A micro-textured ion-sulfurized CoCrFeNiMo high-entropy alloy cladding layer and its application
By micro-texturing and ion sulfurizing the CoCrFeNiMo high-entropy alloy cladding layer on the surface of the substrate, the wear resistance problem of the sulfurized layer under dry friction and heavy load conditions is solved, and the service life and wear resistance are significantly improved. , achieving a lower friction coefficient and smaller wear scar area.
Patent Information
- Application Number
- CN202210067588.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-20
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-01-20
AI Technical Summary
The existing sulfurized layer is difficult to last under dry friction and heavy load conditions. The sulfide solid lubricating film layer is thin and easy to wear, resulting in a short service life.
Micro-textured ion-sulfurized CoCrFeNiMo high-entropy alloy cladding layer is used. CoCrFeNiMo high-entropy alloy powder is clad on the surface of the substrate, and micro-textured and sulfurized to form a texture pattern of pit array or parallel grooves. , combined with ion sulfurization technology to enhance the wear resistance of the lubricating layer.
The friction-reducing and wear-resisting performance of the substrate is significantly improved, and the service life is extended. Through the combination of laser cladding and ion sulfurizing processes, a lower friction coefficient and a smaller wear scar area are achieved.
Smart Images

Figure CN114411147B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of surface modification and coating, and particularly relates to a micro-textured ion-sulfurized CoCrFeNiMo high-entropy alloy cladding layer and application thereof. Background Art
[0002] Solid lubrication meets the lubrication requirements of harsh working conditions such as vacuum, high temperature, seawater, and dry friction, and has great development and application prospects. Exploring new solid self-lubricating films and their preparation technologies is a hot topic in tribology research. Sulfurization is an economical and effective method to form a sulfide solid lubricating film layer on the surface of the friction pair. Ion sulfurization is a new sulfurization technology independently developed in my country. It is an in-situ synthesis process. It is known as a "green" sulfurization technology because of its energy saving and pollution-free nature. It can achieve low-temperature sulfurization. However, the radius of sulfur atoms is large and it is difficult to diffuse in metals, so the sulfurized layer is generally thin; in addition, the sulfide solid lubricating film layer is a soft film that is prone to wear during service and is difficult to last under dry friction and heavy load conditions. Therefore, how to improve its service life is an important issue facing the sulfurized layer. Summary of the invention
[0003] The present invention provides a micro-textured ion-sulfurized CoCrFeNiMo high-entropy alloy cladding layer, which is obtained by cladding CoCrFeNiMo high-entropy alloy powder on the surface of a substrate, and sequentially performing micro-texturing and sulfurization treatments on the cladding layer. The CoCrFeNiMo high-entropy alloy powder is obtained by mixing atomized powder CoCrFeNi and elemental powder Mo in a molar ratio of 1:1 and drying at 100-150°C.
[0004] In the present invention, microtexture is to process the surface of the cladding layer to form a texture pattern, and the texture pattern is a pit array or parallel grooves. The pit diameter of the pit array is 100-500 μm, and the center distance is 150-1500 μm; the width of the parallel groove is 50-200 μm, and the center distance is 50-500 μm.
[0005] In the present invention, the microtexturing process is carried out in a laser marking machine. The pit array is textured by the following parameters: marking speed 100-1000 mm / s, power 5-20 W, filling radius 0.001-0.05 mm, marking times 1-10 times, jump speed 3000 mm / s, Q frequency 25 khz, Q release 1 μs. The parallel grooves are textured by the following parameters: marking speed 100-1000 mm / s, power 5-20 W, marking times 1-10 times, jump speed 3000 mm / s, Q frequency 25 khz, Q release 1 μs.
[0006] Before the micro-texturing treatment, the surface of the cladding layer may be polished, preferably, using sandpaper for polishing; more preferably, using 600#, 1000#, 1500#, and 2000# sandpaper for polishing in sequence.
[0007] In the present invention, the sulfurization treatment adopts an ion sulfurization method, and the sulfurization treatment parameters are: voltage 520-750V, insulation temperature 210-290°C, H2S gas flow rate 20-30sccm, insulation time 2-3h.
