A composite material delamination damage monitoring method

By arranging matte paint speckles on the surface of the composite structure and using three-dimensional optical measurement equipment, the accuracy problem of composite delamination damage monitoring is solved, the precise positioning of the damage location, size and shape is achieved, providing efficient and automated monitoring methods.

CN114354350BActive Publication Date: 2024-10-29CHINA SPECIAL TYPE FLIER RES INST
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202111593893.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-23
Publication Date
2024-10-29
Estimated Expiration
2041-12-23

AI Technical Summary

Technical Problem

Existing technology is difficult to accurately identify the regional outline and damage extent of delamination damage in composite material structures. Traditional non-destructive testing and built-in sensor methods have great limitations and cannot effectively monitor the expansion of delamination damage in composite materials.

Method used

Matte paint is used to evenly arrange speckle spots on the surface of the composite structure, and three-dimensional optical measurement equipment is used for optical measurement. The initial damage characteristics and damage expansion characteristics of the structure are obtained by applying specific loads and repeated measurements, and the damage location, size and shape are accurately located. .

Benefits of technology

It achieves accurate monitoring of delamination damage and expansion status of composite structures, avoids the complexity of sensor prefabrication and installation, and provides a non-contact, automated, and high-precision damage monitoring method.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114354350B_ABST
    Figure CN114354350B_ABST
Patent Text Reader

Abstract

The present application provides a method for monitoring delamination damage of a composite material, the method comprising: uniformly arranging scattered spots on the surface of a composite material structure with matte paint; applying a specific load to the composite material structure, and performing optical measurement with a three-dimensional optical measurement device; obtaining the initial damage characteristics of the composite material structure; repeatedly applying a specific load to the composite material structure, and performing optical measurement on the composite material structure based on a preset cycle to obtain the expansion characteristics of the delamination damage of the composite material structure; the present application provides a method for monitoring delamination damage of a composite material, which monitors the delamination damage and its expansion state of a composite material structure through three-dimensional optical measurement technology, and accurately determines the location, size, shape and other characteristics of the delamination damage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of aircraft structure health monitoring, and in particular, relates to a composite material delamination damage monitoring method. Background Art

[0002] The proportion of composite materials used is an important indicator of the advancement of contemporary aircraft. As the number of composite materials used in aircraft structures increases and the amount of composite materials used increases, damage monitoring and accurate identification of composite materials are of great significance to the integrity of aircraft structures. Composite material structure delamination damage and its extension are usually difficult to monitor because they occur inside the structure and are highly concealed.

[0003] Currently, the delamination damage and its extension of aircraft composite structures are usually monitored by non-destructive testing or by prefabricating advanced sensors in the structure to measure the structural response.

[0004] However, as a traditional detection method, the applicability of non-destructive testing is restricted by many factors and has great limitations. The built-in sensor monitoring method uses sensor perception or driver to generate excitation - the sensor obtains the structural response. At present, the commonly used sensors for composite material delamination damage monitoring are mainly optical fiber sensors, piezoelectric waveguide sensors, acoustic emission sensors, metal core waveguide fiber sensors, smart coating sensors, etc. After the corresponding algorithms and mechanical modeling technologies, through a large number of optimization algorithms and deep learning, the obtained natural or excitation response signals of the structure are matched with the prefabricated delamination damage characteristics of the structure, and the damage characterization information of the structure is obtained. Combined with the measured results of the structural response, the delamination damage state and extension of the structure can be evaluated and monitored.

[0005] The relative methods in the technology can effectively monitor the location and damage area of ​​layered damage, but cannot accurately and effectively identify the contour of the damaged area and the degree of damage. Summary of the invention

[0006] In order to solve the above technical problems, the present invention provides a composite material delamination damage monitoring method, the method comprising:

[0007] Evenly arrange scattered spots on the surface of the composite structure using matte paint;

[0008] applying a specific load to the composite structure and performing optical measurement using a three-dimensional optical measurement device;

[0009] The initial damage characteristics of the composite material structure are obtained.

[0010] Preferably, after the method of evenly arranging scattered spots on the surface of the composite material structure with matte paint, the method further comprises:

[0011] The three-dimensional optical measurement device is initially calibrated.

[0012] Preferably, the initial calibration of the three-dimensional optical measurement device includes:

[0013] When the composite material structural component is in a free state, the three-dimensional optical measurement device is initially calibrated as an initial value.

[0014] Preferably, the method further comprises:

[0015] A specific load is repeatedly applied to the composite material structure, and optical measurement is performed using the three-dimensional optical measurement device.

