy resin composition according to
[11] above, wherein the content of the modified aromatic hydrocarbon formaldehyde resin (A) is 0.01 to 30 parts by mass based on 100 parts by mass of the epoxy resin (B).
[0023]
[13] A cured product obtained by curing the water-based epoxy resin composition described in
[11] or
[12] .
[0024] Effects of the Invention
[0025] According to the present invention, a modified aromatic hydrocarbon formaldehyde resin having excellent emulsification, an aqueous epoxy resin composition containing the resin, and a cured product thereof having excellent water resistance, corrosion resistance and adhesion can be obtained. DETAILED DESCRIPTION
[0026] Hereinafter, a scheme for implementing the present invention (hereinafter referred to as "this embodiment") is described in detail. The following embodiment is an example for illustrating the present invention and is not intended to limit the present invention to this embodiment. The present invention can be appropriately modified and implemented within the scope of its main purpose. In this specification, preferred limitations can be arbitrarily adopted, and more preferably, a combination of preferred limitations. In this specification, the recorded meaning of "XX to YY" is "above XX and below YY".
[0027] <Aromatic hydrocarbon formaldehyde resin>
[0028] Aromatic hydrocarbon formaldehyde resin is obtained by reacting aromatic hydrocarbon with formaldehyde. As aromatic hydrocarbon, at least one selected from the group consisting of benzene, toluene, xylene, mesitylene, pseudocumene, ethylbenzene, propylbenzene, decylbenzene, cyclohexylbenzene, biphenyl, methylbiphenyl, naphthalene, methylnaphthalene, dimethylnaphthalene, ethylnaphthalene, anthracene, methylanthracene, dimethylanthracene, ethylanthracene and binaphthyl can be cited. From the viewpoint of giving better flexibility and adhesion, water resistance and corrosion resistance to the cured product formed by curing the aqueous epoxy resin composition containing the resin, at least one selected from the group consisting of xylene, toluene, mesitylene and pseudocumene is preferred, xylene is more preferred, and m-xylene is further preferred. From the same viewpoint as above, the aromatic hydrocarbon formaldehyde resin preferably includes: at least one selected from the group consisting of xylene formaldehyde resin obtained by reacting xylene with formaldehyde, toluene formaldehyde resin obtained by reacting toluene with formaldehyde and mesitylene formaldehyde resin obtained by reacting mesitylene with formaldehyde, more preferably including xylene formaldehyde resin.
[0029] Aromatic hydrocarbon formaldehyde resins can be commercially available or prepared by known methods. Commercially available products include, for example, xylene resins "NIKANOL Y-100", "NIKANOL Y-300", "NIKANOLLLL" and "NIKANOL H" manufactured by Fudow Co., Ltd. Known methods include, for example, methods described in Japanese Patent Publication No. 37-5747, in which aromatic hydrocarbons and formaldehyde are subjected to a condensation reaction in the presence of a catalyst.
[0030] The weight average molecular weight (Mw) of the aromatic hydrocarbon formaldehyde resin is preferably 200 to 10,000, more preferably 300 to 2,000, further preferably 350 to 1,500, and further preferably 500 to 1,000 in terms of polystyrene. The Mw of the aromatic hydrocarbon formaldehyde resin is preferably within the above range because it can sufficiently maintain compatibility with other resin components when the composition is prepared. The weight average molecular weight (Mw) can be measured by the method described in the examples of the present application using gel filtration chromatography (GPC).
[0031] <Polyether monool or polyether polyol>
[0032] The polyether monool or polyether polyol is not particularly limited, and examples thereof include ethylene oxide adducts or oxetane adducts of monools or polyols having 1 to 20 carbon atoms. The ethylene oxide adducts or oxetane adducts of monools or polyols have a carbon number of more preferably 1 to 10, and even more preferably 1 to 5.
