A high-nickel sodium ion positive electrode material and preparation method thereof and battery
By introducing MVOx and CNP-Al into high-nickel sodium ion cathode materials and using ammonium sulfate/ammonium bisulfate coating layers, the performance problems caused by cation mixing and environmental reactions are solved, and sodium ion diffusion and electrochemical performance are improved. , suitable for battery applications.
Patent Information
- Application Number
- CN202111540231.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-16
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-12-16
AI Technical Summary
Existing high-nickel sodium-ion batteries have low sodium ion diffusivity and poor electrochemical performance due to the passivation layer caused by the cation mixing effect and the material's reaction to the environment, which limits its application.
NaNiaCobMncO2·fCNP-Al/tMVOx is used as the high-nickel sodium ion cathode material. MVOx suppresses cation mixing, CNP-Al increases the material hardness, and optimizes the material surface through the ammonium sulfate/ammonium bisulfate coating layer to improve sodium ion diffusion. and electrochemical performance.
It improves the conductivity of the nickel-electrolyte interface, enhances the hardness and structural stability of the material, and improves the cycle stability and electrochemical performance of the sodium ion cathode material, making it suitable for battery applications.
Smart Images

Figure CN114400318B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of battery cathode materials, and particularly relates to a high-nickel sodium-ion cathode material, a preparation method thereof, and a battery. Background Art
[0002] Lithium, sodium and other ion batteries are very popular in the current electric vehicle and energy storage battery markets due to their high energy density, excellent power characteristics and stability. Specifically, cathode materials with a fast ion diffusion rate, anode materials with relatively small structural changes and low voltage are crucial aspects for achieving high-power and high-performance battery performance. Although sodium has the basic advantage of being cheaper, due to the chemical composition of sodium-ion batteries and the crystal structure of cathode materials being different from those of lithium-ion batteries, their high specific capacity and reversible cycle life are still inferior to those of lithium-ion batteries. One of the most promising ways to solve the above problems is to develop high-nickel sodium-ion batteries.
[0003] However, the currently available high-nickel sodium-ion batteries have obvious disadvantages. For example, the mixing effect of high-nickel and low-manganese cobalt and other cations reduces the rate of sodium-ion diffusion, resulting in poor performance during discharge; after the material sintering temperature drops, the high-nickel sodium-ion cathode material in the battery reacts relatively quickly with the external environment it contacts, and is prone to react with H2O, CO2, etc. in the environment to generate Na2CO3 and NaOH, and NaOH dehydrates to form Na2O. Na2CO3, NaOH, and Na2O will form a passivation layer on the cathode surface, further hindering the diffusion of sodium ions at the interface between the material and the electrolyte, increasing the impedance between the interface of the material and the electrolyte, and easily causing a decline in the electrochemical performance of the battery. Therefore, this greatly limits the potential application of sodium-ion cathode materials. Summary of the Invention
[0004] The present invention aims to solve at least one of the technical problems existing in the prior art. For this purpose, the present invention provides a high-nickel sodium-ion cathode material, a preparation method thereof, and a battery. The high-nickel sodium-ion cathode material has good electrochemical performance, which is beneficial to the application of the high-nickel sodium-ion cathode material in batteries.
[0005] The above technical object of the present invention is achieved by the following technical solutions:
[0006] A high-nickel sodium-ion cathode material, the chemical formula of the high-nickel sodium-ion cathode material is NaNi a Co b Mn c O2·fCNP-Al / tMVO x , where a + b + c = 1, 0.5 ≤ a < 1, 0 < b ≤ 0.25, a / b ≥ 2.5, 0 < c ≤ 0.3, 0 < t ≤ 0.1, 0 < f ≤ 0.1, and M is at least one of sodium, copper, zinc, zirconium or ammonium.
[0007] Preferably, the MVO x It is at least one of vanadate, metavanadate and pyrovanadate.
[0008] Further preferably, the MVO x It is at least one of sodium vanadate, sodium metavanadate, sodium pyrovanadate, copper vanadate, copper metavanadate, copper pyrovanadate, zinc vanadate, zinc metavanadate, zinc pyrovanadate, zirconium vanadate, zirconium metavanadate, zirconium pyrovanadate, ammonium vanadate, ammonium metavanadate and ammonium pyrovanadate.
[0009] Preferably, the NaNi a Co b Mn c O2·fCNP-Al / tMVO x The CNP-Al (carbon nano-aluminum) is composed of a mixture of carbon nano-powder, aluminum source and dispersant, wherein the mass ratio of aluminum source to carbon nano-powder is (0.1-30): (40-150).