[0016] Preferably, the repeatedly applying a specific load to the composite material structure and performing optical measurement using the three-dimensional optical measurement device comprises:

[0017] A specific load is repeatedly applied to the composite material structure, and optical measurements are performed on the composite material structure based on a preset cycle.

[0018] Preferably, after repeatedly applying a specific load to the composite material structure and optically measuring the composite material structure based on a preset cycle, the method further comprises:

[0019] The extension characteristics of the delamination damage of the composite material structure are obtained.

[0020] Preferably, the extension characteristics include the location, size and contour of the delamination damage.

[0021] Preferably, the free state is a state where the composite material structure is not subjected to load.

[0022] Beneficial technical effects of this application:

[0023] The present application provides a composite material delamination damage monitoring method, which monitors the delamination damage and its extension state of the composite material structure through three-dimensional optical measurement technology, and accurately determines the location, size, shape and other characteristics of the delamination damage. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 is a schematic diagram of a structure surface speckle setting provided in an embodiment of the present application;

[0025] Figure 2 This is a schematic diagram of a defective area of ​​a structural component provided in an embodiment of the present application;

[0026] Figure 3 is a schematic diagram of out-of-plane deformation of a delamination defect area provided in an embodiment of the present application;

[0027] Figure 4is a schematic diagram of the damage extension area provided in an embodiment of the present application;

[0028] Figure 5 is a schematic diagram of measurement offset correction provided by an embodiment of the present application;

[0029] Figure 6 is a schematic diagram of three-dimensional optical measurement contour lines provided in an embodiment of the present application;

[0030] Figure 7 It is a damage expansion diagram of a composite structure delamination provided in an embodiment of the present application. DETAILED DESCRIPTION

[0031] This application intends to monitor the delamination damage and its extension status of composite material structures through three-dimensional optical measurement technology, and accurately determine the location, size, shape and other characteristics of the delamination damage. The analysis of the delamination damage and its extension of composite materials in this application is based on the digital image correlation method.

[0032] See also Figure 1-7 ,First, the surface of the composite structure is evenly arranged spots ,on the surface of the composite structure using matt paint, ,e.g. Figure 1 As shown, the three-dimensional optical measurement equipment is initially calibrated; a certain load is applied to the structure and optical measurement is performed, and the initial damage characteristics of the structure are obtained due to the changes in the local structural stiffness and displacement of the structural delamination damage area; as the structure is subjected to repeated loads, the structure is measured at regular intervals to obtain the expansion characteristics of the structural delamination damage.

[0033] Compared with the existing technology of composite material structure delamination damage monitoring, this application has the following advantages:

[0034] 1. No need to prefabricate sensors in the structure, avoiding complicated process flow and avoiding the inability to measure or inaccurate measurement due to damage to the sensor;

[0035] 2. The monitoring area is wide and the position is variable, which is different from the fixed position of the sensor and the limited monitoring area;

[0036] 3. Non-contact measurement, no need to touch the measured object to interfere with the deformation of the measured surface and affect the accuracy of the measurement results, no cumbersome installation, collection, analysis and other processes;

[0037] 4 Directly measure the location, size, degree, contour, etc. of layered damage to form a three-dimensional view. The data processing is simple, and there is no need to pre-calibrate or calibrate the damage through large amounts of data and deep machine learning;

[0038] 5. High measurement automation, simple measurement process and operation.

[0039] Among them, the three-dimensional optical measurement is a non-contact measurement, which characterizes the delamination damage and its extension of the test piece by observing the out-of-plane deformation of the surface defect area of ​​the composite structure when it is subjected to pneumatic pressure, such as Figure 2 As shown in the figure, the circled part is the defect area and the damaged area after the defect expands.

[0040] It should be noted that when the structural member is in a free state (not subject to load), the three-dimensional optical measurement calibration is performed as the initial 0 value. When the structure is subjected to axial compression load, its surface defect area will produce local out-of-plane deformation, such as Figure 3 As shown in the figure, the degree of out-of-plane deformation is characterized by its Z-direction displacement ΔZ (ΔZ=Z-0). The deformation ΔZ0 corresponding to the edge of the initial defect area of ​​the structure is used as the benchmark. When the defect damage expands after N cycles of loading, the area corresponding to the position of the ΔZ0 contour line is the expanded damage area. The longest axial distance L of the damage area at this time is recorded as the damage extension length after N cycles, as shown in Figure 4 shown.