[0033] As monohydric alcohol or polyhydric alcohol having 1 to 20 carbon atoms, aliphatic monohydric alcohol or polyhydric alcohol such as methanol, ethanol, ethylene glycol, polyethylene glycol, propylene glycol, polypropylene glycol, trimethylolpropane, neopentyl glycol, or aromatic monohydric alcohol or polyhydric alcohol such as phenol, cresol, butylphenol, nonylphenol, etc. can be used. Among the above monohydric alcohol or polyhydric alcohol, aliphatic polyhydric alcohol is preferred. The aliphatic polyol is not particularly limited, and examples thereof include trimethylolpropane, neopentyl glycol, ethylene glycol esters, spirodiol, pentaerythritol, ethylene glycol, diethylene glycol, dipropylene glycol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 2,5-hexanediol, 1,2-hexanediol, trimethylolethane, 1,2-octanediol, 1,10-decanediol, 3-hexyne-2,5-diol, 2,5-dimethyl-3-hexyne-2,5-diol, 2,2,4-trimethyl-1,3-pentanediol, polyethylene glycol, and polyoxypropylene glycol. Among these, at least one selected from the group consisting of ethylene glycol, propylene glycol, glycerol, trimethylolpropane, and neopentyl glycol is preferred, ethylene glycol or glycerol is more preferred, and ethylene glycol is further preferred. These monohydric alcohols or polyhydric alcohols may be used alone or in combination of two or more.
[0034] Polyether monool or polyether polyol refers to a compound formed by adding ethylene oxide or oxetane to the above-mentioned monool or polyol, more preferably a compound with ethylene oxide added thereto, and there is no particular limitation as long as this condition is met. As a specific polyether monool or polyether polyol, at least one selected from the group consisting of polyoxyethylene monomethyl ether, polyethylene glycol, polyoxyethylene glycerol ether, polyoxyethylene trimethylol propane ether, polyoxyethylene neopentyl glycol ether and polyoxyethylene pentaerythritol ether can be cited. Among them, from the viewpoint of ease of acquisition, polyethylene glycol or polyoxyethylene glycerol ether is more preferably used, and polyethylene glycol is further preferably used. These polyether monools or polyether polyols can be used alone or in combination of two or more.
[0035] The weight average molecular weight (Mw) of the above-mentioned polyether monool or polyether polyol is preferably in the range of 450 to 50,000 in terms of polystyrene. The weight average molecular weight of the polyether monool or polyether polyol can be measured by the GPC method and by the method described in the examples of the present application. When the weight average molecular weight of the polyether monool or polyether polyol is in the above range, the static stability of the composition emulsion containing the aqueous medium, other resins and the modified aromatic hydrocarbon formaldehyde resin is excellent.
[0036] The weight average molecular weight of the polyether monool or polyether polyol is more preferably 750 to 25,000, and even more preferably 1,100 to 14,000, in terms of polystyrene.
[0037] <Modified aromatic hydrocarbon formaldehyde resin>
[0038] The modified aromatic hydrocarbon formaldehyde resin of the present embodiment can be obtained by reacting the above-mentioned aromatic hydrocarbon formaldehyde resin (unmodified) with a polyether monool or a polyether polyol.
[0039] The modified aromatic hydrocarbon formaldehyde resin of the present embodiment uses as a raw material an aromatic hydrocarbon formaldehyde resin whose structure is difficult to identify by analysis. Therefore, it is also difficult to identify the structure of the modified aromatic hydrocarbon formaldehyde resin modified with the adduct described above by analysis.
[0040] The modified aromatic hydrocarbon formaldehyde resin of the present embodiment preferably comprises at least one selected from the group consisting of a polyether monool- or polyether polyol-modified xylene formaldehyde resin, a polyether monool- or polyether polyol-modified toluene formaldehyde resin, and a polyether monool- or polyether polyol-modified mesitylene formaldehyde resin, and more preferably comprises a polyether monool- or polyether polyol-modified xylene formaldehyde resin, from the viewpoint of imparting flexibility to a cured product formed by curing an aqueous epoxy resin composition comprising the resin.
[0041] Specifically, the modified aromatic hydrocarbon formaldehyde resin of the present embodiment can be prepared by adding a polyether monool or a polyether polyol to an aromatic hydrocarbon formaldehyde resin in the presence of an acidic catalyst.
[0042] The acidic catalyst is not particularly limited, and p-toluenesulfonic acid, m-xylenesulfonic acid, or p-toluenesulfonic acid chloride can be used. The reaction temperature of the aromatic hydrocarbon formaldehyde resin and the polyether monool or polyether polyol can be generally 100 to 190° C., preferably 120 to 150° C. The reaction time is not particularly limited, and is, for example, 0.5 to 30 hours, preferably 0.5 to 15 hours.