[0010] Preferably, the CNP-Al is prepared by mixing carbon nanopowder with a dispersant, and then mixing with an aluminum source, and then treating at 900-1300° C. for 3-12 hours under a protective atmosphere.
[0011] Preferably, the CNP-Al contains Al4C3.
[0012] Preferably, the aluminum source is at least one of aluminum hydroxide, aluminum acetate, aluminum chloride, aluminum sulfate, aluminum nitrate and aluminum fluoride.
[0013] Preferably, the dispersant is at least one of polyethylene glycol, methyl cellulose, acrylic acid, sodium silicate, methanol, ethanol and propanol.
[0014] Preferably, the NaNi a Co b Mn c O2·fCNP-Al / tMVO x The particle size D50 is 1-10 μm.
[0015] Preferably, the NaNi a Co b Mn c O2·fCNP-Al / tMVO x Particle size D max 30-100μm.
[0016] Preferably, the NaNi a Co b Mn c O2·fCNP-Al / tMVO xThe hardness (HB) is 100-500.
[0017] Preferably, the NaNi a Co b Mn c O2·fCNP-Al / tMVO x The specific surface area BET is 0.2-3m 2 / g.
[0018] Preferably, the NaNi a Co b Mn c O2·fCNP-Al / tMVO x The tap density is 2.5-4.5m 3 / g.
[0019] A method for preparing the high nickel sodium ion positive electrode material as described above comprises the following steps: mixing a sodium source, carbon nano-aluminum and a nickel-cobalt-manganese material, drying and dehydrating, calcining, annealing, and then mixing with MVO x , obtained by two-stage calcination.
[0020] Preferably, after the second-stage calcination, the method further comprises the step of removing residual sodium from the high-nickel sodium ion positive electrode material to form a sodium salt-coated high-nickel sodium ion positive electrode material.
[0021] Preferably, the high nickel sodium ion positive electrode material after the second-stage calcination is placed in an alcohol solution, a sodium removal agent is added, and the solution is stirred, allowed to stand, and hydrothermally dried to obtain a sodium salt-coated high nickel sodium ion positive electrode material.
[0022] Preferably, the sodium removal agent is 0.001-0.2M ammonium sulfate or 0.001-0.2M ammonium bisulfate.
[0023] Preferably, the amount of the sodium remover added is 0.001-10w% of the high-nickel sodium ion positive electrode material.
[0024] Further preferably, the amount of the sodium removing agent added is 0.1-2w% of the high nickel sodium ion positive electrode material.
[0025] Preferably, the sodium source is at least one of sodium hydroxide, sodium acetate, sodium oxalate, sodium phosphate and sodium carbonate.
[0026] Preferably, the nickel-cobalt-manganese material is recovered from discarded ternary lithium batteries.
[0027] Preferably, the method for recycling and treating waste ternary lithium batteries is: subjecting the ternary positive electrode materials recovered from the waste ternary lithium batteries to acid leaching, aluminum removal, copper removal, and extraction to obtain a nickel-cobalt-manganese mixture, determining the nickel-cobalt-manganese ratio in the nickel-cobalt-manganese mixture, adding a supplement and a dispersant as described above to the nickel-cobalt-manganese mixed solution, stirring thoroughly to obtain a homogeneous solution, maintaining a constant temperature, adding a precipitant, stirring until complete precipitation, and standing to obtain a nickel-cobalt-manganese material.
[0028] Preferably, the nickel-cobalt-manganese mixture is at least one of a nickel-cobalt-manganese sulfate mixed salt solution, a nickel-cobalt-manganese nitrate mixed salt solution and a nickel-cobalt-manganese chlorate mixed salt solution.
[0029] Preferably, the supplement is at least one of nickel sulfate, nickel nitrate, manganese sulfate and manganese nitrate.
[0030] Preferably, the precipitant is at least one of carbonic acid, carbon dioxide, sodium carbonate, potassium carbonate, sodium bicarbonate, ammonium carbonate, ammonium bicarbonate and lithium carbonate.
[0031] Preferably, the first stage calcination temperature is 400-900°C, and the calcination time is 5-12h, and the second stage calcination temperature is 600-1000°C, and the calcination time is 5-16h.
[0032] A battery comprises the high nickel sodium ion positive electrode material as described above.
[0033] The beneficial effects of the present invention are:
[0034] (1) The high nickel sodium ion positive electrode material of the present invention contains MVO x , which can inhibit Na + / Ni 2+ Mixed arrangement overcomes the structural defects of the existing high nickel sodium ion positive electrode materials, thereby improving the conductivity of the nickel-electrolyte interface. At the same time, the CNP-Al in the high nickel sodium ion positive electrode material of the present invention contains Al4C3, which can increase the hardness and strength of the high nickel sodium ion positive electrode material of the present invention, and can also cooperate with MVO x Improving the electrochemical properties of high-nickel sodium-ion positive electrode materials is beneficial to the application of high-nickel sodium-ion positive electrode materials in batteries.
