Semiconductor device and method for manufacturing the same, and image sensor
By forming a second trench in the image sensor, silicon defects on the trench surface are reduced, the dark current problem caused by surface damage of the deep trench isolation structure is solved, and the pixel performance and isolation effect are improved.
Patent Information
- Application Number
- CN202210063575.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-20
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-01-20
AI Technical Summary
The existing deep trench isolation structure in CMOS image sensors is seriously damaged due to long dry etching time, which generates dark current and affects pixel performance. If the trench depth is reduced, the isolation effect is poor and cannot be effectively solved. Optical and electrical crosstalk issues.
A plurality of first trenches are formed on the substrate, and silicon is oxidized into a silicon dioxide film layer using an oxidizing reagent, and then etched with chemical reagents to form second trenches, thereby reducing silicon defects on the trench surface and forming deep trenches. Isolation structure.
By reducing silicon defects on the trench surface, better pixel performance is obtained, while the isolation effect is improved, solving the problems of trench surface damage and poor isolation effect.
Smart Images

Figure CN114388429B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor manufacturing technology, and in particular to a semiconductor device and a manufacturing method thereof, and an image sensor. Background Art
[0002] The deep trench isolation (DTI) structure has a good isolation effect, especially in the field of CMOS image sensor (CIS) technology. The DTI technology has been widely used to solve optical and electrical crosstalk problems.
[0003] The DTI structure is formed by dry etching Si and then filling it with a high dielectric (HIK) film and a dielectric film layer. Since the DTI structure is deep, the dry etching time is relatively long, and the surface of the DTI structure groove is impacted by plasma for a long time. As a result, the surface of the DTI structure groove is severely damaged, which will cause the substrate to leak electricity and generate a large dark current, which will have an adverse effect on the performance of white pixels. If the depth of the DTI structure groove is reduced, the isolation effect of the DTI structure is poor, and it is not conducive to solving the optical and electrical crosstalk problems. Summary of the invention
[0004] Therefore, the present invention provides a semiconductor device with excellent pixel performance and a method for manufacturing the same.
[0005] In addition, the present invention also provides an image sensor including the semiconductor device as described above.
[0006] To solve the above problems, the technical solution provided by the present invention is as follows:
[0007] The present invention provides a method for manufacturing a semiconductor device, comprising the steps of:
[0008] providing a first substrate;
[0009] forming a plurality of first grooves on the first substrate;
[0010] Oxidizing the first trench to oxidize a portion of the substrate on the inner wall of the first trench into a silicon dioxide film layer; and
[0011] The silicon dioxide film layer is removed to form a plurality of second trenches.
[0012] In an optional embodiment of the present application, the method further includes the step of filling insulating material in each of the plurality of the second trenches to form a plurality of trench isolation structures.
[0013] In an optional embodiment of the present application, the trench isolation structure is a deep trench isolation structure.
[0014] In an optional embodiment of the present application, in a cross section perpendicular to the first substrate, a depth of the second groove is greater than a depth of the first groove.
[0015] In an optional embodiment of the present application, the first groove is oxidized by an oxidizing agent.
[0016] In an optional embodiment of the present application, the oxidizing agent is hydrogen peroxide.
[0017] In an optional embodiment of the present application, the silicon dioxide film layer is removed by a chemical reagent.
[0018] In an optional embodiment of the present application, the chemical reagent is hydrofluoric acid.
[0019] The present application also provides a semiconductor device, which is manufactured using the semiconductor device manufacturing method as described above.
[0020] The present application also provides an image sensor, comprising a plurality of transistors; the image sensor further comprises the semiconductor device as described above, and each of the transistors is located between at least two of the second trenches.
[0021] The semiconductor device and its manufacturing method and image sensor provided by the present application form a plurality of first grooves on a substrate, then oxidize the silicon exposed in the first grooves into silicon dioxide by an oxidizing agent to form a silicon dioxide film layer on the inner wall of the first groove, and then etch the silicon dioxide film layer by a chemical reagent to form a second groove. In this way, a deep groove structure with fewer silicon defects on the groove surface can be obtained, thereby achieving better pixel performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.