[0043] When the aromatic hydrocarbon formaldehyde resin is reacted with the polyether monool or polyether polyol, preferably 10 to 990 parts by mass, more preferably 30 to 900 parts by mass of the polyether monool or polyether polyol is reacted with respect to 100 parts by mass of the aromatic hydrocarbon formaldehyde resin. When the amount of the polyether monool or polyether polyol is within the above range, the static stability of the composition emulsion containing the aqueous medium, other resins and the obtained modified aromatic hydrocarbon formaldehyde resin can be well maintained.
[0044] The weight average molecular weight (Mw) of the modified aromatic hydrocarbon formaldehyde resin of the present embodiment is preferably 300 to 100000, more preferably 700 to 30000, and even more preferably 700 to 10000 in terms of polystyrene. The weight average molecular weight can be measured by the method described in Examples of the present application using the GPC method.
[0045] <Waterborne Epoxy Resin Composition>
[0046] The aqueous epoxy resin composition in the present embodiment contains a modified aromatic hydrocarbon formaldehyde resin (A), an epoxy resin (B), and an aqueous medium (C).
[0047] As the modified aromatic hydrocarbon formaldehyde resin (A), the above-mentioned modified aromatic hydrocarbon formaldehyde resin is used.
[0048] The epoxy resin (B) is not particularly limited, and any epoxy resin derived from alicyclic alcohols, epoxy resin derived from aromatic alcohols (phenols), or alicyclic epoxy resins may be used. Specifically, epoxy resins having a glycidyl ether moiety derived from bisphenol A, epoxy resins having a glycidyl ether moiety derived from bisphenol F, and alicyclic aliphatic epoxy resins having an epoxycyclohexyl ring in the molecule may be mentioned. Among these, epoxy resins having a glycidyl ether moiety derived from bisphenol A are particularly preferred from the viewpoint of viscosity and availability.
[0049] In the waterborne epoxy resin composition of the present embodiment, it is preferred that the modified aromatic hydrocarbon formaldehyde resin (A) and the epoxy resin (B) are contained in an amount of 0.01 to 30 parts by mass relative to 100 parts by mass of the epoxy resin (B). If the amount relationship between the two is within the above range, the waterborne epoxy resin composition can be fully cured, and a cured product having sufficient adhesion can be obtained.
[0050] The content of the modified aromatic hydrocarbon formaldehyde resin (A) in the aqueous epoxy resin composition of the present embodiment is more preferably 1 to 25 parts by mass, and further preferably 9 to 20 parts by mass, relative to 100 parts by mass of the epoxy resin (B).
[0051] The aqueous medium (C) is not particularly limited, and known aqueous media such as water and water-soluble organic solvents can be used. As water, ion exchange water, distilled water, tap water and industrial water can be mentioned. As water-soluble organic solvents, alcohols with 1 to 3 carbon atoms (methanol, ethanol and isopropanol, etc.), ketones with 3 to 6 carbon atoms (acetone, methyl ethyl ketone and methyl isobutyl ketone, etc.), ethers with 2 to 6 carbon atoms (dimethyl ether, ethyl cellosolve and butyl cellosolve, etc.) and ether esters with 4 to 6 carbon atoms (butyl cellosolve acetate, etc.) and dimethylformamide can be mentioned. These can also be used in combination of two or more. Among the aqueous media, from the viewpoint of safety, water and a mixed solvent of water and a hydrophilic organic solvent are preferred, and water is more preferred.
[0052] (Other additives)
[0053] In the water-based epoxy resin composition of this embodiment, fillers, plasticizers and other modifying components, reactive or non-reactive diluents, thixotropy-imparting agents and other flow regulating components, pigments and other components, anti-shrinkage agents, flow-spreading agents, defoaming agents, ultraviolet absorbers, preservatives and other additives can be used according to the application, within the range that does not impair the effects of the embodiments of the present invention.