[0035] (2) During the preparation process of the high nickel sodium ion positive electrode material of the present invention, a multifunctional coating layer can be created on the surface of the high nickel sodium ion positive electrode material by adding a sodium removal agent (ammonium sulfate / ammonium bisulfate), thereby further optimizing the performance of the high nickel sodium ion positive electrode material. On the one hand, ammonium sulfate / ammonium bisulfate removes the residual Na2CO3, NaOH, and Na2O alkaline substances on the surface of the material, so that the removed Na2CO3, NaOH, and Na2O alkaline substances are converted into a more stable sodium salt coating layer. On the other hand, the sodium salt coating layer will be directly converted into a more stable sodium salt coating layer.+ Conductive sodium salt coating improves the stability of the material structure and enhances the Na + Transfer, improve the diffusion of sodium ions at the interface between the material and the electrolyte, and improve the specific capacity, so that the high nickel sodium ion positive electrode material has better cycle stability, surface structure stability and good electrochemical performance.
[0036] (3) The nickel-cobalt-manganese material used in the production process of the high-nickel-sodium-ion positive electrode material of the present invention is obtained by recycling discarded ternary lithium batteries, thereby turning waste into treasure and effectively reducing environmental pollution. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 This is a SEM image of the high-nickel sodium ion positive electrode material of Example 1;
[0038] Figure 2 This is a TEM image of the high-nickel sodium ion positive electrode material of Example 1;
[0039] Figure 3 This is the TEM image of the high nickel sodium ion positive electrode material of comparative example 1. DETAILED DESCRIPTION
[0040] The present invention will be further described below in conjunction with specific embodiments.
[0041] Embodiment 1:
[0042] A high nickel sodium ion positive electrode material, the chemical formula of which is NaNi 0.8 C o0.1 Mn 0.1 O2·0.059CNP-Al / 0.03NH4VO3.
[0043] The method for preparing the above-mentioned high-nickel sodium ion positive electrode material comprises the following steps:
[0044] (1) Preparation of nickel-cobalt-manganese material: The ternary positive electrode material recovered from the discarded ternary lithium battery was subjected to acid leaching, aluminum removal, copper removal, and extraction to obtain a nickel-cobalt-manganese sulfate mixed salt solution, and the nickel-cobalt-manganese molar ratio in the nickel-cobalt-manganese sulfate mixed salt solution was determined (0.965:0.12:0.11). 500 mL was placed in a beaker, and 0.011 M nickel sulfate, 0.002 M cobalt sulfate, and 0.012 M manganese sulfate were added to the nickel-cobalt-manganese sulfate mixed salt solution. 40 ml of methyl cellulose was added, and the mixture was stirred thoroughly. The temperature was kept constant at 45° C. Sodium carbonate was added, and the mixture was stirred until complete precipitation was achieved. The mixture was allowed to stand for 3 h to obtain the nickel-cobalt-manganese material.
[0045] (2) Preparation of CNP-Al: 4 g of carbon nanopowder was dispersed in 30 mL of polyethylene glycol, and 75 mL of 0.47 M aluminum chloride solution was added to mix. The mixture was sent to an electric furnace and treated at 940 °C for 6 h under Ar to obtain 5.5 g of CNP-Al containing Al4C3.
[0046] (3) Synthesis of NaNi 0.8 C o0.1 Mn 0.1 O2·0.059CNP-Al / 0.03NH4VO3: 35g of sodium hydroxide, 46.17g of the nickel-cobalt-manganese material prepared in step (1), and 4.7g of CNP-Al prepared in step (2) were mixed, ball-milled, stirred, dried and dehydrated, and sent to an electric furnace for calcination at 540°C for 8h, annealed, 2.4g of NH4VO3 was added, mixed, ball-milled, and calcined at 740°C for 10h to obtain a high-nickel sodium ion positive electrode material NaNi 0.8 C o0.1 Mn 0.1 O2·0.059CNP-Al / 0.03NH4VO3.
[0047] (4) Sodium removal and sodium salt coating: 20 g of the high nickel sodium ion positive electrode material prepared in step (3) was placed in a beaker containing 55 mL of polyethylene glycol, 25 mL of 0.019 M ammonium bisulfate solution was added, the mixture was stirred vigorously, allowed to stand, the upper layer of liquid was removed, and the solid layer was washed. Then, the lower layer of solid was placed in a microwave heating device and dried at 180° C. for 42 min, dehydrated, dealcoholized, and deaminated to obtain a sodium salt-coated high nickel sodium ion positive electrode material NaNi 0.8 C o0.1 Mn 0.1 O2·0.059CNP-Al / 0.03NH4VO3.