[0008] In the present invention, the cladding is selected from laser cladding. The laser cladding parameters are: laser power of 1500-5000W, cladding speed of 200-800mm / min, overlap rate of 20-50%. Before cladding, the substrate surface can be preferably polished to remove the oxide scale.
[0009] During the cladding process, the CoCrFeNiMo high entropy alloy powder laid on the substrate preferably has a thickness of 0.8 to 2 mm. Before laying the high entropy alloy powder, the substrate surface may be preferably polished to remove the oxide scale.
[0010] In the process of marking and constructing micro-textures, oxides and raised burrs will be formed on the surface of the texture pattern due to ablation. Therefore, before sulfurization treatment, the texture pattern needs to be polished to eliminate craters or burrs. The polishing can preferably be done with 2000# sandpaper.
[0011] The micro-textured ion-sulfurized CoCrFeNiMo high-entropy alloy cladding layer of the present invention has excellent friction-reducing and wear-resistant properties, and can therefore be used to improve the friction-reducing and wear-resistant properties of a substrate, thereby increasing the use efficiency and service life of the substrate.
[0012] In the present invention, the substrate is selected from metal materials, including but not limited to steel or nonferrous metals. Steel can be selected from carbon structural and low alloy structural steel (Q195, Q215A, Q215B, Q235A, Q235B, Q235C, etc.), high quality carbon structural steel and high quality carbon spring steel (08F, 20, 20A, 45, 45E, 65Mn, etc.), alloy structural steel and alloy spring steel (20CrMnSi, 35CrMo, 60Si2Mn, etc.), tool steel, bearing steel and stainless steel (2Cr13, 1Cr18Ni9), etc. Nonferrous metals can be selected from titanium alloys, aluminum alloys, copper alloys, etc.
[0013] The beneficial effects of the present invention are:
[0014] The micro-textured ion-sulfurized CoCrFeNiMo high-entropy alloy cladding layer of the present invention has excellent friction-reducing and wear-resistant properties, and can effectively improve the friction-reducing and wear-resistant properties of the substrate, thereby increasing the use efficiency and service life of the substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 Schematic diagram of micro-textured ion sulfurization process;
[0016] Figure 2 This is the color penetration test image of the CoCrFeNiMo high entropy alloy cladding layer on the surface of Q235 steel;
[0017] Figure 3 This is the cross-sectional hardness test analysis diagram of the CoCrFeNiMo high entropy alloy cladding layer;
[0018] Figure 4 SEM images of the pit texture and groove texture of the CoCrFeNiMo high entropy alloy cladding layer before sulfurization; wherein, (a) is a low-magnification SEM image of the pit texture, (b) is a high-magnification SEM image of the pit texture, (c) is a low-magnification SEM image of the groove texture, and (d) is a high-magnification SEM image of the groove texture;
[0019] Figure 5 The three-dimensional morphology of the pit texture and groove texture of the CoCrFeNiMo high entropy alloy cladding layer before sulfurization; wherein, (a) is a front view of the three-dimensional morphology of the pit texture, (b) is a side view of the three-dimensional morphology of the pit texture, (c) is a front view of the three-dimensional morphology of the groove texture, and (d) is a side view of the three-dimensional morphology of the groove texture;
[0020] Figure 6 The cross-sectional profile data diagram of the pit texture and groove texture of the CoCrFeNiMo high entropy alloy cladding layer before sulfurization; wherein (a) is the cross-sectional profile (depth) diagram of the pit texture, and (b) is the cross-sectional profile (depth) diagram of the groove texture;
[0021] Figure 7 This is the pit texture pattern after sanding with sandpaper;
[0022] Figure 8 This is the XPS elemental analysis diagram of the internal material of the CoCrFeNiMo high entropy alloy cladding layer after sulphurization of the pit texture and groove texture;
[0023] Fig. 9 The SEM images of the pit texture and groove texture of the CoCrFeNiMo high entropy alloy cladding layer after sulfurization; wherein, (a) is a low-magnification SEM image of the pit texture, (b) is a high-magnification SEM image of the pit texture, (c) is a low-magnification SEM image of the groove texture, and (d) is a high-magnification SEM image of the groove texture;
[0024] Fig.10 The friction coefficient of different cladding layers changes with time;
[0025] Fig.11SEM images of the wear scar morphologies of different cladding layers; among them, (a) is the wear scar morphology of the non-ion-sulfurized cladding layer, (b) is the wear scar morphology of the coating with general ion-sulfurized process, (c) is the wear scar morphology of the cladding layer with only texture, and (d) is the wear scar morphology of the micro-textured ion-sulfurized CoCrFeNiMo high-entropy alloy cladding layer of the present invention; the wear scar widths are 1200μm, 879μm, 511μm, and 453μm, respectively. DETAILED DESCRIPTION
[0026] Compared with the general ion sulfurization process, the present invention also performs micro-texturing on the substrate before the ion sulfurization process. In order to intuitively show the difference between the micro-texturized ion sulfurization process and the general ion sulfurization process, the present invention provides Figure 1 , for basic display and understanding.