[0054] (Cured product of waterborne epoxy resin composition)
[0055] The cured product of the aqueous epoxy resin composition of the present embodiment can be obtained by known various methods, can be cured at room temperature, and can also be cured by heating. When cured at room temperature, the curing time can be about 1 day to 10 days. The heating conditions are appropriately selected according to the epoxy resin, the components in the composition containing the resin, the resin and the content of each component, preferably selected within the range of 90 minutes to 150 minutes at 60 to 120°C, more preferably selected within the range of 100 minutes to 140 minutes at 70 to 90°C.
[0056] The cured product of the water-based epoxy resin composition of the present embodiment is preferably obtained by adding an epoxy resin curing agent to the above-mentioned water-based epoxy resin composition and reacting the mixture.
[0057] The epoxy resin curing agent is not particularly limited, and for example, amine compounds, polyfunctional phenols, anhydride compounds, amide compounds, etc. can be used. Among these, amine compounds are preferably used from the viewpoint of improving the water resistance, adhesion and corrosion resistance of the cured product of the waterborne epoxy resin composition.
[0058] When an epoxy resin curing agent is used in the water-based epoxy resin composition of the present embodiment, the content of the epoxy resin curing agent is preferably 10 to 300 parts by mass, more preferably 50 to 280 parts by mass, and further preferably 100 to 250 parts by mass relative to 100 parts by mass of the epoxy resin (B). The content of the epoxy resin curing agent within the above range can improve the water resistance, adhesion and corrosion resistance of the cured product of the water-based epoxy resin composition.
[0059] The aqueous epoxy resin composition of the present embodiment contains the modified aromatic hydrocarbon formaldehyde resin (A) having excellent emulsification effect, and therefore has the advantage that the coating film of the obtained cured product is excellent in adhesion, corrosion resistance, flexibility, and hardness.
[0060] Example
[0061] Hereinafter, the present invention will be described in further detail with reference to Examples and Comparative Examples, but the present invention is not limited to these Examples.
[0062] The evaluation methods used in the present examples and comparative examples are as follows.
[0063] (1) Weight average molecular weight (Mw)
[0064] The polystyrene-equivalent weight average molecular weight (Mw) of the aromatic hydrocarbon formaldehyde resin and polyether polyol used in the present example described below, the modified aromatic hydrocarbon formaldehyde resin obtained in the present example, and the resin mixture obtained in the present comparative example was determined by GPC analysis. The apparatus and analysis conditions used in the analysis are as follows.
[0065] Device: Shоdex GPC-101 (manufactured by Showa Denko K.K.)
[0066] Column: Shоdex LF-804×3 (manufactured by Showa Denko K.K.)
[0067] Eluent: Tetrahydrofuran
[0068] Flow rate: 1.0 mL / min.
[0069] Column temperature: 40°C
[0070] Detector: RI (differential refractive index detector)
[0071] (2) Static stability of emulsion
[0072] The obtained emulsion for static stability evaluation was placed in a 50 mL test tube and allowed to stand for 7 days at 23°C. The phase separation of the emulsion was visually observed. The volume of the entire emulsion and the volume of the emulsified phase were measured using a ruler, and the volume ratio (%) of the emulsified phase in the entire emulsion was calculated.
[0073] (Calculation method)
[0074] Volume of emulsified phase / volume of total emulsion × 100 = emulsified phase volume ratio (%)
[0075] (evaluate)
[0076] The volume ratio of the emulsified phase is more than 90%: A
[0077] The emulsified phase volume ratio is less than 90% and more than 80%: B
[0078] The emulsified phase volume ratio is less than 80% and more than 70%: C
[0079] Not emulsified: D
[0080] (3) Erichsen test
[0081] The obtained cured coating film was measured using the following apparatus in accordance with JIS K 5600-5-2:1999.
[0082] Equipment: Erickson film strength tester model HD-4510 (manufactured by Ueshima Manufacturing Co., Ltd.)
[0083] (evaluate)
[0084] When the obtained cured coating film was squeezed by the above-mentioned device, the depth (mm) of cracks in the cured coating film was measured and recorded.
[0085] (4) Adhesion
[0086] The obtained cured coating film was cut into 25 notches at intervals of 1 mm or 2 mm in a grid pattern in accordance with JIS K 5600-5-6:1999, and the adhesion was evaluated.
[0087] (evaluate)
[0088] Evaluation was conducted on a 6-level scale of 0 to 5 in accordance with JIS K 5600-5-6:1999.