[0048] The principle of sodium salt coating is shown in reaction formula ①-⑦: ①-② are sodium hydroxide heated and dehydrated to obtain disodium oxide and sodium carbonate obtained by reaction with carbon dioxide, ③-④ are ammonium sulfate decomposition reactions to obtain, respectively, ⑤-⑦ are ammonium sulfate decomposition reactions to obtain ammonium bisulfate, sulfuric acid and sodium hydroxide, disodium oxide, sodium carbonate reaction formula to obtain sodium sulfate.
[0049] ①2NaOH→Na2O+H2O
[0050] ②2NaOH+CO2→Na2CO3+H2O
[0051] ③(NH4)2SO4→NH4HSO4+NH3
[0052] ④NH4HSO4→H2SO4+NH3
[0053] ⑤NH4HSO4+H2SO4+4NaOH→2Na2SO4+NH3+4H2O
[0054] ⑥NH4HSO4+H2SO4+2Na2CO3→2Na2SO4+NH3+2H2O+2CO2
[0055] ⑦NH4HSO4+H2SO4+2Na2O→2Na2SO4+NH3+2H2O
[0056] Embodiment 2:
[0057] A high nickel sodium ion positive electrode material, the chemical formula of which is NaNi 0.74 Co 0.16 Mn 0.1 O2·0.045CNP-Al / 0.02NH4VO3.
[0058] The method for preparing the above-mentioned high-nickel sodium ion positive electrode material comprises the following steps:
[0059] (1) Preparation of nickel-cobalt-manganese material: The ternary positive electrode material recovered from the discarded ternary lithium battery was subjected to acid leaching, aluminum removal, copper removal, and extraction to obtain a nickel-cobalt-manganese sulfate mixed salt solution, and the nickel-cobalt-manganese molar ratio in the nickel-cobalt-manganese sulfate mixed salt solution was determined (0.965:0.12:0.11). 500 mL was placed in a beaker, and 0.09 M cobalt sulfate and 0.02 M manganese sulfate were added to the nickel-cobalt-manganese sulfate mixed salt solution. 40 ml of methyl cellulose was added and stirred thoroughly. Sodium carbonate was added at a constant temperature of 45°C, and stirred until complete precipitation was achieved. The solution was allowed to stand for 3 h to obtain the nickel-cobalt-manganese material.
[0060] (2) Preparation of CNP-Al: 4 g of carbon nanopowder was dispersed in 48 mL of polyethylene glycol, and 80 mL of 0.47 M aluminum chloride solution was added to mix. The mixture was sent to an electric furnace and treated at 940 °C for 6 h under Ar to obtain 5.4 g of CNP-Al containing Al4C3.
[0061] (3) Synthesis of NaNi 0.74 Co 0.16 Mn 0.1 O2·0.045CNP-Al / 0.02NH4VO3: 51g of sodium hydroxide, 55.4g of the nickel-cobalt-manganese material prepared in step (1), and 4.8g of CNP-Al prepared in step (2) were mixed, ball-milled, stirred, dried and dehydrated, and sent to an electric furnace for calcination at 540°C for 8h, annealed, 2.1g of NH4VO3 was added, mixed, ball-milled, and calcined at 740°C for 10h to obtain a high-nickel sodium ion positive electrode material NaNi 0.74 Co 0.16 Mn 0.1O2·0.045CNP-Al / 0.02NH4VO3.
[0062] (4) Sodium removal and sodium salt coating: 20 g of the high nickel sodium ion positive electrode material prepared in step (3) was placed in a beaker containing 55 mL of polyethylene glycol, 25 mL of 0.019 M ammonium sulfate solution was added, the mixture was stirred vigorously, allowed to stand, the upper liquid was removed, and the lower solid was placed in a microwave heating device and dried at 180° C. for 42 min, dehydrated, dealcoholized, and deaminated to obtain a sodium salt-coated high nickel sodium ion positive electrode material NaNi 0.74 Co 0.16 Mn 0.1 O2·0.045CNP-Al / 0.02NH4VO3.
[0063] Embodiment 3:
[0064] A high nickel sodium ion positive electrode material, the chemical formula of which is NaNi 0.68 Co 0.23 Mn 0.09 O2·0.037CNP-Al / 0.015NaVO3.
