A method for establishing a numerical prediction model for residual stress in laser melting deposition
Through ABAQUS finite element software and experimental optimization of process parameters, a three-dimensional transient evolution numerical prediction model of laser melting deposition was established, which solved the problem of residual stress in laser melting deposition, achieved accurate prediction of workpiece stress, and reduced workpiece defects and costs.
Patent Information
- Application Number
- CN202210001492.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-04
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-01-04
AI Technical Summary
The residual stress generated in the laser fusion deposition process causes defects such as workpiece deformation and coating cracking, which affects the mechanical properties and forming accuracy of the formed components. It is difficult to obtain the overall three-dimensional stress field distribution in real time with existing technology.
ABAQUS finite element software was used to establish a three-dimensional transient evolution numerical prediction model of the initial laser melting deposition temperature field based on the life and death element method. The melt pool morphology data and process parameters were optimized through experiments, and the process parameters were adjusted to reduce residual stress and an optimized three-dimensional model was established. Model, collect and compare melt pool morphology and stress data in real time, and adjust model parameters to achieve prediction.
It achieves rapid and accurate prediction of the three-dimensional transient evolution of residual stress in laser melting deposition, reduces the occurrence of workpiece defects, improves the mechanical properties and forming accuracy of molded parts, and saves process costs.
Smart Images

Figure CN114386303B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of laser additive manufacturing, and in particular to a method for establishing a numerical prediction model of residual stress in laser melting deposition. Background Art
[0002] Laser melting deposition is a non-contact processing technology that does not require molds and can reduce the number of parts required for the equipment, which can greatly reduce production costs, improve reliability, and shorten the development cycle. At the same time, this technology currently shows good performance in rapid prototyping, coating, tool and part repair, and the design of new alloys or functional gradient materials.
[0003] This technology provides a new technical approach for the manufacture of large and difficult-to-process metal components in aerospace equipment that is fast, flexible, high-performance and low-cost. In recent years, it has become one of the frontier hot research directions in the intersection of advanced manufacturing technology and materials processing engineering, and has received great attention from governments, industries and academia around the world.
[0004] However, the laser melting deposition process still has many shortcomings from the material perspective, including powder spheroidization, poor density, and high residual stress. High residual stress is mainly caused by a very fast cooling rate and a very large temperature gradient caused by a high energy density heat source. Many failures of laser additive manufacturing products, such as stress corrosion and fatigue, are closely related to surface residual stress, which will not only affect the mechanical properties of the molded components, but also affect their forming accuracy, dimensional stability and service life. The residual stress generated during the laser melting deposition process can cause defects such as workpiece deformation and coating cracking, resulting in workpiece repair failure or dimensional deviation and other undesirable problems. At the same time, the residual stress of the coating will affect the mechanical properties of the coating such as corrosion resistance and fatigue strength. Therefore, it is necessary to effectively predict the residual stress generated by the laser melting deposition process in laser additive.
[0005] Under current technical conditions, equipment monitoring can only obtain the stress distribution of the molten pool in real time, but it is often difficult to obtain the overall three-dimensional stress field distribution. The evolution of the molten pool and the overall stress field of the workpiece has an important impact on the quality of the workpiece. Therefore, the use of finite element technology to simulate the three-dimensional transient stress field in the additive process is of great significance for predicting the evolution law of residual stress of components, and will also lay a certain foundation for subsequent research on the mechanical properties and defects of the part forming surface. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a method for establishing a numerical prediction model of residual stress in laser melting deposition, which can quickly and accurately establish a three-dimensional transient evolution prediction model for predicting the residual stress distribution field, which is simple and reliable.
[0007] In order to solve the above technical problems, the present invention provides a method for establishing a numerical prediction model of residual stress in laser melting deposition, comprising the following steps:
[0008] Step 1: Using the birth-death unit method of ABAQUS finite element software, an initial three-dimensional transient evolution numerical prediction model of the laser melting deposition temperature field is established based on the laser melting deposition process parameters; the laser melting deposition process parameters include pulse laser duty cycle, energy density and laser head path planning.