[0089] 0: The cut edges are completely smooth and all grids are not peeled off.
[0090] 1: Slight peeling of the coating occurs at the intersection of the cuts. The affected cross-cut portion is significantly greater than 5%.
[0091] 2: The coating peels off along the cut edges and / or at the intersections. The affected cross-cut portion is significantly greater than 5% but not higher than 15%.
[0092] 3: The coating film peels off significantly along the cut edge, partially or entirely, and / or multiple parts of the grid peel off partially or entirely. The affected cross-cut portion is significantly greater than 15% but not higher than 35%.
[0093] 4: The coating of the whole grid peels off significantly along the cut edge, partially or entirely, and / or multiple grids peel off partially or entirely. The affected cross-cut portion does not obviously exceed 35%.
[0094] 5: Any degree of peeling that cannot be classified as category 4.
[0095] (5) Pencil hardness
[0096] The obtained cured coating film was measured in accordance with JIS K 5600-5-4:1999.
[0097] (evaluate)
[0098] The highest pencil hardness at which no scratches were generated on the surface of the obtained cured coating film was recorded as the pencil hardness of the cured coating film.
[0099] (6) Resistance to heavy objects falling
[0100] The measurement was performed in accordance with JIS K 5600-5-3:1999 by dropping a weight onto the surface on which the cured coating film was formed.
[0101] Equipment: No.603 DuPont drop impact tester (manufactured by MYS-TSESTER Company Limited)
[0102] Weight: 1000g
[0103] Impact die and platform: 1 / 4 inch
[0104] Height of heavy objects: 20cm, 30cm, 40cm, 50cm
[0105] (evaluate)
[0106] No cracks or peeling of the coating film were observed: A
[0107] Cracks and peeling of the coating film were confirmed: D
[0108] (7) Specular glossiness
[0109] The 60° specular glossiness of the obtained cured coating film was measured using Elcometer 480 (manufactured by Elcometer Co., Ltd.) in accordance with JIS Z 8741:1997.
[0110] (8) Salt spray test (corrosion resistance)
[0111] The obtained cured coating film was scratched with cross-line notches intersecting at 60° reaching the blank using a cutter, and then tested in accordance with JIS K 5600-7-1:1999.
[0112] Equipment: Salt spray / CASS test machine model STP-90 (manufactured by Suga Test Instruments Co., Ltd.)
[0113] Brine concentration: sodium chloride concentration 50g / L
[0114] Test tank temperature: 35°C
[0115] Exposure time: 680 hours
[0116] (evaluate)
[0117] Rust width: Use a ruler to measure the range of rust caused by notches and scratches.
[0118] Specular gloss after salt spray test: The 60° specular gloss of the cured coating film after the salt spray test was measured by the same method as above.
[0119] It should be noted that the measurement result of the mirror gloss after the salt spray test was used as a standard of water resistance.
[0120] (9) Water resistance (liquid drop method)
[0121] About 0.2 ml of ion exchange water was dripped onto the obtained cured coating film, and the dripped drop was covered with a glass cover, and then left to stand for 24 hours in an atmosphere of 23°C and 50% RH. After that, the drop was wiped off with a clean rag, and then left to stand for 24 hours in an atmosphere of 23°C and 50% RH. After the above operation, the position on the cured coating film that was in contact with the drop was visually observed, and the following evaluation was performed.
[0122] (evaluate)
[0123] No traces of droplets were confirmed on the coating film: A
[0124] Droplet traces were confirmed on the coating film: D
[0125] <Example 1>
[0126] In a reaction vessel with an internal volume of 500 mL equipped with a stirring device, a thermometer, a steam introduction tube, and a distillation port, 234 g (100 parts by mass) of a xylene resin "NIKANOL Y-100" (hydroxyl value: 25 mgKOH / g, weight average molecular weight: 350) manufactured by Fudow Co., Ltd. as an aromatic hydrocarbon formaldehyde resin and 26 g (11 parts by mass) of polyethylene glycol 2000 (manufactured by Kanto Chemical Co., Ltd.) as a polyether polyol were placed, and the mixture was heated to 60° C. and stirred. An acidic catalyst aqueous solution composed of 0.33% (0.87 g) of p-toluenesulfonic acid monohydrate and 2 g of ion-exchanged water based on the total amount of the aromatic hydrocarbon formaldehyde resin and the polyether polyol was added to the reaction vessel, and the temperature was raised to 140° C. over 80 minutes. The solution was kept at 140° C. for 30 minutes, and an alkaline aqueous solution composed of 1.03 g of triethanolamine and 2 g of ion-exchanged water was added to terminate the reaction. Then, the temperature was raised to 150° C., and steam distillation was performed under reduced pressure for 60 minutes, and then water was removed under reduced pressure. The solution was cooled to 80° C. and taken out from the flask to obtain the target polyether polyol-modified aromatic hydrocarbon formaldehyde resin.