[0065] The method for preparing the above-mentioned high-nickel sodium ion positive electrode material comprises the following steps:
[0066] (1) Preparation of nickel-cobalt-manganese material: The ternary positive electrode material recovered from the discarded ternary lithium battery was subjected to acid leaching, aluminum removal, copper removal, and extraction to obtain a nickel-cobalt-manganese sulfate mixed salt solution, and the nickel-cobalt-manganese molar ratio in the nickel-cobalt-manganese sulfate mixed salt solution was determined (0.965:0.12:0.11). 500 mL was placed in a beaker, and 0.143 M cobalt sulfate and 0.018 M manganese sulfate were added to the nickel-cobalt-manganese sulfate mixed salt solution. 50 mL of acrylic acid was added, and the mixture was stirred thoroughly. The temperature was kept constant at 45° C. Ammonium carbonate was added, and the mixture was stirred until complete precipitation was achieved. The mixture was allowed to stand for 3 h to obtain the nickel-cobalt-manganese material.
[0067] (2) Preparation of CNP-Al: 6.5 g of carbon nanopowder was dispersed in 50 mL of polyethylene glycol, and 70 mL of 0.47 M aluminum chloride solution was added to mix. The mixture was sent to an electric furnace and treated at 1284 °C for 6 h under Ar to obtain 7.9 g of CNP-Al containing Al4C3.
[0068] (3) Synthesis of NaNi 0.68 Co 0.23 Mn 0.09O2·0.037CNP-Al / 0.015NaVO3: 122.0 g of sodium acetate, 60.1 g of the nickel-cobalt-manganese material prepared in step (1), and 6.8 CNP-Al prepared in step (2) were mixed, ball-milled, stirred, dried and dehydrated, and sent to an electric furnace for calcination at 590°C for 6 h, annealed, 2.7 g of NaVO3 was added, mixed, ball-milled, and calcined at 680°C for 16 h to obtain a high-nickel sodium ion positive electrode material NaNi 0.68 Co 0.23 Mn 0.09 O2·0.037CNP-Al / 0.015NaVO3.
[0069] (4) Sodium removal and sodium salt coating: 20 g of the high nickel sodium ion positive electrode material prepared in step (3) was placed in a beaker containing 45 mL of polyethylene glycol, 25 mL of 0.019 M ammonium sulfate solution was added, the mixture was stirred vigorously, allowed to stand, the upper liquid layer was removed, and the lower solid layer was placed in a microwave heating device and dried at 180° C. for 42 min, dehydrated, dealcoholized, and deaminated to obtain a sodium salt-coated high nickel sodium ion positive electrode material NaNi 0.68 Co 0.23 Mn 0.09 O2·0.037CNP-Al / 0.015NaVO3.
[0070] Embodiment 4:
[0071] A high nickel sodium ion positive electrode material, the chemical formula of which is NaNi 0.55 Co 0.18 Mn 0.27 O2·0.034CNP-Al / 0.02NaVO3.
[0072] The method for preparing the above-mentioned high-nickel sodium ion positive electrode material comprises the following steps:
[0073] (1) Preparation of nickel-cobalt-manganese material: The ternary positive electrode material recovered from the discarded ternary lithium battery was subjected to acid leaching, aluminum removal, copper removal, and extraction to obtain a nickel-cobalt-manganese sulfate mixed salt solution, and the nickel-cobalt-manganese molar ratio in the nickel-cobalt-manganese sulfate mixed salt solution was determined (0.965:0.12:0.11). 500 mL was placed in a beaker, and 0.2 M cobalt sulfate and 0.25 M manganese sulfate were added to the nickel-cobalt-manganese sulfate mixed salt solution. 50 mL of acrylic acid was added, and the solution was stirred thoroughly. The temperature was kept constant at 45° C. Ammonium carbonate was added, and the solution was stirred until completely precipitated. The solution was allowed to stand for 3 h to obtain the nickel-cobalt-manganese material.
[0074] (2) Preparation of CNP-Al: 5.3 g of carbon nanopowder was dispersed in 40 mL of polyethylene glycol, and 60 mL of 0.47 M aluminum chloride solution was added to mix. The mixture was sent to an electric furnace and treated at 1284 °C for 6 h under Ar to obtain 6.4 g of CNP-Al containing Al4C3.
[0075] (3) Synthesis of NaNi 0.55 Co 0.18 Mn 0.27 O2·0.034CNP-Al / 0.02NaVO3: 98.8g of sodium acetate, 55.1g of the nickel-cobalt-manganese material prepared in step (1), and 5.2CNP-Al prepared in step (2) were mixed, ball-milled, stirred, dried and dehydrated, and sent to an electric furnace for calcination at 590°C for 6h, annealed, 3.1g of NaVO3 was added, mixed, ball-milled, and calcined at 680°C for 16h to obtain a high-nickel sodium ion positive electrode material NaNi 0.55 Co 0.18 Mn 0.27 O2·0.034CNP-Al / 0.02NaVO3.