[0041] In one possible implementation, Figure 5 As shown in the figure, during the measurement, due to the load on the structure, there will be a slight overall offset ΔZ on the surface of the test piece during each optical measurement. m , that is, the contour line ΔZ of each measurement i Measured and actual contour ΔZ i There is actually the same small offset ΔZ between m Therefore, the actual value of the damage extension length L and the measured value of L will be different due to the deviation of the contour line. Therefore, ΔZ should be considered when taking the contour line. m The offset can be calculated by measuring the minimum offset value ΔZ of the test piece surface each time. min The change in is used to characterize the contour line after the offset:

[0042] ΔZ i实际 =ΔZ i测量 +ΔZ m

[0043] ΔZ m =ΔZ i-min -ΔZ 0-min

[0044] Where:

[0045] ΔZ i实际 ——Actual displacement contour at the i-th cycle, mm;

[0046] ΔZ i测量 ——displacement contour measured at the i-th cycle, mm;

[0047] ΔZ m——The overall slight deviation of the test piece surface at the i-th cycle, mm;

[0048] ΔZ i-min ——Minimum value of the overall displacement of the test piece surface at the i-th cycle, mm;

[0049] ΔZ 0-min ——Minimum value of the overall displacement of the test piece surface after initial loading, mm.

[0050] Among them, after determining the contour value of each measurement, the major axis distance corresponding to the contour value is taken as the damage extension length L, and the area surrounded by the contour line is the layered damage extension area.

[0051] The present application has been actually applied in the monitoring of delamination damage and extension of composite honeycomb sandwich structures, and has achieved good results. The composite material structure delamination damage extension monitoring result diagram obtained by the method provided in the present application can clearly and unambiguously obtain key parameters such as the location, size, degree, and contour of the delamination damage.

[0052] It should be noted that this application has been applied to multiple subjects and projects, and can effectively and accurately measure the location, size, shape and development status of composite material delamination damage, and has a good effect on monitoring the delamination damage and its extension of composite material structures.

Claims

1. A composite material delamination damage monitoring method, characterized in that: The method comprises: Evenly arrange scattered spots on the surface of the composite structure using matte paint; applying a specific load to the composite structure and performing optical measurement using a three-dimensional optical measurement device; obtaining initial damage characteristics of the composite material structure; Repeatedly applying a specific load to the composite material structure, and optically measuring the composite material structure based on a preset cycle to obtain the extension characteristics of delamination damage of the composite material structure; The step of repeatedly applying a specific load to the composite material structure and optically measuring the composite material structure based on a preset period to obtain the extension characteristics of delamination damage of the composite material structure includes: During the measurement process, due to the load on the structure, there will be a slight overall offset ΔZ on the surface of the test piece during each optical measurement. m , that is, the contour line ΔZ of each measurement i Measured and actual contour ΔZ i There is actually the same small offset ΔZ between m Therefore, the actual value of the damage extension length L and the measured value of L will be different due to the deviation of the contour line. Therefore, ΔZ should be considered when taking the contour line. m The offset is determined by the minimum offset value ΔZ of the test piece surface measured each time. min The change in is used to characterize the contour line after the offset: ΔZ i实际 =ΔZ i测量 +ΔZ m ΔZ m =ΔZ i-min -ΔZ 0-min Where: ΔZ i实际 ——Actual displacement contour at the i-th cycle, mm; ΔZ i测量 ——displacement contour measured at the i-th cycle, mm; ΔZ m ——The overall slight deviation of the test piece surface at the i-th cycle, mm; ΔZ i-min ——Minimum value of the overall displacement of the test piece surface at the i-th cycle, mm; ΔZ 0-min ——Minimum value of the overall displacement of the initial loading test piece surface, mm; After determining the contour value of each measurement, the major axis distance corresponding to the contour value is taken as the damage extension length L, and the area surrounded by the contour is the layered damage extension area; Based on the delamination damage extension area, the extension characteristics of the delamination damage of the composite material structure are determined; wherein the extension characteristics include the location, size and contour of the delamination damage.

2. The method according to claim 1, characterized in that After the method of using matte paint to evenly arrange scattered spots on the surface of the composite material structure, the method further comprises: The three-dimensional optical measurement device is initially calibrated.

3. The method according to claim 2, characterized in that The initial calibration of the three-dimensional optical measurement device includes: When the composite material structural component is in a free state, the three-dimensional optical measurement device is initially calibrated as an initial value.

4. The method according to claim 3, characterized in that The free state is a state in which the composite material structure is not subjected to load.

Citation Information

Patent Citations

  • Fatigue crack expansion test image online acquisition method based on stroboscopic illumination

    CN106338445A

  • Aeroengine damaged blade three-dimensional digital speckle moulding method

    CN106643492A