[0027] The CoCrFeNiMo high entropy alloy powder used in the present invention is prepared by the following method: atomized powder CoCrFeNi and elemental powder Mo are uniformly mixed in a molar ratio of 1:1, and dried and dehumidified at 120° C. to obtain the CoCrFeNiMo high entropy alloy powder.
[0028] The substrate used in the present invention is Q235 steel (with a size of about 100 mm×50 mm×10 mm), and its surface needs to be polished with a grinder to remove oxide scale before laser cladding.
[0029] The laser cladding of the present invention is carried out in a HWF60 composite welding robot workstation with argon protection. The laser output by the IPG YLS-6000 fiber laser is transmitted via optical fiber to a rectangular spot cladding head fixed on a FANUC robot (model R-1000iA / 100F).
[0030] The present invention adopts a YLP-MP20 laser marking machine to prepare surface microtexture. The laser is mainly composed of an IPGMOPA fiber laser, a main control system, a software operating system, and a German ScanLab galvanometer system. The laser outputs a laser beam with a wavelength of 1064nm during operation, and after the beam is expanded by a beam expander and reflected by a galvanometer system, the laser beam is moved on a two-dimensional plane under the action of a control system, and the laser beam is focused by a focusing lens, and finally a fine high-energy spot is formed on the surface of the sample, so that the processed surface is instantly vaporized, and radiated point by point on the surface of the sample according to a pre-set pattern, and finally a texture morphology with a certain depth and width is formed.
[0031] The present invention adopts LDMC-15A pulse ion sulfurizing furnace to carry out low-temperature ion sulfurizing.
[0032] The present invention adopts TIME6610M semi-automatic microhardness tester to measure the microhardness of the cross section of the cladding layer sample, loads 1.96N, maintains the load for 15s, tests once every 0.1mm from the surface of the cladding layer sample vertically downward to the substrate, and takes the average value of three tests.
[0033] The present invention adopts PHI-Versaprobe 5000III X-ray photoelectron spectrometer to perform XPS analysis on the sulfurized sample, the X-ray source is a monochromatic AlKa source, the energy is 1486.6eV, the voltage is 15kV, and the beam current is 4.5mA.
[0034] The present invention adopts Zeta-20 surface profiler to observe the three-dimensional morphology of the texture surface of the cladding layer.
[0035] The terms used in the present invention, unless otherwise specified, generally have the meanings commonly understood by those of ordinary skill in the art. The present invention will be further described in detail below in conjunction with specific examples and with reference to data. The following examples are intended to illustrate the present invention and are not intended to limit the scope of the present invention in any way.
[0036] Example 1
[0037] The preparation steps of micro-textured ion-sulfurized CoCrFeNiMo high entropy alloy cladding layer are as follows:
[0038] (1) Laser cladding
[0039] The CoCrFeNiMo high entropy alloy powder was evenly laid on the surface of Q235 steel with a thickness of 2mm for laser cladding. The laser cladding conditions were as follows: laser power 1800W, cladding speed 300mm / min, overlap rate 30%, spot size 10mm×1mm, protective gas 4L / min. After each cladding, another layer of powder was laid on the overlapping part, and finally a cladding layer with a thickness of about 1mm was formed. After the cladding layer sample was air-cooled to room temperature, impurities such as surface oxide slag were removed with a grinder.