[0009] Step 2: Collect the morphology of the molten pool in the single-pass laser melting deposition experiment, optimize the collected molten pool morphology data, and use the optimized molten pool morphology data to establish an optimized laser melting deposition molten pool three-dimensional model;
[0010] Step 3: Conduct a single-pass laser melting deposition experiment, collect the molten pool morphology online and in real time, and measure the residual stress. Compare the residual stress of the molten pool collected online and in real time through the experiment with the residual stress obtained by the three-dimensional model. If the residual stress is too large or cracks and other defects appear in the molten pool, adjust the parameter settings in the three-dimensional transient evolution numerical prediction model through the relationship between different laser melting deposition process parameters and residual stress, so that the residual stress obtained under the adjusted process parameter combination becomes smaller, that is, the molten pool morphology is improved, and the optimized three-dimensional transient evolution numerical prediction model is obtained at the same time.
[0011] Furthermore, in the step 2, the optimized molten pool morphology data is used to establish an optimized three-dimensional model of the laser melting deposition molten pool. The specific process is: the process parameters are optimized according to the collected molten pool morphology data using the range analysis method to obtain the most suitable operating conditions (suitable factor level combination) corresponding to the minimum residual stress. Based on this factor level combination, i.e. the optimal parameter combination, a three-dimensional model of the laser melting deposition molten pool is established using CAD software.
[0012] Furthermore, the specific process of step three is as follows:
[0013] (1) The energy density and the path planning of the laser head are fixed, and the pulse laser duty cycle is changed to conduct experiments. The molten pool morphology is collected online and in real time, and the residual stress is measured. At the same time, according to the three-dimensional model established in step 2, the residual stress size in the three-dimensional model for the optimization of the laser melting deposition process is obtained. The residual stress size data measured in the experiment are compared with the data obtained from the three-dimensional model, and finally the mechanism of the influence of the change of the pulse laser duty cycle on the residual stress is obtained, and the relationship Q1 between the residual stress and the change of the pulse laser duty cycle is determined; according to the relationship Q1, the pulse laser duty cycle corresponding to the minimum residual stress is recorded.
[0014] (2) The pulse laser duty cycle and the laser head path planning are fixed and the energy density is changed for experiments. The molten pool morphology is collected online and in real time, and the residual stress is measured. At the same time, based on the three-dimensional model established in step 2, the residual stress size in the three-dimensional model for laser melting deposition process optimization is obtained; the residual stress size data measured in the experiment are compared with the data obtained from the three-dimensional model, and finally the mechanism of the influence of the change of energy density on the residual stress is obtained, and the relationship Q2 of the change of residual stress with energy density is determined; according to the relationship Q2, the energy density corresponding to the minimum residual stress is recorded.
[0015] (3) Fix the pulse laser duty cycle and energy density, change the laser head path planning to conduct experiments, record the molten pool morphology and residual stress, and at the same time, based on the three-dimensional model established in step 2, obtain the residual stress size in the three-dimensional model for laser additive manufacturing process optimization; compare the residual stress size data measured in the experiment with the data obtained from the three-dimensional model, and finally obtain the mechanism of the influence of the change of laser head path planning on the residual stress, and determine the relationship Q3 between the change of residual stress and the change of laser head path planning; based on the relationship Q3, record the laser head path planning method corresponding to the minimum residual stress.
[0016] According to the optimal value of each laser melting deposition process parameter determined in steps (1) to (3), the following two laser melting deposition process parameter variables are experimented and optimized:
[0017] (4) While the energy density is fixed, experiments are conducted with different pulse laser duty cycles and laser head path planning, and the molten pool morphology and residual stress are recorded. At the same time, based on the three-dimensional model established in step 2, the residual stress size in the three-dimensional model for laser melting deposition process optimization is obtained. The residual stress size data measured in the experiment are compared with the data obtained from the three-dimensional model, and finally the comprehensive influence mechanism of the pulse laser duty cycle and laser head path planning on the residual stress is obtained when the two factors change, and the comprehensive relationship Q4 of the residual stress changing with the simultaneous change of the pulse laser duty cycle and the laser head path planning is determined. According to the relationship Q4, the pulse laser duty cycle and the laser head path planning method corresponding to the minimum residual stress are recorded.