[0076] (4) Sodium removal and sodium salt coating: 20 g of the high nickel sodium ion positive electrode material prepared in step (3) was placed in a beaker containing 45 mL of polyethylene glycol, 25 mL of 0.019 M ammonium sulfate solution was added, the mixture was stirred vigorously, allowed to stand, the upper liquid layer was removed, and the lower solid layer was placed in a microwave heating device and dried at 180° C. for 42 min, dehydrated, dealcoholized, and deaminated to obtain a sodium salt-coated high nickel sodium ion positive electrode material NaNi 0.55 Co 0.18 Mn 0.27 O2·0.034CNP-Al / 0.02NaVO3.
[0077] Comparative Example 1:
[0078] A high nickel sodium ion positive electrode material, the chemical formula of which is NaNi 0.8 C o0.1 Mn 0.1 O2·0.059CNP-Al / 0.03NH4VO3.
[0079] The method for preparing the above-mentioned high-nickel sodium ion positive electrode material comprises the following steps:
[0080] (1) Preparation of nickel-cobalt-manganese material: The ternary positive electrode material recovered from the discarded ternary lithium battery was subjected to acid leaching, aluminum removal, copper removal, and extraction to obtain a nickel-cobalt-manganese sulfate mixed salt solution, and the nickel-cobalt-manganese molar ratio in the nickel-cobalt-manganese sulfate mixed salt solution was determined (0.965:0.12:0.11). 500 mL was placed in a beaker, and 0.011 M nickel sulfate, 0.002 M cobalt sulfate, and 0.012 M manganese sulfate were added to the nickel-cobalt-manganese sulfate mixed salt solution. 40 ml of methyl cellulose was added, and the mixture was stirred thoroughly. The temperature was kept constant at 45° C. Sodium carbonate was added, and the mixture was stirred until complete precipitation was achieved. The mixture was allowed to stand for 3 h to obtain the nickel-cobalt-manganese material.
[0081] (2) Preparation of CNP-Al: 4 g of carbon nanopowder was dispersed in 30 mL of polyethylene glycol, and 75 mL of 0.47 M aluminum chloride solution was added to mix. The mixture was sent to an electric furnace and treated at 940 °C for 6 h under Ar to obtain 5.5 g of CNP-Al containing Al4C3.
[0082] (3) Synthesis of NaNi 0.8 C o0.1 Mn 0.1 O2·0.059CNP-Al / 0.03NH4VO3: 35g of sodium hydroxide, 46.17g of the nickel-cobalt-manganese material prepared in step (1), and 4.7g of CNP-Al prepared in step (2) were mixed, ball-milled, stirred, dried and dehydrated, and sent to an electric furnace for calcination at 540°C for 8h, annealed, 2.4g of NH4VO3 was added, mixed, ball-milled, and calcined at 740°C for 10h to obtain a high-nickel sodium ion positive electrode material NaNi 0.8 C o0.1 Mn 0.1 O2·0.059CNP-Al / 0.03NH4VO3.
[0083] Comparative Example 2:
[0084] A high nickel sodium ion positive electrode material, the chemical formula of which is NaNi 0.68 Co 0.23 Mn 0.09 O2·0.037CNP-Al.
[0085] The method for preparing the above-mentioned high-nickel sodium ion positive electrode material comprises the following steps:
[0086] (1) Preparation of nickel-cobalt-manganese material: The ternary positive electrode material recovered from the discarded ternary lithium battery was subjected to acid leaching, aluminum removal, copper removal, and extraction to obtain a nickel-cobalt-manganese sulfate mixed salt solution, and the nickel-cobalt-manganese molar ratio in the nickel-cobalt-manganese sulfate mixed salt solution was determined (0.965:0.12:0.11). 500 mL was placed in a beaker, and 0.143 M cobalt sulfate and 0.018 M manganese sulfate were added to the nickel-cobalt-manganese sulfate mixed salt solution. 50 mL of acrylic acid was added, and the mixture was stirred thoroughly. The temperature was kept constant at 45° C. Sodium carbonate was added, and the mixture was stirred until complete precipitation was achieved. The mixture was allowed to stand for 3 h to obtain the nickel-cobalt-manganese material.
[0087] (2) Preparation of CNP-Al: 6.5 g of carbon nanopowder was dispersed in 50 mL of polyethylene glycol, and 70 mL of 0.47 M aluminum chloride solution was added to mix. The mixture was sent to an electric furnace and treated at 1284 °C for 6 h under Ar to obtain 7.9 g of CNP-Al containing Al4C3.