[0023] Figure 1 A manufacturing flow chart of a method for manufacturing a semiconductor device provided in a preferred embodiment of the present invention.
[0024] Figure 2 A cross-sectional view of a substrate and a mask layer provided for a preferred embodiment of the present invention.
[0025] Figure 3 For Figure 2 The mask layer shown is a cross-sectional view of a substrate after being patterned using the mask layer as a mask.
[0026] Figure 4 To remove Figure 3 Cross-sectional view after the mask layer is shown.
[0027] Figure 5 The cross-sectional view is a view after the silicon exposed in the trench is oxidized into silicon dioxide by an oxidizing agent to form a silicon dioxide film layer.
[0028] Figure 6 To etch away with chemical reagents Figure 5 A cross-sectional view of the silicon dioxide film layer after forming a second groove.
[0029] Figure 7 For Figure 6 The second trench is shown as a cross-sectional view after an insulating material is filled in the second trench to form a trench isolation structure.
[0030] Figure 8 This is a schematic diagram of the image sensor provided by the present application (only some transistors and trench isolation structures are shown in the figure). DETAILED DESCRIPTION
[0031] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.
[0032] In the description of the present invention, it should be understood that the orientation or positional relationship indicated by the terms "upper", "lower", etc. is based on the orientation or positional relationship shown in the accompanying drawings, and is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present invention. In addition, the terms "first" and "second" are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined.
[0033] The present invention may repeat reference numerals and / or reference letters in different embodiments. Such repetition is for the purpose of simplicity and clarity and does not in itself indicate the relationship between the various embodiments and / or settings discussed.
[0034] The present invention aims to solve the technical problem that the groove surface of the existing semiconductor device is seriously damaged, and proposes a semiconductor device and a manufacturing method thereof. After a plurality of first grooves are formed on a substrate, the silicon exposed in the grooves is oxidized into silicon dioxide by an oxidizing reagent to form a silicon dioxide film layer on the inner wall of the first groove, and the silicon dioxide film layer is etched away by a chemical reagent to form a second groove. In this way, a deep groove structure with fewer silicon defects on the groove surface can be obtained, thereby achieving better pixel performance.
[0035] The semiconductor device and the method for manufacturing the semiconductor device and the image sensor of the present invention will be described in detail below in conjunction with specific embodiments.
[0036] First, see Figure 1 A preferred embodiment of the present invention provides a method for manufacturing a semiconductor device 110, comprising:
[0037] Step S1, see Figure 1 and Figure 2 , providing a first substrate 10.
[0038] The step S1 further includes the step of: forming a mask layer 20 on the first substrate 10 , wherein the mask layer 20 includes a plurality of openings 21 .
[0039] The first substrate 10 may be a silicon substrate, or a composite substrate formed by bonding at least two silicon material film layers together via other film layers (eg, silicon dioxide, silicon nitride, or other medium).
[0040] The first substrate 10 includes a plurality of spacing regions 11 and a plurality of pixel preparation regions 12, and the plurality of spacing regions 11 and the plurality of pixel preparation regions 12 are arranged at intervals, that is, two pixel preparation regions 12 are formed on both sides of one spacing region 11. The openings 21 correspond to the spacing regions 11 one by one.
[0041] The first substrate 10 further includes a first surface 101 and a second surface 102 , and the second surface 102 is opposite to the first surface 101 .
[0042] In this embodiment, the mask layer 20 is directly formed on the first surface 101 . A portion of the first surface 101 is exposed from the opening 21 .
[0043] In other embodiments, a pad oxide layer or a high dielectric constant film layer may be further included between the mask layer 20 and the first surface 101. The pad oxide layer is used to buffer stress. The high dielectric constant film layer is, for example, at least one of aluminum oxide, hafnium oxide, zirconium oxide or other high dielectric constant film layers, and the high dielectric constant film layer can both increase the transmittance of light on the surface of the silicon substrate and reduce parasitic capacitance.
[0044] The mask layer 20 may be composed of a single mask layer or a plurality of mask layers made of different materials.