[0018] (5) The pulse laser duty cycle is fixed and the experiment is carried out with different energy densities and laser head path planning, and the molten pool morphology and residual stress are recorded; at the same time, according to the three-dimensional model established in step 2, the residual stress size in the three-dimensional model for the optimization of the laser melting deposition process is obtained; the residual stress size data measured in the experiment is compared with the data obtained from the three-dimensional model, and finally the comprehensive influence mechanism of the residual stress when the energy density and laser head path planning change, and the comprehensive relationship Q5 of the residual stress changing with the simultaneous change of energy density and laser head path planning is determined; according to the relationship Q5, the energy density size and laser head path planning method corresponding to the minimum residual stress are recorded.
[0019] (6) The laser head path planning is fixed and the experiment is carried out with different pulse laser duty cycles and energy densities, and the molten pool morphology and residual stress are recorded; at the same time, according to the three-dimensional model established in step 2, the residual stress size in the three-dimensional model for the optimization of the laser melting deposition process is obtained; the residual stress size data measured in the experiment is compared with the data obtained from the three-dimensional model, and finally the comprehensive influence mechanism of the pulse laser duty cycle and energy density on the residual stress when the two factors change, is obtained, and the comprehensive relationship Q6 of the residual stress change with the simultaneous change of the pulse laser duty cycle and energy density is determined; according to the relationship Q6, the pulse laser duty cycle and energy density corresponding to the minimum residual stress are recorded.
[0020] According to the pulse laser duty cycle, energy density and laser head path planning method recorded above, the parameters of the three-dimensional transient evolution numerical prediction model established in step one are set, and finally an optimized three-dimensional transient evolution numerical prediction model is obtained.
[0021] Furthermore, in the step 3, the “conducting a single-pass laser melting deposition experiment, collecting the molten pool morphology online and in real time and measuring the residual stress” specifically includes:
[0022] The residual stress of the deposited layer obtained by the blind hole method is tensile stress. The principle is to drill a small hole in the part with residual stress. Because the residual stress near the small hole is released, the residual stress field near the hole area changes. As long as the strain change in the local area is measured, the residual stress value before the release of the drilling can be calculated. When the residual tensile stress is too large, it will reduce the strength and cause process defects such as deformation and cracking of the workpiece during manufacturing; on the other hand, it will reduce the mechanical properties of the material such as fatigue strength and stress corrosion during the natural release process after manufacturing.
[0023] Beneficial effects of the present invention:
[0024] (1) The present invention can establish a numerical prediction model for residual stress in laser melting deposition, and reduce the negative impact of high residual stress on the mechanical properties of the coating by early prediction, especially thermal cracking, warping and other phenomena, which lead to the scrapping of rapid prototyping or repaired parts. The prediction can be achieved before the process, reducing losses and saving costs.
[0025] (2) The present invention collects the molten pool morphology and residual stress in real time. When the residual stress is too high or there are defects such as cracks and warping in the molten pool, the pulse laser duty cycle, energy density or laser head scanning path is changed based on the relationship between the laser melting deposition process parameters and the residual stress, so that the initial three-dimensional transient evolution numerical prediction model of the laser melting deposition temperature field is optimized.
[0026] (3) The present invention uses ABAQUS commercial finite element software to establish a three-dimensional transient evolution numerical prediction model of the laser melting deposition temperature field, and performs predictive calculations on the laser melting deposition process. It can explore the evolution law of the stress field in the molten pool processing process in laser melting deposition, and predict the residual stress distribution and thermal deformation of the workpiece in different directions. It can not only achieve the purpose of prediction, but also be simple and reliable, greatly saving process costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a schematic diagram of the process of the present invention;
[0028] Figure 2 The present invention provides a schematic diagram of the structure of a real-time morphology data acquisition device and a single-channel laser melting deposition experiment using the online prediction method for laser melting deposition provided by the present invention.
[0029] The following are marked in the accompanying drawings:
[0030] 1-workpiece; 2-laser head; 3-laser head displacement sensor; 4-infrared pyrometer; 5-CMOS coaxial camera; 6-thermal imager.
[0031] Figure 3 The residual stress distribution along the path perpendicular to the scanning direction predicted by the optimized three-dimensional transient evolution numerical prediction model. DETAILED DESCRIPTION
[0032] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0033] Reference Figure 1As shown, the present invention discloses a method for establishing a numerical prediction model of residual stress in laser melting deposition.