[0127] <Examples 2 to 15>
[0128] The reaction was carried out in the same manner as in Example 1 except that the type and charge amount of the aromatic hydrocarbon formaldehyde resin or polyether polyol were changed as shown in Table 1, thereby obtaining a polyether polyol-modified aromatic hydrocarbon formaldehyde resin.
[0129] <Comparative Example 1>
[0130] In a reaction container having an internal volume of 500 mL equipped with a stirring device, a thermometer, a steam inlet pipe, and a distillation outlet, 130 g (100 parts by mass) of a xylene resin "NIKANOL Y-100" (hydroxyl value: 25 mgKOH / g, weight average molecular weight: 350) manufactured by Fudow Co., Ltd. as an aromatic hydrocarbon formaldehyde resin and 130 g (100 parts by mass) of polyethylene glycol 2000 (manufactured by Kanto Chemical Co., Ltd.) as a polyether polyol were added, the temperature was raised to 80° C. and stirred for 30 minutes, and then taken out from the flask to obtain a resin mixture of the polyether polyol and the aromatic hydrocarbon formaldehyde resin.
[0131] <Comparative Example 2>
[0132] In a reaction container having an internal volume of 500 mL equipped with a stirring device, a thermometer, a steam inlet pipe, and a distillation outlet, 130 g (100 parts by mass) of a xylene resin "NIKANOL H" (hydroxyl value: 33 mgKOH / g, weight average molecular weight: 1000) manufactured by Fudow Co., Ltd. as an aromatic hydrocarbon formaldehyde resin and 130 g (100 parts by mass) of polyethylene glycol 2000 (manufactured by Kanto Chemical Co., Ltd.) as a polyether polyol were added, the temperature was raised to 80° C. and stirred for 30 minutes, and then taken out from the flask to obtain a resin mixture of the polyether polyol and the aromatic hydrocarbon formaldehyde resin.
[0133] [Table 1]
[0134]
[0135] <Emulsion for evaluation of static stability (Evaluation of static stability of emulsion)>
[0136] 100 parts by mass of epoxy resin jER1003 (trade name, manufactured by Mitsubishi Chemical Corporation, epoxy equivalent: 700) derived from bisphenol A and having a glycidyl ether portion is dissolved in 50 parts by mass of methyl isobutyl ketone (MIBK) to prepare a base resin. 10.75 parts by mass of the modified aromatic hydrocarbon formaldehyde resin or resin mixture obtained in each embodiment or comparative example is added to 20 parts by mass of the base resin, and 5 parts by mass of ion exchange water is added dropwise while stirring at 1000 rpm using TK HOMO DISPER MODEL2.5 (manufactured by Premix Co., Ltd.), and stirred for 3 minutes. Then, 20 parts by mass of ion exchange water is further prepared and added dropwise while stirring. After temporarily stopping the addition of ion exchange water at the time point when the viscosity of the liquid decreases rapidly, stirring is performed for 3 minutes. After that, the remaining ion exchange water is added and stirred for 1 minute to obtain an emulsion for static stability evaluation. The static stability evaluation of the above-mentioned emulsion is implemented. The results are shown in Table 2.
[0137] <Reference example>
[0138] The modified aromatic hydrocarbon formaldehyde resin or resin mixture obtained in each example or comparative example was replaced with a xylene resin "NIKANOL L5" (hydroxyl value: 35, weight average molecular weight: 1200 (polystyrene conversion)) manufactured by Fudow Co., Ltd., and an emulsion for static stability evaluation of the reference example was obtained in the same manner as described above. The static stability evaluation of the emulsion described above was performed on the emulsion for static stability evaluation of the reference example. The results are shown in Table 2.