[0088] (3) Synthesis of NaNi 0.68 Co 0.23 Mn 0.09O2·0.037CNP-Al: 122.0 g of sodium acetate, 60.1 g of the nickel-cobalt-manganese material prepared in step (1), and 6.8 CNP-Al prepared in step (2) were mixed, ball-milled, stirred, dried and dehydrated, and sent to an electric furnace for calcination at 590° C. for 6 h, annealed, and calcined at 680° C. for 16 h to obtain a high-nickel sodium ion positive electrode material NaNi 0.68 Co 0.23 Mn 0.09 O2·0.037CNP-Al.
[0089] (4) Sodium removal and sodium salt coating: 20 g of the high nickel sodium ion positive electrode material prepared in step (3) was placed in a beaker containing 45 mL of polyethylene glycol, 25 mL of 0.019 M ammonium sulfate solution was added, the mixture was stirred vigorously, allowed to stand, the upper liquid layer was removed, and the lower solid layer was placed in a microwave heating device and dried at 180° C. for 42 min, dehydrated, dealcoholized, and deaminated to obtain a sodium salt-coated high nickel sodium ion positive electrode material NaNi 0.68 Co 0.23 Mn 0.09 O2·0.037CNP-Al.
[0090] Comparative Example 3:
[0091] A high nickel sodium ion positive electrode material, the chemical formula of which is NaNi 0.68 Co 0.23 Mn 0.09 O2 / 0.015NaVO3.
[0092] The method for preparing the above-mentioned high-nickel sodium ion positive electrode material comprises the following steps:
[0093] (1) Preparation of nickel-cobalt-manganese material: The ternary positive electrode material recovered from the discarded ternary lithium battery was subjected to acid leaching, aluminum removal, copper removal, and extraction to obtain a nickel-cobalt-manganese sulfate mixed salt solution, and the nickel-cobalt-manganese molar ratio in the nickel-cobalt-manganese sulfate mixed salt solution was determined (0.965:0.12:0.11). 500 mL was placed in a beaker, and 0.143 M cobalt sulfate and 0.018 M manganese sulfate were added to the nickel-cobalt-manganese sulfate mixed salt solution. 50 mL of acrylic acid was added, and the mixture was stirred thoroughly. The temperature was kept constant at 45° C. Sodium carbonate was added, and the mixture was stirred until complete precipitation was achieved. The mixture was allowed to stand for 3 h to obtain the nickel-cobalt-manganese material.
[0094] (2) Synthesis of NaNi 0.68 Co 0.23 Mn 0.09O2 / 0.015NaVO3: 122.0g sodium acetate and 60.1g nickel-cobalt-manganese material prepared in step (1) were mixed, ball-milled, stirred, dried and dehydrated, and sent to an electric furnace for calcination at 590°C for 6h, annealed, 2.7g NaVO3 was added, mixed, ball-milled, and calcined at 680°C for 16h to obtain a high-nickel sodium ion positive electrode material NaNi 0.68 Co 0.23 Mn 0.09 O2 / 0.015NaVO3.
[0095] (3) Sodium removal and sodium salt coating: 20 g of the high nickel sodium ion positive electrode material prepared in step (3) was placed in a beaker containing 45 mL of polyethylene glycol, 25 mL of 0.019 M ammonium sulfate solution was added, the mixture was stirred vigorously, allowed to stand, the upper liquid layer was removed, and the lower solid layer was placed in a microwave heating device and dried at 180° C. for 42 min, dehydrated, dealcoholized, and deaminated to obtain a sodium salt-coated high nickel sodium ion positive electrode material NaNi 0.68 Co 0.23 Mn 0.09 O2 / 0.015NaVO3.
[0096] Test example:
[0097] The particle size, hardness, BET and tap density of the high nickel sodium ion positive electrode materials of Examples 1-4 and Comparative Examples 1-3 were measured respectively, and then the high nickel sodium ion positive electrode materials of Examples 1-4 and Comparative Examples 1-3 were mixed with acetylene black and polyvinylidene fluoride (PVDF) in a beaker at a mass ratio of 80:15:5, and ground into slurry after adding a small amount of NMP. The slurry was then evenly applied to aluminum foil with a coater having a thickness of 120 μm, placed in a vacuum drying oven at 100°C for 8 hours, and punched into a positive electrode sheet with a diameter of 16 mm for standby use (wherein the mass of the active material is about 15-20 mg). An organic solution of ethylene carbonate of 1.2 M NaPF6 was used as the electrolyte, and a metal sodium sheet was used as the negative electrode, and assembled into a CR2025 button cell in a glove box filled with Ar. The battery performance was tested using a BTS battery tester with a test voltage of 2.5-4.0 V, a current density of 2 C, and a scan rate of 0.1 mV / s. The test results are shown in Table 1.