[0034] (1) Using ABAQUS finite element software based on the birth-death unit method, the initial three-dimensional transient evolution numerical prediction model of the laser melting deposition temperature field was established. The thermal-mechanical full coupling method was used to calculate the model. The control equations of each module are as follows:
[0035] According to the law of conservation of energy and Fourier's law, the heat conduction equation is derived:
[0036]
[0037] Among them, ρ, k and C p are material density, thermal conductivity and specific heat capacity at constant pressure, respectively. is the heat source term. The boundary condition of the free surface is:
[0038]
[0039] Where n is the free surface normal, T a is the ambient temperature, σ r is the Boltzmann constant, and ε is the surface emissivity of the material.
[0040] Select the three-dimensional spherical heat source model as the heat source:
[0041]
[0042] Where A is the laser absorptivity, a, b, c are the semi-axes of the ellipsoid, and P is the laser power.
[0043] (2) The range analysis method was used to obtain the optimal parameter combination based on historical experimental data (pulse duty cycle of 2, energy density of 100, and Z-shaped scanning path of the laser head) and a single-pass laser melting deposition experiment was conducted. Figure 2 The residual stress of the deposited layer sample was measured by blind hole method and the molten pool morphology of the deposited layer sample was recorded. The measured residual stress was 97MPa. The molten pool morphology data of the deposited layer sample was used to build a three-dimensional model using CAD software.
[0044] (3) Use the orthogonal experimental design method to design the experimental combination of process parameters, as shown in the following table:
[0045]
[0046] The energy density is given by It is calculated that D represents the laser spot diameter; v represents the scanning speed; and P represents the laser power.
[0047] According to the above table, a single-pass laser melting deposition experiment was carried out. Figure 2 The platform shown is used for:
[0048] a. The energy density is fixed at 88.9, the laser head path planning is unchanged in unidirectional scanning mode, the initial pulse laser duty cycle is set to 4, and the residual stress of this group of deposited layer samples measured by the blind hole method is 121MPa (greater than 97MPa). The residual stress increases with the increase of the duty cycle by adjusting the duty cycle. Finally, the residual stress is minimum when the duty cycle is 2.
[0049] b. The pulse laser duty cycle is fixed to 2, the laser head path planning is unchanged in unidirectional scanning mode, the initial energy density is set to 40, and the residual stress of this group of deposited layer samples measured by the blind hole method is 182MPa (greater than 97MPa). The energy density is adjusted and the experiment is carried out. It is found that the residual stress decreases with the increase of energy density. Finally, the residual stress is minimum when the energy density is 46.7.
[0050] c. The energy density is fixed at 46.7, the pulse laser duty cycle is unchanged at 2, the initial laser head path planning is a unidirectional scanning mode, and the residual stress of the deposited layer sample measured by the blind hole method is 134MPa (greater than 97MPa). By changing the laser head path planning and conducting experiments, it is found that the residual stress of the sample obtained under the Z-shaped scanning mode is smaller than the residual stress of the sample obtained under the unidirectional scanning mode.
[0051] d. The energy density is fixed at 46.7, the initial laser head path planning is a Z-shaped scanning mode, and the pulse laser duty cycle is set to 3. The residual stress of this group of deposited layer samples measured by the blind hole method is 124MPa (greater than 97MPa). Experiments were performed by changing the laser head path planning and the pulse laser duty cycle. It was found that the residual stress was the smallest when the Z-shaped scanning mode and the duty cycle were 2.
[0052] e. The pulse laser duty cycle is fixed at 2, the initial laser head path planning is a Z-shaped scanning mode, and the energy density is set to 46.7. The residual stress of this group of deposited layer samples measured by the blind hole method is 108MPa (greater than 97MPa). Experiments by changing the laser head path planning and energy density found that the residual stress is minimum when the Z-shaped scanning mode and energy density are 77.8.
