A fuel cell gas diffusion layer and a preparation method thereof and a fuel cell

By using a gas diffusion layer combined with a carbon fiber base layer and a microporous layer in the fuel cell, the problem of water retention effect of the fuel cell under low humidity conditions and water management under high humidity conditions is solved, and the operation without water cooling system and humidification system is realized. Simplifies system design and reduces weight and complexity.

CN114464834BActive Publication Date: 2024-10-18SHENZHEN GENERAL HYDROGEN ENERGY TECH CORP LTD

Patent Information

Application Number
CN202210088485.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-25
Publication Date
2024-10-18
Estimated Expiration
2042-01-25

AI Technical Summary

Technical Problem

Existing fuel cells require additional water cooling systems and humidification systems to deal with heat and humidity issues, resulting in increased system complexity and occupied space and weight.

Method used

A gas diffusion layer combining a carbon fiber base layer and a microporous layer is used. Through hydrophobic treatment and sintering process of polymer mixed slurry, a gas diffusion layer with self-humidifying function is formed, reducing dependence on water cooling and humidification systems.

Benefits of technology

It achieves good water retention under low humidity conditions, avoids occupying additional space and weight, and prevents flooding under high humidity conditions, simplifying the process and reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114464834B_ABST
    Figure CN114464834B_ABST
Patent Text Reader

Abstract

The present invention discloses a fuel cell gas diffusion layer and a preparation method thereof and a fuel cell, wherein a fuel cell gas diffusion layer comprises a carbon fiber base layer and a microporous layer, the microporous layer is arranged on the carbon fiber base layer, and the microporous layer comprises 9 to 15 parts of carbon black, 5 to 15 parts of hydrophilic polymer, 5 to 15 parts of polytetrafluoroethylene, and 70 to 90 parts of water by weight. The gas diffusion layer comprises a hydrophilic polymer, which improves the water retention effect of the gas diffusion layer, so that the gas diffusion layer has a self-humidification function, and the hydrophilic polymer cooperates with polytetrafluoroethylene to hydrophobic the gas diffusion layer, so that the gas diffusion layer does not need to be provided with a water cooling system and a humidification system, thereby reducing the space and weight of the fuel cell itself.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a fuel cell gas diffusion layer and a preparation method thereof, and a fuel cell. Background Art

[0002] Hydrogen energy is considered to be the cleanest energy with the greatest development potential in this century. Proton exchange membrane hydrogen-oxygen fuel cells are a new type of energy utilization method. Proton exchange membrane hydrogen-oxygen fuel cells can directly convert the chemical energy of fuel into electrical energy, so they are not restricted by the Carnot cycle and have the advantages of high power, simple structure, and easy operation.

[0003] The fuel cell is mainly composed of gas diffusion layers on the anode and cathode sides, bipolar plates, catalyst layers, and proton exchange membranes in the middle layer. The gas diffusion layer is one of the important core components and has many important functions. The gas diffusion layer mainly provides a path for the reaction gas to the catalyst layer, conducts water generated in the catalyst layer, conducts electricity and heat, and supports the catalyst layer.

[0004] Fuel cells generate a certain amount of heat when working, so conventional fuel cells are equipped with a water cooling system and a humidification system. The water cooling system is used to adjust the temperature of the battery. This not only increases the complexity of the system, but also takes up a certain amount of space and weight of the fuel cell itself, which is not conducive to portability. How to develop a gas diffusion layer that is resistant to low humidity and has a certain degree of water retention has become a technical problem that needs to be solved urgently. Summary of the invention

[0005] Based on this, it is necessary to provide a fuel cell gas diffusion layer and a preparation method thereof and a fuel cell to solve the technical problem in the prior art that the fuel cell needs to add a water cooling system and a humidification system, thereby occupying a certain amount of space and weight of the fuel cell itself.

[0006] The present invention provides a fuel cell gas diffusion layer, comprising a carbon fiber base layer and a microporous layer, wherein the microporous layer is arranged on the carbon fiber base layer, and the microporous layer comprises, by mass:

[0007]

[0008]

[0009] Furthermore, the hydrophilic polymer includes one or more of polyaniline, polydopamine, polyvinyl pyrrolidone, polyethylene glycol, polyvinyl alcohol, and phenolic resin.

[0010] Furthermore, the thickness of the carbon fiber base layer is 0.18 mm to 0.25 mm.

[0011] The present invention provides a method for preparing a fuel cell gas diffusion layer, comprising:

[0012] Performing hydrophobic treatment on the carbon fiber base layer;

[0013] The carbon black, the hydrophilic polymer, the polytetrafluoroethylene emulsion of the first concentration and water are stirred and mixed to form a mixed slurry;

[0014] Applying the mixed slurry on the hydrophobically treated carbon fiber base layer to obtain a first intermediate;

[0015] The first intermediate is dried at a temperature of 60 to 80° C. for 10 to 30 minutes to obtain a second intermediate;

[0016] The second intermediate is sintered at a temperature of 350-370° C. for 10-30 minutes to obtain a fuel cell gas diffusion layer.

