A method for harmless disposal and resource recovery of secondary fly ash
Through the steps of acid washing, alkali preparation, zinc addition reduction and evaporation crystallization, the heavy metals in the secondary fly ash are separated and purified, which solves the problem of heavy metal enrichment in the secondary fly ash and achieves efficient resource recovery and harmless disposal. The heavy metal recovery rate is high, the process is environmentally friendly and there is no secondary pollution.
Patent Information
- Application Number
- CN202210097398.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-27
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2042-01-27
AI Technical Summary
Heavy metal elements such as zinc, lead, copper, and cadmium in secondary fly ash are further enriched under high temperature conditions, which increases the hazard and makes disposal more difficult. The existing high-temperature melting method cannot effectively solve this problem.
The heavy metal elements in the secondary fly ash are separated and purified by the steps of pickling, alkali preparation, zinc addition, reduction and evaporation crystallization, and through the alternating treatment of acid and alkali, to form high-purity zinc chloride, cadmium hydroxide and Metal copper and lead realize resource recycling.
Efficient recovery of heavy metals in secondary fly ash has been achieved, with the recovery rate of copper and cadmium reaching 99%, and the recovery rate of zinc and lead reaching 98%, and the harmless disposal of water-soluble salts and heavy metal salts has been achieved. The process There is basically no secondary pollution, and the moisture in the zinc chloride and secondary alkali cleaning solution can be recycled.
Smart Images

Figure CN114472482B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of harmless disposal and resource recovery of hazardous wastes, and in particular to a method for harmless disposal and resource recovery of secondary fly ash. Background Art
[0002] Waste incineration fly ash is a general term for solid particles separated from the gas purification system during the waste incineration process. Since fly ash contains high levels of dioxins and volatile heavy metals, it is generally defined as hazardous waste by various countries. According to my country's "List of Hazardous Wastes", waste incineration fly ash is clearly defined as hazardous waste that needs to be disposed of. At present, the conventional treatment methods for waste incineration fly ash are mostly chelation solidification, cement co-treatment, high-temperature melting treatment, and acid washing metal extraction.
[0003] The high-temperature melting method is one of the effective methods for large-scale harmless disposal of fly ash. After high-temperature melting treatment, dioxins in the fly ash are decomposed by heat, and non-volatile heavy metal elements are solidified in the glassy slag formed by melting, eliminating the risk of heavy metals leaching again. The final glassy slag can also be used as a building material. Therefore, the high-temperature melting method is considered to be a relatively thorough technology for harmless disposal of fly ash. However, most of the volatile heavy metals contained in fly ash will evaporate again under high temperature conditions through the promotion of chlorides in the fly ash, and mix with salts of alkali metals such as potassium and sodium to form secondary fly ash. Heavy metal elements such as zinc, lead, copper, and cadmium in secondary fly ash are further enriched, which is more harmful than ordinary fly ash and more difficult to dispose of. This has become a major technical problem affecting the promotion of the high-temperature melting method of fly ash.