[0098] Table 1: Test results
[0099]
[0100] At the same time, the high nickel sodium ion positive electrode material of Example 1 was subjected to SEM test and TEM test. The results of the SEM test are as follows: Figure 1 The results of TEM test are shown in Figure 2 As shown; TEM test was performed on the high nickel sodium ion positive electrode material of Comparative Example 1, and the test results are as follows Figure 3 shown.
[0101] As shown in Table 1, the first discharge capacity of the CR2025 button cell made of the high nickel sodium ion positive electrode material of the present application can reach 161.9 mAh g -1 After 150 cycles, the discharge capacity is still 124.5 mAh g -1 The CR2025 button cell made of the high nickel sodium ion positive electrode material of the present application can achieve an initial discharge / charge efficiency of 73.2% or more, and a discharge / charge efficiency of 99.7% or more after 150 cycles.
[0102] At the same time, by comparing Example 1 and Comparative Example 1, it can be seen that when other conditions remain unchanged, the high nickel sodium ion positive electrode material is not subjected to residual sodium removal at the end, and the discharge specific capacity and discharge / charge efficiency of the high nickel sodium ion positive electrode material finally obtained are poor, which makes the cycle stability of the high nickel sodium ion positive electrode material worse.
[0103] By comparing Example 3 with Comparative Examples 2-3, it can be seen that when other conditions remain unchanged, the high nickel sodium ion positive electrode material does not contain MVO x Or CNP-Al, the hardness of the high nickel sodium ion positive electrode material will decrease, and its discharge specific capacity and discharge / charge efficiency will be poor.
[0104] In addition, by Figure 1 It can be seen that the size of the high-nickel sodium ion positive electrode material in Example 1 is mainly 5-10 μm, the particles are relatively compact, and the dispersed high-nickel sodium ion positive electrode material is less.
[0105] Depend on Figure 2 It can be seen that there is a 38nm coating layer on the surface of the high nickel sodium ion positive electrode material of Example 1. The existence of the coating layer can avoid structural defects and improve the electrochemical performance. Figure 3 It can be seen that the surface of the high nickel sodium ion positive electrode material of Comparative Example 1 is smooth and no coating layer is visible.
[0106] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A high nickel sodium ion positive electrode material, Features: The chemical formula of the high-nickel sodium-ion cathode material is NaNi a Co b Mn c O 2 ·fCNP-Al / tMVO x , where a + b + c = 1, 0.5 ≤ a < 1, 0 < b ≤ 0.25, a / b ≥ 2.5, 0 < c ≤ 0.3, 0 < t ≤ 0.1, 0 < f ≤ 0.1, and M is at least one of sodium, copper, zinc, zirconium or ammonium; the MVO a Co b Mn c O 2 ·fCNP-Al / tMVO x in NaNi x Co 4 C 3 is at least one of vanadate, metavanadate and pyrophosphate; the CNP-Al is prepared by mixing carbon nanoflour with a dispersant, then mixing with an aluminum source, and then treating at 900-1300 °C for 3-12 h under a protective atmosphere; the CNP-Al contains Al .
2. A method for preparing the high nickel sodium ion positive electrode material as claimed in claim 1, Features: The following steps are involved: Mix the sodium source, CNP-Al and nickel-cobalt-manganese materials, dry and dehydrate, calcine and anneal, and then mix with MVO x , and two-stage calcination, wherein the first-stage calcination temperature is 400-900°C, the calcination time is 5-12h, and the second-stage calcination temperature is 600-1000°C, and the calcination time is 5-16h.
3. A method for preparing a high nickel sodium ion positive electrode material according to claim 2, Features: After the second-stage calcination, the method further includes removing residual sodium from the high-nickel sodium ion positive electrode material to form a sodium salt-coated high-nickel sodium ion positive electrode material.
4. The method for preparing a high nickel sodium ion positive electrode material according to claim 3, Features: The residual sodium removal operation steps are as follows: placing the high nickel sodium ion positive electrode material after the second stage calcination in an alcohol solution, adding a sodium removal agent, stirring, standing, and hydrothermally drying to obtain a sodium salt-coated high nickel sodium ion positive electrode material.
5. A method for preparing a high-nickel sodium ion positive electrode material according to any one of claims 2 to 4, Features: The nickel-cobalt-manganese material is obtained by recycling discarded ternary lithium batteries.
6. A battery, Features: Including the high nickel sodium ion positive electrode material as described in claim 1.