[0040] The cladding layer samples were subjected to color penetrant testing, such as Figure 2 As shown in the figure, the CoCrFeNiMo high entropy alloy powder is well formed after cladding, and no red color reaction is found when it is tested with a flaw detector, indicating that the cladding layer has no cracks and no flaw detection defects. This shows that the high entropy alloy prepared by the present invention has high advantages in composition and formulation. The cross-section hardness of the cladding layer sample is tested, and the results are as follows: Figure 3 As shown, the hardness of the high entropy alloy layer on the substrate surface after cladding is several times higher than that of the substrate.
[0041] (2) Texture treatment
[0042] After no defects were found after flaw detection, the cladding layer samples were cut into samples of the required size (15mm×15mm×10mm) by electric spark wire cutting, and then ground and polished with 600#, 1000#, 1500#, and 2000# sandpaper respectively, placed in anhydrous ethanol for ultrasonic cleaning for 30 minutes, and then blown dry for use.
[0043] The pit texture and groove texture were constructed on the surface of different cladding layer samples. ① The marking parameters of the pit texture are: diameter 200μm, center distance 600μm, surface density 8.727%, power 17W, marking speed 200mm / s, filling radius 0.005mm, marking times 1 time, empty jump speed 3000mm / s, Q frequency 25khz, Q release 1μs, forming a texture pattern, the texture pattern is a uniformly distributed pit array. ② The marking parameters of the groove texture are: width 60μm, center distance 400μm, surface density 15%, power 16W, marking speed 400mm / s, marking times 5 times, empty jump speed 3000mm / s, Q frequency 25khz, Q release 1μs, forming a texture pattern, the texture pattern is parallel grooves.
[0044] The pit and groove texture Figure 4 As shown in Figure 2, there are craters and burrs on the surface of the cladding layer. The three-dimensional morphology of the pit and groove texture is shown in Figure 2. Figure 5 As shown in Figure 2, the cross-sectional profile (depth) of the pit and groove texture is as follows: Figure 6 As shown by Figure 5 and Figure 6 It can be seen that texturing treatment can cause physical changes to the surface of the cladding layer. The pits or grooves formed can not only increase the sulfurization area and sulfurization thickness of the cladding layer surface, but also store grinding chips and lubricating media, reduce the wear of abrasive particles on the friction pair, and prevent the loss of lubricating media.
[0045] The texture pattern was lightly ground and polished in one direction with 2000# sandpaper to eliminate the craters and burrs on the surface of the cladding layer, and ultrasonically cleaned in anhydrous ethanol for 30 minutes to remove the residual polishing paste, oil stains and other stains on the surface, and then dried for later use. Figure 7 As shown, after grinding, the craters on the surface of the cladding layer are smoothed and the burrs disappear.
[0046] (3) Sulfurization treatment
[0047] The cladding layer sample after the above texture treatment was subjected to sulfurization treatment. The parameters of the sulfurization treatment were: voltage 660V, holding temperature 280℃, H2S gas flow rate 24sccm, and holding time 2h. After the sulfurization treatment, a micro-textured ion-sulfurized CoCrFeNiMo high-entropy alloy cladding layer was obtained.
[0048] XPS elemental analysis of the material inside the pit and groove texture Figure 8As shown in Figure 1, the pit and groove texture contains sulfides such as MoS2 and MoS, which proves the success of the sulfurization treatment. The SEM image of the pit and groove texture after sulfurization is shown in Figure 1. Fig. 9 As shown in the figure, there are fluffy substances inside the pit and groove texture, which can be compared with Figure 8 Mutual verification confirms that the fuzzy substances in the pit and groove texture are sulfides (the main substance of the sulfurized layer), which further verifies that the combination of texture and sulfurization can cause great changes in the physical structure of the cladding layer, which is beneficial to the improvement of wear resistance.
[0049] Friction and wear test
[0050] A dry friction test was performed on the micro-textured ion-sulfurized CoCrFeNiMo high entropy alloy cladding layer (pit pattern) prepared in Example 1. At the same time, three control groups were set up: Control group A was a non-ion-sulfurized cladding layer, which was a CoCrFeNiMo high entropy alloy cladding layer formed by laser cladding on the surface of Q235 steel; Control group B was a general ion-sulfurized process coating, which was obtained by sulfurizing the CoCrFeNiMo high entropy alloy cladding layer; Control group C was a cladding layer with only texture, which was obtained by texturing the CoCrFeNiMo high entropy alloy cladding layer.