[0004] Therefore, a method for harmlessly disposing of secondary fly ash and recycling resources is provided to solve the above problems. Summary of the invention
[0005] The technical problem to be solved by the present invention is that most of the volatile heavy metals contained in the current fly ash will volatilize again under high temperature conditions through the promotion of chlorides in the fly ash, and mix with salts of alkali metals such as potassium and sodium to form secondary fly ash. Heavy metal elements such as zinc, lead, copper, and cadmium in the secondary fly ash are further enriched, which is more harmful than ordinary fly ash and more difficult to dispose of. Therefore, a method for harmless disposal and resource recovery of secondary fly ash is provided, and the method for harmless disposal and resource recovery of secondary fly ash includes:
[0006] Step 1: primary pickling, adding water, acid solution and sodium hypochlorite to the secondary fly ash, and fully stirring, so that the pH value of the obtained slurry is the designed value PH1, and filtering the slurry to obtain the primary pickling liquid and the primary pickling filter residue;
[0007] Step 2: primary alkali modulation, adding alkali solution to the primary acid wash solution, fully stirring and adjusting the pH value to make the pH value reach the designed value PH2, filtering to obtain the primary alkali wash solution and the primary alkali wash residue;
[0008] Step 3: secondary alkali modulation, adding alkali solution to the primary alkali washing solution again, fully stirring and adjusting the pH value to make the pH value reach the designed value PH3, filtering to obtain the secondary alkali washing solution and the secondary alkali washing residue;
[0009] Step 4: secondary acid washing, adding acid solution to the primary alkali washing residue to fully dissolve the primary alkali washing residue and adjusting the pH of the resulting solution to the designed value of pH 4 to obtain a secondary acid washing solution;
[0010] Step 5: Add zinc for reduction, add zinc powder to the secondary pickling solution, stir thoroughly, so that the zinc powder replaces the copper and lead in the secondary pickling solution, and filter to obtain a reduced filtrate and a reduced filter residue;
[0011] Step 6: Evaporation and crystallization: the reduction filtrate is evaporated and crystallized to obtain zinc chloride crystals, which are recycled after steam condensation; the secondary alkaline washing liquid is neutralized by adding acid solution to acid-base neutrality, then evaporated and crystallized, and recycled after steam condensation.
[0012] Furthermore, the primary pickling filter residue is used to be put into a waste incinerator.
[0013] Furthermore, the main component of the secondary alkaline washing residue is cadmium hydroxide.
[0014] Furthermore, the main components of the reduced filter residue are metallic copper and lead.
[0015] Furthermore, the mixing mass ratio of secondary fly ash to water is 0.15-1.35, the mixing mass ratio of secondary fly ash to sodium hypochlorite is 250-1000, and the design value PH1 is 3.5±0.2.
[0016] Furthermore, in the first alkali modulation step and the second alkali modulation step, the added alkali solution is sodium hydroxide or potassium hydroxide.
[0017] Further, the design value PH2 is 9.3±0.3, preferably 9.3±0.15.
[0018] Further, the design value PH3 is 11.4±0.3, preferably 11.4±0.10.
[0019] Furthermore, the design value PH4 is 4.0±0.1.
[0020] Furthermore, the acid solution added in the first pickling, second pickling and evaporation crystallization steps is hydrochloric acid, nitric acid or a mixture thereof.
[0021] The implementation of the present invention has the following beneficial effects:
[0022] 1. The heavy metal element recovery rate of the present invention is high, and the recovery rate of copper and cadmium can reach more than 99%, and the recovery rate of zinc and lead can reach 98%.
[0023] 2. The present invention basically realizes complete resource-based harmless disposal of water-soluble salts and heavy metal salts in secondary fly ash, realizes classified purification of heavy metal elements enriched in secondary fly ash, recovers zinc chloride and cadmium hydroxide with high purity, and directly recovers lead and copper in the form of metal, which has high economic value.