[0017] Furthermore, the first concentration is 30% to 50%.

[0018] Furthermore, the hydrophobicity of the carbon fiber base layer after the hydrophobic treatment is 25% to 30%.

[0019] Furthermore, the hydrophobic treatment of the carbon fiber base layer includes:

[0020] The carbon fiber base layer is immersed in the polytetrafluoroethylene emulsion of the second concentration for a time of 0.5 to 10 minutes;

[0021] The impregnated carbon fiber base layer is dried at a temperature of 50 to 70° C. for 8 to 12 minutes.

[0022] Furthermore, the second concentration is 1% to 10%.

[0023] The present invention also provides a fuel cell, comprising the fuel cell gas diffusion layer.

[0024] The present invention provides a battery fuel gas diffusion layer, comprising a carbon fiber base layer and a microporous layer, wherein the microporous layer is arranged on the carbon fiber base layer, and the microporous layer comprises 9 to 15 parts of carbon black, 5 to 15 parts of hydrophilic polymer, 5 to 15 parts of polytetrafluoroethylene, and 70 to 90 parts of water by weight. The gas diffusion layer comprises a hydrophilic polymer, which improves the water retention effect of the gas diffusion layer, so that the gas diffusion layer has a self-humidification function, and the hydrophilic polymer cooperates with polytetrafluoroethylene to repel the gas diffusion layer, so that the gas diffusion layer does not need to be provided with a water cooling system and a humidification system, thereby reducing the space and weight of the fuel cell itself. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0026] Figure 1 Schematic diagram of the structure of a gas diffusion layer of a fuel cell in an embodiment of the present invention;

[0027] Figure 2 This is a diagram showing the hydrophilic effect of adding a hydrophilic polymer in an embodiment of the present invention;

[0028] Figure 3 This is a diagram showing the hydrophilic effect of an embodiment of the present invention without adding a hydrophilic polymer.

[0029] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0030] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] It should be noted that all directional indications in the embodiments of the present invention (such as up, down, left, right, front, back, etc.) are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.

[0032] In addition, the descriptions of "first", "second", etc. in the present invention are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, "and / or" in the full text includes three solutions. Taking A and / or B as an example, it includes technical solution A, technical solution B, and technical solution that satisfies both A and B. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the ability of ordinary technicians in this field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0033] like Figure 1 As shown, in some embodiments, a fuel cell gas diffusion layer 1 includes a carbon fiber base layer 2 and a microporous layer 3, the microporous layer 3 is disposed on the carbon fiber base layer 2, and the microporous layer 3 includes 9 to 15 parts of carbon black, 5 to 15 parts of hydrophilic polymer, 5 to 15 parts of polytetrafluoroethylene, and 70 to 90 parts of water by mass. The gas diffusion layer 1 includes a hydrophilic polymer to improve the water retention effect of the gas diffusion layer 1, so that the gas diffusion layer 1 has a self-humidification function, and the hydrophilic polymer cooperates with polytetrafluoroethylene to hydrophobic the gas diffusion layer, so that the gas diffusion layer 1 does not need to be provided with a water cooling system and a humidification system, thereby reducing the space and weight of the fuel cell itself.

[0034] like Figure 2 As shown in the figure, it is the hydrophilic effect diagram of adding hydrophilic polymer. Figure 3 The figure shows the hydrophilic effect without adding hydrophilic polymer. Figure 2 The contact angle is 139.42°. Figure 3 The contact angle is 161°. Figure 2 The contact angle is less than Figure 3 The smaller the contact angle, the better the hydrophilic effect. Therefore, after adding the hydrophilic polymer, the water retention effect of the fuel cell gas diffusion layer 1 is improved, and the gas diffusion layer 1 has a self-humidifying function. The hydrophilic polymer cooperates with the hydrophobic property of polytetrafluoroethylene and can replace the water cooling system and humidification system set in the fuel cell in the prior art.

[0035] Specifically, the hydrophilic polymer includes one or more of polyaniline, polydopamine, polyvinyl pyrrolidone, polyethylene glycol, polyvinyl alcohol, and phenolic resin.

[0036] More specifically, the mass percentage of the hydrophilic polymer is 5% to 10%.

[0037] Furthermore, the thickness of the carbon fiber base layer is 0.18 mm to 0.25 mm. Furthermore, the carbon black may be 50% compressed.

[0038] In another embodiment, a method for preparing a fuel cell gas diffusion layer includes:

[0039] S100, performing hydrophobic treatment on the carbon fiber base layer.