[0045] In an optional embodiment of the present application, the mask layer 20 is composed of a single hard mask. Specifically, the hard mask is an inorganic film material generated by chemical vapor deposition (CVD). Its main components are usually TiN, SiN, SiO2, etc.
[0046] In an optional embodiment of the present application, the mask layer 20 includes a first mask layer and a second mask layer, wherein the first mask layer covers the first substrate 10, and the second mask layer covers the first mask layer; the first mask layer is a hard mask, and the second mask layer is a photoresist. In this way, the increase in the characteristic size of the groove caused by the over-etching of the photoresist in contact with the first substrate can be avoided, thereby limiting the characteristic size of the groove and increasing the degree of freedom of the groove design.
[0047] Step S2, see Figures 1 to 3 , a plurality of first grooves 13 are formed on the first substrate 10 .
[0048] Preferably, the first groove 13 extends concavely from the first surface 101 of the first substrate 10 to the second surface 102 of the first substrate 10. In an optional embodiment of the present application, the cross-sectional width of the first groove 13 on the cross-section perpendicular to the first substrate 10 gradually decreases from the first surface 101 of the first substrate 10 to the inside of the first substrate 10, and the first groove 13 on the cross-section perpendicular to the first substrate 10 is in the shape of an inverted quadrangular prism or an inverted quadrangular pyramid; in another optional embodiment, the cross-sectional width of the first groove 13 on the cross-section perpendicular to the first substrate 10 is the same from the first surface 101 of the first substrate 10 to the inside of the first substrate 10, and the first groove 13 on the cross-section perpendicular to the first substrate 10 is rectangular.
[0049] Specifically, the first substrate 10 is etched using the mask layer 20 as a mask to form a plurality of first grooves 13 on the first substrate 10. The first grooves 13 correspond one to one with the openings 21. Specifically, the first grooves 13 can be formed by a dry etching process or a wet etching process. Since dry etching and wet etching processes are well known to those skilled in the art, they will not be further described here.
[0050] Step S3, see Figure 1 and Figure 4 , remove the mask layer 20.
[0051] The mask layer 20 may be removed by ashing or other processes.
[0052] Step S4, see Figure 1 and Figure 5 , the first trench 13 is oxidized to oxidize a portion of the substrate on the inner wall of the first trench 13 into a silicon dioxide film layer 30 .
[0053] In this embodiment, the silicon exposed in the first trench 13 is oxidized into silicon dioxide by an oxidizing agent, so as to form the silicon dioxide film layer 30 on the inner wall of the first trench 13 .
[0054] The oxidizing agent may be hydrogen peroxide or the like.
[0055] The silicon surface exposed in the first groove 13 is subjected to long-term plasma impact during the formation process, resulting in an increase in defects. After contacting oxidizing agents such as hydrogen peroxide, the silicon surface with defects in the first groove 13 will be oxidized into silicon dioxide.
[0056] In an optional embodiment of the present application, part of the silicon on the first surface 101 of the first substrate 10 is also oxidized into silicon dioxide. Therefore, the silicon dioxide film layer 30 can also be formed on the surface of the first substrate 10 .
[0057] Step S5, see Figure 1 and Figure 6 , the silicon dioxide film layer 30 is removed to form a plurality of second trenches 14 .
[0058] In this embodiment, the silicon dioxide film layer 30 is etched away by chemical reagents to form the second trench 14 .
[0059] In an optional embodiment of the present application, in step S5, part of the first substrate 10 oxidized to silicon dioxide is also etched away by the chemical reagent, thereby obtaining a second substrate 40. The second groove 14 is formed on the second substrate 40, so that, in a cross section perpendicular to the first substrate 10, the width of the second groove 14 is greater than the width of the first groove 13, and the depth of the second groove 14 is greater than the depth of the first groove 13.
[0060] Wherein, the chemical reagent may be hydrofluoric acid or the like.