[0024] 3. The process of the present invention generates substantially no secondary pollution, and the water evaporated from the zinc chloride solution and the secondary alkaline washing solution can be collected and recycled. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a flow chart of the present invention. DETAILED DESCRIPTION
[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example
[0027] Please refer to the instruction manual Figure 1 The technical problem to be solved in this embodiment is that most of the volatile heavy metals contained in the current fly ash will volatilize again under high temperature conditions through the promotion of chlorides in the fly ash, and mix with salts of alkali metals such as potassium and sodium to form secondary fly ash. Heavy metal elements such as zinc, lead, copper, and cadmium in the secondary fly ash are further enriched, which is more harmful than ordinary fly ash and more difficult to dispose of. Therefore, a method for harmless disposal and resource recovery of secondary fly ash is provided, and the method for harmless disposal and resource recovery of secondary fly ash includes:
[0028] Step 1: primary pickling 1. The main purpose of this step is to dissolve most of the heavy metal elements and separate them from the insoluble impurities in the secondary fly ash. The specific operation is to mix the secondary fly ash 7, water 8, acid solution 9 and sodium hypochlorite 10 in proportion and stir them fully, so that the acid solution and the secondary fly ash 7 react fully. The strong oxidizing property of sodium hypochlorite 10 prevents the metals (such as lead, copper, cadmium, etc.) that are sensitive to redox from forming colloids, thereby ensuring the full dissolution of heavy metal elements. The pH value of the obtained slurry is controlled at 3.5±0.2. After the slurry is fully stirred and allowed to stand, it is filtered to obtain a primary pickling liquid 11 and a primary pickling filter residue 12. Since most of the heavy metal components in the secondary fly ash 7 enter the primary pickling liquid 11 after pickling, the heavy metal content in the primary pickling filter residue 12 is extremely low, and it can be directly treated with reference to the disposal method of the bottom ash of garbage incineration, or it can be put into the garbage incinerator again.
[0029] Step 2: primary alkali modulation, the main purpose of this step is to separate the three metal elements of copper, zinc and lead from the primary pickling solution. The specific operation is to add alkali solution 13 to the primary pickling solution 11, fully stir and adjust the pH value to 9.3±0.3, preferably 9.3±0.15. Under this pH value condition, the copper, zinc and lead elements are converted into hydroxides insoluble in water, and the primary alkali washing solution and the primary alkali washing residue are obtained by filtration, wherein the primary alkali washing residue 15 is mainly composed of the hydroxides of the copper, zinc and lead elements.
[0030] Step 3: Secondary alkali modulation, the main purpose of this step is to further separate the cadmium element from the primary alkali washing solution. The specific operation is to add the alkali solution 13 to the primary alkali washing solution 14 again, fully stir and adjust the pH value to 11.4±0.3, preferably 11.4±0.10, and filter to obtain the secondary alkali washing solution 16 and the secondary alkali washing residue 17, wherein the secondary alkali washing solution 16 is mainly a solution of alkali metal salts and residual alkali, and the secondary alkali washing residue 17 is mainly composed of cadmium hydroxide.
[0031] Step 4: Secondary acid washing. The main purpose of this step is to dissolve the hydroxides of copper, lead and zinc in the primary alkali washing residue 15 again for subsequent separation. The specific operation is to add acid solution to the primary alkali washing residue 15 to fully dissolve the primary alkali washing residue and adjust the pH value of the obtained solution to 4.0±0.1 to obtain a secondary acid washing solution 18;
[0032] Step 5: Add zinc for reduction. The main purpose of this step is to replace the copper and lead metals in the secondary pickling solution 18 with zinc powder. The specific operation is to add zinc powder to the secondary pickling solution, stir it thoroughly, and filter it to obtain a reduced filtrate 20 and a reduced filter residue 21. The main components of the reduced filter residue are copper and lead metals, and the main component of the reduced filtrate is zinc chloride solution;
[0033] Step 6: Evaporation and crystallization. The reduction filtrate 20 is evaporated and crystallized to obtain zinc chloride crystals 22. The water vapor obtained by evaporation can be recycled after condensation. The secondary alkaline washing liquid is neutralized to acid-base neutrality and then evaporated and crystallized to obtain industrial salt 24 rich in elements such as sodium and potassium. The water vapor 23 obtained by evaporation can be recycled after condensation.
[0034] After the above steps, the metal elements such as zinc, lead, copper, cadmium, alkali metal salts and other impurities enriched in the secondary fly ash are separated out respectively and can be used for subsequent resource utilization. For example, the secondary alkali washing residue obtained in step 3 is cadmium hydroxide, and the reduction residue obtained in step 5 is mainly metal copper and lead, which can be smelted and purified later; the zinc chloride crystals and industrial salts obtained in step 6 are both important industrial raw materials. The heavy metal content in the primary acid washing residue obtained in step 1 is low, and it can be directly treated with reference to the disposal method of the bottom ash of garbage incineration, or it can be put into the garbage incinerator again.