[0053] f. The laser head path planning is fixed to the Z-shaped scanning mode, the initial pulse laser duty cycle is set to 2, the energy density is 77.8, and the residual stress of the deposited layer sample measured by the blind hole method is 101MPa (close to 97MPa). Using the pulse laser duty cycle (2), energy density (77.8), and laser head path planning (Z-shaped scanning mode) recorded by af, the parameters of the three-dimensional transient evolution numerical prediction model established in step 1 are set, and finally the optimized three-dimensional transient evolution numerical prediction model is obtained, as shown in FIG. Figure 3As shown, this prediction model can predict the residual stress distribution along the path perpendicular to the scanning direction.
Claims
1. A method for establishing a numerical prediction model for residual stress in laser melting deposition. It is characterized in that Here are the steps: Step 1: Using the birth-death unit method of ABAQUS finite element software, an initial three-dimensional transient evolution numerical prediction model of the laser melting deposition temperature field is established based on the laser melting deposition process parameters; the laser melting deposition process parameters include pulse laser duty cycle, energy density and laser head path planning; Step 2: Collect the morphology of the molten pool in the single-pass laser melting deposition experiment, optimize the collected molten pool morphology data, and use the optimized molten pool morphology data to establish an optimized laser melting deposition molten pool three-dimensional model; Step three: Conduct a single-pass laser melting deposition experiment, collect the molten pool morphology online and in real time, and measure the residual stress; compare the molten pool residual stress collected online and in real time through the experiment with the residual stress obtained by the three-dimensional model. If the residual stress is too large or cracks and other defects appear in the molten pool, adjust the parameter settings in the three-dimensional transient evolution numerical prediction model through the relationship between different laser melting deposition process parameters and residual stress, so that the residual stress obtained under the adjusted process parameter combination becomes smaller, that is, the molten pool morphology is improved, and the optimized three-dimensional transient evolution numerical prediction model is obtained.
2. The method for establishing a numerical prediction model for residual stress in laser melting deposition according to claim 1, It is characterized in that In the step 2, the optimized molten pool morphology data is used to establish an optimized three-dimensional model of the laser melting deposition molten pool. The specific process is: the process parameters are optimized according to the collected molten pool morphology data using the range analysis method to obtain the most suitable operating conditions corresponding to the minimum residual stress. Based on this factor level combination, that is, the optimal parameter combination, a three-dimensional model of the laser melting deposition molten pool is established using CAD software.
3. A method for establishing a numerical prediction model for residual stress in laser melting deposition according to claim 1 or 2, It is characterized in that The specific process of step three is as follows: (1) The energy density and the path planning of the laser head are fixed, and different pulse laser duty cycles are changed to conduct experiments, and the molten pool morphology is collected online and in real time and the residual stress is measured; at the same time, according to the three-dimensional model established in step 2, the residual stress size in the three-dimensional model for the optimization of the laser melting deposition process is obtained; the residual stress size data measured in the experiment is compared with the data obtained from the three-dimensional model, and finally the mechanism of the influence of the change of the pulse laser duty cycle on the residual stress is obtained, and the relationship Q1 between the residual stress and the change of the pulse laser duty cycle is determined; according to the relationship Q1, the pulse laser duty cycle size corresponding to the minimum residual stress is recorded; (2) The pulse laser duty cycle and the laser head path planning are fixed, and the energy density is changed to conduct experiments, the molten pool morphology is collected online in real time and the residual stress is measured. At the same time, according to the three-dimensional model established in step 2, the residual stress size in the three-dimensional model for the optimization of the laser melting deposition process is obtained; the residual stress size data measured in the experiment is compared with the data obtained from the three-dimensional model, and finally the mechanism of the influence of the change of energy density on the residual stress is obtained, and the relationship Q2 between the change of residual stress and the change of energy density is determined; according to the relationship Q2, the energy density corresponding to the minimum residual stress is recorded; (3) Fix the pulse laser duty cycle and energy density, change the laser head path planning to conduct experiments, record the molten pool morphology and residual stress, and obtain the residual stress size in the three-dimensional model for laser additive manufacturing process optimization based on the three-dimensional model established in step 2; compare the residual stress size data measured in the experiment with the data obtained from the three-dimensional model, and finally obtain the mechanism of the influence of the change of laser head path planning on the residual stress, and determine the relationship Q3 between the change of residual stress and the change of laser