[0139] "NIKANOL L5" is a compound in which ethylene oxide is added to a xylene resin, and the average number of moles of the added ethylene oxide is 12.
[0140] [Table 2]
[0141] Table 2
[0142] Static stability of emulsion Example 1 B Example 2 A Example 3 A Example 4 A Example 5 A Example 6 B Example 7 A Example 8 A Example 9 A Example 10 A Embodiment 11 A Example 12 A Embodiment 13 A Embodiment 14 A Embodiment 15 C Comparative Example 1 D Comparative Example 2 D Reference example C
[0143] As shown in Table 2, compared with Examples 1 to 15, no emulsions were produced in Comparative Examples 1 to 2.
[0144] <Examples A to J and Comparative Examples A to D>
[0145] 10 parts by mass of the modified aromatic hydrocarbon formaldehyde resin or resin mixture obtained in the examples or comparative examples described in Tables 3 and 4 were added to 100 parts by mass of epoxy resin (epoxy resin jER828 [trade name, manufactured by Mitsubishi Chemical Corporation, epoxy equivalent: 190] derived from bisphenol A type and having a glycidyl ether portion), and 15 parts by mass of ion exchange water as an aqueous medium (C) was added dropwise while stirring at 1000 rpm, and stirred for 1 minute. Then, 85 parts by mass of ion exchange water were further prepared and added dropwise while stirring. After temporarily stopping the addition of ion exchange water at the time point when the viscosity of the liquid decreased rapidly, stirring was performed for 2 minutes. After that, the remaining ion exchange water was added and stirred for 5 minutes to obtain each aqueous epoxy resin composition described in Tables 3 and 4.
[0146] The obtained water-based epoxy resin compositions, amine epoxy resin curing agents (ARADUR 3986, manufactured by HUNTSMAN), and aqueous solvents (water, butyl cellosolve) were mixed in the mass parts described in the table to obtain curable resin compositions.
[0147] The curable resin composition was applied to a steel plate ("PB-N144" manufactured by PALTEK Co., Ltd., thickness 0.5 mm, 150×70 mm) using an applicator and aged for 7 days in an atmosphere of 23°C and 50% RH to obtain a cured coating film having a thickness of about 40 μm. The obtained cured coating film was subjected to the above evaluation test. The results are shown in Tables 3 and 4.
[0148] <Reference Examples A and B>
[0149] Except that the modified aromatic hydrocarbon formaldehyde resin or resin mixture obtained in the examples or comparative examples was changed to "NIKANOL L5" (hydroxyl value: 35, weight average molecular weight: 1200 (polystyrene conversion)) described in Tables 3 and 4, the water-based epoxy resin composition, curable resin composition and cured coating film described in Tables 3 and 4 were obtained in the same manner as in Examples A to J and Comparative Examples A to D.
[0150] [Table 3]
[0151]
[0152] [Table 4]
[0153]
[0154] Compared with Examples A to J, Comparative Examples A to D did not obtain an aqueous epoxy resin composition in the form of an emulsion, nor did they obtain a cured coating film.
[0155] In addition, when the cured coating films of Reference Examples A and B using the xylene resin "NIKANOL L5" were prepared, they tended to be inferior in pencil hardness, specular glossiness, corrosion resistance, etc., compared with the case of using the modified formaldehyde hydrocarbon resin of the present embodiment.
[0156] <Example K>
[0157] Using TK HOMO DISPER MODEL 2.5 (manufactured by Premix Co., Ltd.), 10.6 parts by mass of the modified aromatic hydrocarbon formaldehyde resin obtained in Example 1 was added dropwise with stirring at 3000 rpm, and 4.0 parts by mass of ion exchanged water as an aqueous medium (C) was stirred for 10 minutes. Then, 2.2 parts by mass of ion exchanged water was added, and after stirring for 5 minutes, this operation was further repeated twice to obtain an emulsion of Example K. A total of 10.6 parts by mass of ion exchanged water as an aqueous medium (C) was added.