[0061] Among them, after a plurality of first grooves are formed on the first substrate 10, the silicon exposed in the first groove 13 is oxidized into silicon dioxide by an oxidizing reagent to form a silicon dioxide film layer 30 on the inner wall of the first groove 13, and the silicon dioxide film layer 30 is etched away by a chemical reagent to form a second groove 14. In this way, silicon defects on the groove surface can be reduced and a deep groove structure with fewer defects on the groove surface can be obtained, thereby achieving better pixel performance.
[0062] Since the silicon dioxide film layer 30 is formed in a reagent (solution), the silicon dioxide film layer 30 is also formed at the bottom of the first groove 13. When the silicon dioxide film layer 30 is etched away by chemical reagents, part of the substrate at the bottom of the first groove 13 is etched away, further increasing the depth of the first groove 13, and achieving a better isolation effect.
[0063] Step S6, see Figure 1 and Figure 7 , insulating material 15 is filled in each of the plurality of second trenches 14 to form a plurality of trench isolation structures 50 .
[0064] The plurality of trench isolation structures 50 and the second substrate 40 constitute the semiconductor device 110 .
[0065] In this embodiment, the trench isolation structure 50 is a deep trench isolation structure.
[0066] Each trench isolation structure 50 includes at least one second trench 14 and an insulating material 15 filled in the second trench 14 .
[0067] Second, see Figure 7 The present application further provides a semiconductor device 110 , which is manufactured by the above-mentioned method for manufacturing a semiconductor device. Specifically, the semiconductor device 110 includes a plurality of the trench isolation structures 50 .
[0068] Third, see Figure 8The present application also provides an image sensor 100, which includes a plurality of transistors 120 and a semiconductor device 110. The semiconductor device 110 includes a second substrate 40. A plurality of second grooves 14 are formed on the second substrate 40, which are recessed from the surface of the second substrate 40 to the inside of the second substrate 40. The second grooves 14 are also filled with insulating materials 15. The second grooves 14 and the insulating materials 15 filled in the second grooves 14 constitute a trench isolation structure 50. Of course, the trench isolation structure 50 may also include other materials or film layers. Each of the transistors 120 is located between at least two of the trench isolation structures 50, and the trench isolation structure 50 is used to isolate two adjacent transistors 120.
[0069] Of course, the image sensor 100 also includes other structures of image sensors in the prior art, which will not be described in detail here.
[0070] The semiconductor device and its manufacturing method and image sensor provided by the present application form a plurality of first grooves on a substrate, then oxidize the silicon exposed in the grooves into silicon dioxide by an oxidizing agent to form a silicon dioxide film layer on the inner wall of the first groove, and then etch the silicon dioxide film layer by a chemical reagent to form a second groove. In this way, a deep groove structure with fewer silicon defects on the groove surface can be obtained, thereby achieving better pixel performance.
[0071] In summary, although the present invention has been disclosed as above in terms of preferred embodiments, the above preferred embodiments are not intended to limit the present invention. A person skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be based on the scope defined in the claims.
Claims
1. A method for manufacturing a semiconductor device, characterized in that: Includes steps: providing a first substrate; forming a plurality of first grooves on the first substrate; Oxidizing the first trench by using an oxidizing agent to oxidize a portion of the substrate on the inner wall of the first trench into a silicon dioxide film layer; and Removing the silicon dioxide film layer by chemical reagents to form a plurality of second grooves, wherein the depth of the second grooves is greater than the depth of the first grooves in a cross section perpendicular to the first substrate; Insulating materials are respectively filled in the plurality of the second trenches to form a plurality of trench isolation structures, wherein the trench isolation structures are deep trench isolation structures.
2. The method for manufacturing a semiconductor device according to claim 1, wherein: The oxidizing agent is hydrogen peroxide.
3. The method for manufacturing a semiconductor device according to claim 1, wherein: The chemical reagent is hydrofluoric acid.
4. A semiconductor device, characterized in that: The semiconductor device is manufactured by the method for manufacturing a semiconductor device according to any one of claims 1 to 3.
5. An image sensor comprising a plurality of transistors, characterized in that: The image sensor further comprises the semiconductor device according to claim 4, wherein each of the transistors is located between at least two of the second trenches.