[0040] S200, stirring and mixing carbon black, a hydrophilic polymer, a polytetrafluoroethylene emulsion of a first concentration and water to form a mixed slurry.

[0041] S300, coating the mixed slurry on the hydrophobically treated carbon fiber base layer to obtain a first intermediate.

[0042] S400, drying the first intermediate at a temperature of 60 to 80° C. for 10 to 30 minutes to obtain a second intermediate.

[0043] S500: The second intermediate is sintered at a temperature of 350-370° C. for 10-30 minutes to obtain a fuel cell gas diffusion layer.

[0044] Specifically, the prior art discloses a microporous layer with a "hydrophilic-hydrophobic-hydrophilic" sandwich structure to achieve the purpose of gradient water retention, but such a method is cumbersome and complicated, which is not conducive to industrial production. The preparation method can simplify the complex, has a simple process, is convenient to prepare, requires less materials, and reduces production costs. Compared with the complexity and cumbersomeness of the prior art, the preparation method adopts a "one-pot method" to prepare a mixed slurry of the microporous layer, adopts a scraping method to coat it on the carbon fiber base layer (carbon paper surface), and sintered once to prepare a gas diffusion layer suitable for the anode and cathode of the air-cooled stack. The fuel cell can still have a good water retention effect under low humidity conditions, operate normally, and eliminate the humidification system, thereby saving space and reducing the weight of the battery itself. In addition, under high humidity conditions, due to the presence of hydrophobic pores, it can play a role in water management to prevent flooding, solving the problems of complex processes and water management of air-cooled stacks in the prior art.

[0045] More specifically, the blade thickness of the first intermediate body is 200 to 400 micrometers.

[0046] Furthermore, the hydrophobicity of the carbon fiber base layer is 25% to 30%. The drying process may be a baking process.

[0047] Specifically, the step of performing hydrophobic treatment on the carbon fiber base layer in S100 includes:

[0048] S110, immersing the carbon fiber base layer in a polytetrafluoroethylene emulsion of a second concentration for a time of 0.5 to 10 minutes;

[0049] S120, drying the impregnated carbon fiber base layer at a temperature of 50 to 70° C. for 8 to 12 minutes.

[0050] More specifically, the second concentration is 1% to 10%.

[0051] In another embodiment, a fuel cell includes a fuel cell gas diffusion layer.

[0052] In order to better illustrate the technical solution of the present invention, specific implementation methods are described in detail below.

[0053] Example 1

[0054] Embodiment 1 provides a method for preparing a fuel cell gas diffusion layer, and the specific steps are as follows:

[0055] (1) A 60% polytetrafluoroethylene emulsion was diluted to 5%, and a carbon fiber paper with a thickness of 0.2 mm was immersed in the diluted polytetrafluoroethylene emulsion for 0.5 min, then taken out and placed in a 60°C oven for drying for 10 min to obtain a carbon fiber base layer with a hydrophobicity of 25%.

[0056] (2) 9 g of carbon black, 6 g of polyaniline, 5 g of 40% polytetrafluoroethylene emulsion, and 80 g of deionized water were placed in a beaker and stirred at 800 rpm for 1 h, and then allowed to stand for 2 h to obtain a mixed slurry.

[0057] (3) The mixed slurry is scraped onto the carbon fiber base layer with a hydrophobicity of 25% in step (1), and the scraper thickness is adjusted to 350 μm to obtain a first intermediate.

[0058] (4) The first intermediate is placed in an oven at 60° C. and baked for 10 min to obtain a second intermediate.

[0059] (5) The temperature of the second intermediate is raised to 350° C. and sintering is continued for 10 min to obtain a fuel cell gas diffusion layer.

[0060] The above fuel cell gas diffusion layer and a commercial catalyst layer (Gore. Inc., PRIMEA Series 5510) were assembled into a membrane motor, and a fuel cell was assembled to test its performance.

[0061] Example 2

[0062] Embodiment 2 provides a method for preparing a fuel cell gas diffusion layer, and the specific steps are as follows:

[0063] (1) A 60% polytetrafluoroethylene emulsion was diluted to 5%, and a carbon fiber paper with a thickness of 0.2 mm was immersed in the diluted polytetrafluoroethylene emulsion for 0.5 min, then taken out and placed in a 60°C oven for drying for 10 min to obtain a carbon fiber base layer with a hydrophobicity of 25%.

[0064] (2) 9 g of carbon black, 6 g of polyvinyl pyrrolidone, 5 g of 40% polytetrafluoroethylene emulsion, and 80 g of deionized water were placed in a beaker and stirred at 800 rpm for 1 h, and then allowed to stand for 2 h to obtain a mixed slurry.

[0065] (3) The mixed slurry is scraped onto the carbon fiber base layer with a hydrophobicity of 25% in step (1), and the scraper thickness is adjusted to 350 μm to obtain a first intermediate.