head path planning; The laser head path planning method corresponding to the minimum residual stress is recorded according to the relationship Q3; According to the optimal value of each laser melting deposition process parameter determined in steps (1) to (3), the following two laser melting deposition process parameter variables are experimented and optimized: (4) Keeping the energy density constant, experiment with different pulse laser duty cycles and laser head path planning, record the molten pool morphology and residual stress; at the same time, based on the three-dimensional model established in step 2, obtain the residual stress size in the three-dimensional model for the optimization of the laser melting deposition process; compare the residual stress size data measured in the experiment with the data obtained from the three-dimensional model, and finally obtain the comprehensive influence mechanism of the residual stress when the pulse laser duty cycle and laser head path planning change, and determine the comprehensive relationship Q4 of the residual stress change with the simultaneous change of the pulse laser duty cycle and the laser head path planning; According to the relationship Q4, the pulse laser duty cycle and laser head path planning method corresponding to the minimum residual stress are recorded; (5) The pulse laser duty cycle is fixed, and experiments are conducted with different energy densities and laser head path planning, and the molten pool morphology and residual stress are recorded; at the same time, according to the three-dimensional model established in step 2, the residual stress size in the three-dimensional model for the optimization of the laser melting deposition process is obtained; the residual stress size data measured in the experiment is compared with the data obtained from the three-dimensional model, and finally the comprehensive influence mechanism of the residual stress when the energy density and laser head path planning change, and the comprehensive relationship Q5 of the residual stress changing with the simultaneous change of energy density and laser head path planning is determined; according to the relationship Q5, the energy density size and laser head path planning method corresponding to the minimum residual stress are recorded; (6) The laser head path planning is fixed and unchanged, and the pulse laser duty cycle and energy density are changed to conduct experiments, and the molten pool morphology and residual stress are recorded; at the same time, according to the three-dimensional model established in step 2, the residual stress size in the three-dimensional model for the optimization of the laser melting deposition process is obtained; the residual stress size data measured in the experiment is compared with the data obtained from the three-dimensional model, and finally the comprehensive influence mechanism of the residual stress when the pulse laser duty cycle and energy density change, and the comprehensive relationship Q6 of the residual stress change with the simultaneous change of the pulse laser duty cycle and energy density is determined; According to the relationship Q6, the pulse laser duty cycle and energy density corresponding to the minimum residual stress are recorded; According to the pulse laser duty cycle, energy density and laser head path planning method recorded above, the parameters of the three-dimensional transient evolution numerical prediction model established in step one are set, and finally an optimized three-dimensional transient evolution numerical prediction model is obtained.
4. A method for establishing a numerical prediction model for residual stress in laser melting deposition according to claim 1 or 2, It is characterized in that In the step 3, the "conducting a single-pass laser melting deposition experiment, collecting the molten pool morphology online and in real time and measuring the residual stress magnitude" specifically includes: The blind hole method is used to measure residual stress, and the residual stress of the deposited layer obtained is all tensile stress. The principle is to drill a small hole in the area with residual stress. Since the residual stress near the small hole is released, the residual stress field near the hole area changes. As long as the strain change in the local area is measured, the residual stress value before the release at the drilling site can be calculated. When the residual tensile stress is too large, it will reduce the strength and cause process defects such as deformation and cracking of the workpiece during manufacturing. On the other hand, it will reduce the mechanical properties of the material such as fatigue strength and stress corrosion during the natural release process after manufacturing.
5. The method for establishing a numerical prediction model for residual stress in laser melting deposition according to claim 3, It is characterized in that In the step 3, the "conducting a single-pass laser melting deposition experiment, collecting the molten pool morphology online and in real time and measuring the residual stress magnitude" specifically includes: The blind hole method is used to measure residual stress, and the residual stress of the deposited layer obtained is all tensile stress. The principle is to drill a small hole in the area with residual stress. Since the residual stress near the small hole is released, the residual stress field near the hole area changes. As long as the strain change in the local area is measured, the residual stress value before the release at the drilling site can be calculated. When the residual tensile stress is too large, it will reduce the strength and cause process defects such as deformation and cracking of the workpiece during manufacturing. On the other hand, it will reduce the mechanical properties of the material such as fatigue strength and stress corrosion during the natural release process after manufacturing.