[0158] The obtained emulsion was mixed with 100.0 parts by mass of a water-based epoxy resin composition (jER WD1155R55, manufactured by Mitsubishi Chemical Corporation), 69.2 parts by mass of an amine epoxy resin curing agent (jER WD11M60, manufactured by Mitsubishi Chemical Corporation), and 63.4 parts by mass of an aqueous solvent (ion-exchanged water) to obtain a curable resin composition of Example K.
[0159] The curable resin composition was applied onto a steel plate (“PB-N144” manufactured by PALTEK Co., Ltd., thickness 0.5 mm, 150×70 mm) using an applicator and aged for 7 days in an atmosphere of 23° C. and 50% RH to obtain a cured coating film of Example K (thickness about 40 μm).
[0160] <Examples L and M>
[0161] The modified aromatic hydrocarbon formaldehyde resin was changed to the modified aromatic hydrocarbon formaldehyde resin obtained in Example 3 or 4, and the modified aromatic hydrocarbon formaldehyde resin and the xylene resin "NIKANOL H" (hydroxyl value: 33 mgKOH / g, weight average molecular weight: 1000) manufactured by Fudow Co., Ltd. were mixed in the proportions described in Table 5 to prepare an emulsion. Except for this, the emulsions, curable resin compositions and cured coating films of Examples L and M were obtained in the same manner as in Example K.
[0162] <Comparative Example E>
[0163] A curable resin composition and a cured coating film of Comparative Example E were obtained in the same manner as in Example K except that the emulsion was not used.
[0164] The cured coating films obtained in Examples K to M and Comparative Example E were evaluated for the above-mentioned surface glossiness, water resistance (liquid drop method), and pencil hardness. The evaluation results are shown in Table 5.
[0165] [Table 5]
[0166] Table 5
[0167]
[0168] From Table 5, it can be confirmed that Examples K to M are superior in specular gloss and water resistance compared to Comparative Example E in which no emulsion obtained by using the modified formaldehyde hydrocarbon resin according to the present embodiment was added.
Claims
1. A modified aromatic hydrocarbon formaldehyde resin obtained by reacting an aromatic hydrocarbon formaldehyde resin with a polyether monool or a polyether polyol, The polyether monool or polyether polyol is polyethylene glycol, The weight average molecular weight of the polyether monool or polyether polyol is 1100-50000.
2. The modified aromatic hydrocarbon formaldehyde resin according to claim 1, wherein The aromatic hydrocarbon is at least one selected from the group consisting of xylene, toluene, mesitylene and pseudocumene.
3. The modified aromatic hydrocarbon formaldehyde resin according to claim 1 or 2, wherein The weight average molecular weight of the polyether monool or polyether polyol is 1100-25000.
4. The modified aromatic hydrocarbon formaldehyde resin according to claim 1 or 2, wherein The weight average molecular weight of the polyether monool or polyether polyol is 1100-14000. 5 . The modified aromatic hydrocarbon formaldehyde resin according to claim 1 , which is obtained by reacting 10 to 990 parts by mass of a polyether monool or a polyether polyol with 100 parts by mass of the aromatic hydrocarbon formaldehyde resin. 6 . The modified aromatic hydrocarbon formaldehyde resin according to claim 5 , which is obtained by reacting 30 to 900 parts by mass of a polyether monool or a polyether polyol with 100 parts by mass of the aromatic hydrocarbon formaldehyde resin.
7. The modified aromatic hydrocarbon formaldehyde resin according to claim 1 or 2, wherein The weight average molecular weight of the modified aromatic hydrocarbon formaldehyde resin is 300 to 100,000.
8. The modified aromatic hydrocarbon formaldehyde resin according to claim 1 or 2, which is prepared by adding the polyether monool or polyether polyol to the aromatic hydrocarbon formaldehyde resin in the presence of an acidic catalyst. 9 . A water-based epoxy resin composition comprising the modified aromatic hydrocarbon formaldehyde resin (A) according to claim 1 , an epoxy resin (B) and an aqueous medium (C).
10. The waterborne epoxy resin composition according to claim 9, wherein The content of the modified aromatic hydrocarbon formaldehyde resin (A) is 0.01 to 30 parts by mass based on 100 parts by mass of the epoxy resin (B). 11 . A cured product obtained by curing the waterborne epoxy resin composition according to claim 9 or 10.