[0066] (4) The first intermediate is placed in an oven at 60° C. and baked for 10 min to obtain a second intermediate.

[0067] (5) The temperature of the second intermediate is raised to 350° C. and sintering is continued for 10 min to obtain a fuel cell gas diffusion layer.

[0068] The above fuel cell gas diffusion layer and a commercial catalyst layer (Gore. Inc., PRIMEA Series 5510) were assembled into a membrane motor, and a fuel cell was assembled to test its performance.

[0069] Example 3

[0070] Embodiment 3 provides a method for preparing a fuel cell gas diffusion layer, and the specific steps are as follows:

[0071] (1) A 60% polytetrafluoroethylene emulsion was diluted to 5%, and a carbon fiber paper with a thickness of 0.2 mm was immersed in the diluted polytetrafluoroethylene emulsion for 0.5 min, then taken out and placed in a 60°C oven for drying for 10 min to obtain a carbon fiber base layer with a hydrophobicity of 25%.

[0072] (2) 9 g of carbon black, 6 g of polyvinyl pyrrolidone, 5 g of 30% polytetrafluoroethylene emulsion, and 80 g of deionized water were placed in a beaker and stirred at 800 rpm for 1 h, and then allowed to stand for 2 h to obtain a mixed slurry.

[0073] (3) The mixed slurry is scraped onto the carbon fiber base layer with a hydrophobicity of 25% in step (1), and the scraper thickness is adjusted to 350 μm to obtain a first intermediate.

[0074] (4) The first intermediate is placed in an oven at 60° C. and baked for 10 min to obtain a second intermediate.

[0075] (5) The temperature of the second intermediate is raised to 350° C. and sintering is continued for 10 min to obtain a fuel cell gas diffusion layer.

[0076] The above fuel cell gas diffusion layer and a commercial catalyst layer (Gore. Inc., PRIMEA Series 5510) were assembled into a membrane motor, and a fuel cell was assembled to test its performance.

[0077] Example 4

[0078] Example 4 provides a method for preparing a fuel cell gas diffusion layer, and the specific steps are as follows:

[0079] (1) A 60% polytetrafluoroethylene emulsion was diluted to 5%, and a carbon fiber paper with a thickness of 0.2 mm was immersed in the diluted polytetrafluoroethylene emulsion for 5 minutes, then taken out and placed in a 60°C oven for drying for 10 minutes to obtain a carbon fiber base layer with a hydrophobicity of 25%.

[0080] (2) 9 g of carbon black, 6 g of polyvinyl pyrrolidone, 5 g of 20% polytetrafluoroethylene emulsion, and 80 g of deionized water were placed in a beaker and stirred at 800 rpm for 1 h, and then allowed to stand for 2 h to obtain a mixed slurry.

[0081] (3) The mixed slurry is scraped onto the carbon fiber base layer with a hydrophobicity of 25% in step (1), and the scraper thickness is adjusted to 350 μm to obtain a first intermediate.

[0082] (4) The first intermediate is placed in an oven at 60° C. and baked for 10 min to obtain a second intermediate.

[0083] (5) The temperature of the second intermediate is raised to 350° C. and sintering is continued for 10 min to obtain a fuel cell gas diffusion layer.

[0084] The above fuel cell gas diffusion layer and a commercial catalyst layer (Gore. Inc., PRIMEA Series 5510) were assembled into a membrane motor, and a fuel cell was assembled to test its performance.

[0085] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification and drawings under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A method for preparing a fuel cell gas diffusion layer, characterized in that: Here are the steps: (1) diluting a 60% polytetrafluoroethylene emulsion to 5%, dipping a carbon fiber paper having a thickness of 0.2 mm in the diluted polytetrafluoroethylene emulsion for 0.5 min, taking it out, and drying it in a 60° C. oven for 10 min to obtain a carbon fiber base layer having a hydrophobicity of 25%; (2) 9 g of carbon black, 6 g of polyaniline, 5 g of 40% polytetrafluoroethylene emulsion, and 80 g of deionized water were placed in a beaker and stirred at 800 rpm for 1 h, and then allowed to stand for 2 h to obtain a mixed slurry; (3) applying the mixed slurry onto the carbon fiber base layer with a hydrophobicity of 25% in step (1) by scraping, and adjusting the scraper thickness to 350 μm to obtain a first intermediate; (4) baking the first intermediate in an oven at 60° C. for 10 min to obtain a second intermediate; (5) The temperature of the second intermediate is raised to 350° C. and sintering is continued for 10 min to obtain a fuel cell gas diffusion layer.

Citation Information

Patent Citations

  • Microporous layer with hydrophilic additives

    CN104541395A

  • Gas diffusion layer for fuel cell and preparation method and application thereof

    CN111029605A

Cited By

  • A gas diffusion layer and a preparation method thereof and a fuel cell made therefrom

    CN118572127B