[0051] The test instrument is a WTM-2E micro friction and wear tester, and the test parameters are as follows: rotation speed 500r / min, rotation radius 2.5mm, load 1.96N, friction time 1h. The grinding ball is made of GCr15 material with a diameter of 5mm.
[0052] The test results are as follows Fig.10 and Fig.11 shown.
[0053] Depend on Fig.10 It can be seen that compared with the general ion sulfurizing process, the friction coefficient of the process of the present invention is lower, which means that the alloy cladding layer prepared by the present invention is more wear-resistant. At the same time, the friction coefficient of the cladding layer is higher when the ion sulfurizing or texturing treatment is performed alone than when the two are combined. This shows that the friction coefficient of the cladding layer can be further effectively reduced by performing sulfurizing and texturing treatment on the cladding layer at the same time. There is a synergistic effect between ion sulfurizing and texturing treatment.
[0054] Depend on Fig.11 (a) It can be seen that there are large abrasive particles on the wear scar, the furrow is deep, and the wear loss is large, which belongs to abrasive wear. Fig.11 (b) It can be seen that after sulfurization, the wear scar is relieved a lot, the wear particles are reduced, the furrows are shallow, and the wear weight loss is reduced. Fig.11 (c) It can be seen that after adding texture, the abrasive particles and furrows on the wear scar disappear, showing adhesive wear. Fig.11(d) It can be seen that the wear scars of the texture and sulfurization are lighter and smaller in area, and the weight loss is minimal.
[0055] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.
Claims
1. A micro-textured ion-sulfurized CoCrFeNiMo high-entropy alloy cladding layer, characterized in that: The method is to clad CoCrFeNiMo high entropy alloy powder on the substrate surface, and sequentially perform microtexturing and sulfurization treatment on the cladding layer; The CoCrFeNiMo high entropy alloy powder is obtained by uniformly mixing atomized powder CoCrFeNi and elemental powder Mo in a molar ratio of 1:1, and drying the mixture at 100-150° C. The cladding is laser cladding; the laser cladding conditions are: laser power 1800W, cladding speed 300mm / min, overlap rate 30%, spot size 10mm×1mm, shielding gas 4L / min, after each cladding, a layer of alloy powder is spread on the overlapped part, and finally a cladding layer with a thickness of 1mm is formed; The microtexture is formed by processing the surface of the CoCrFeNiMo high entropy alloy cladding layer to form a pit array or parallel grooves; The texture parameters of the pit array are as follows: diameter 200 μm, center distance 600 μm, surface density 8.727%, power 17 W, marking speed 200 mm / s, filling radius 0.005 mm, marking times 1 time, empty jump speed 3000 mm / s, Q frequency 25 khz, Q release 1 μs; The texture parameters of the parallel grooves are as follows: width 60 μm, center distance 400 μm, surface density 15%, power 16 W, marking speed 400 mm / s, marking times 5 times, jump speed 3000 mm / s, Q frequency 25 khz, Q release 1 μs; The sulfurization treatment is to perform ion sulfurization treatment on the surface of the CoCrFeNiMo high entropy alloy cladding layer after microtexturing; the sulfurization treatment parameters are: voltage 660V, insulation temperature 280°C, H2S gas flow rate 24sccm, and insulation time 2h.
2. Application of the micro-textured ion-sulfurized CoCrFeNiMo high-entropy alloy cladding layer according to claim 1 to improve the wear-reducing and wear-resistant properties of the substrate.
3. The use according to claim 2, characterized in that: The substrate is made of metal material.
4. The use according to claim 3, characterized in that: The metal material is selected from steel or nonferrous metal.
5. The use according to claim 4, characterized in that: The steel is selected from carbon structural steel or alloy structural steel.
6. The use according to claim 4, characterized in that: The steel is selected from high-quality carbon spring steel or alloy spring steel.
7. The use according to claim 4, characterized in that: The steel is selected from tool steel, bearing steel or stainless steel.
8. The use according to claim 4, characterized in that: The non-ferrous metal is selected from titanium alloy, aluminum alloy or copper alloy.