[0035] In the first pickling step, the mixing mass ratio of secondary fly ash to water is 0.15-0.35, the mixing mass ratio of secondary fly ash to sodium hypochlorite is 250-1000, and the stirring and mixing time is not less than 30 minutes to ensure that the heavy metal elements in the secondary fly ash are fully dissolved.
[0036] In the primary alkali modulation and secondary alkali modulation steps, the alkali solution added is sodium hydroxide, which can also be replaced by potassium hydroxide.
[0037] In the primary pickling, secondary pickling and evaporation crystallization steps, the added acid solution can be hydrochloric acid, nitric acid or a mixture thereof, or can be replaced by a strong acidic liquid such as the acid solution obtained from a wet scrubber; the sodium hypochlorite added in the primary pickling step can be replaced by a strong oxidant such as hydrogen peroxide.
[0038] In the description of the present invention, it is necessary to understand that the terms "coaxial", "bottom", "one end", "top", "middle", "the other end", "upper", "one side", "top", "inside", "front", "center", "both ends" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.
[0039] In the present invention, unless otherwise clearly stipulated and limited, the terms such as "installation", "setting", "connection", "fixation" and "screw-on" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral one; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium; it can be the internal connection of two elements or the interaction relationship between two elements. Unless otherwise clearly defined, ordinary technicians in this field can understand the specific meanings of the above terms in the present invention according to the specific circumstances.
[0040] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for harmless disposal and resource recovery of secondary fly ash, It is characterized in that include: Step 1: primary pickling, adding water, acid solution and sodium hypochlorite to the secondary fly ash, and fully stirring, so that the pH value of the obtained slurry is the designed value PH1, filtering the slurry to obtain a primary pickling liquid and a primary pickling filter residue, wherein the mixing mass ratio of the secondary fly ash to water is 0.15-1.35, the mixing mass ratio of the secondary fly ash to sodium hypochlorite is 250-1000, the designed value PH1 is 3.5±0.2, and the primary pickling filter residue is used to be put into the waste incinerator; Step 2: primary alkali modulation, adding alkali solution to the primary acid wash solution, fully stirring and adjusting the pH value to make the pH value reach the designed value PH2, filtering to obtain the primary alkali wash solution and the primary alkali wash residue, the designed value PH2 is 9.3±0.3; Step 3: secondary alkali modulation, adding alkali solution to the primary alkali washing solution again, fully stirring and adjusting the pH value to make the pH value reach the designed value PH3, filtering to obtain the secondary alkali washing solution and the secondary alkali washing residue, the main component of the secondary alkali washing residue is cadmium hydroxide, and the designed value PH3 is 11.4±0.3; Step 4: secondary acid washing, adding acid solution to the primary alkali washing residue to fully dissolve the primary alkali washing residue and adjusting the pH of the resulting solution to the designed value PH4, to obtain a secondary acid washing solution, the designed value PH4 is 4.0±0.1; Step 5: Add zinc for reduction, add zinc powder to the secondary pickling solution, stir thoroughly, so that the zinc powder replaces the copper and lead in the secondary pickling solution, and filter to obtain a reduced filtrate and a reduced filter residue; Step 6: Evaporation and crystallization: the reduction filtrate is evaporated and crystallized to obtain zinc chloride crystals, which are recycled after steam condensation; the secondary alkaline washing liquid is neutralized by adding acid solution to acid-base neutrality, then evaporated and crystallized, and recycled after steam condensation.
2. The method for harmless disposal and resource recovery of secondary fly ash according to claim 1, It is characterized in that The main components of the reduced filter residue are metallic copper and lead.
3. The method for harmless disposal and resource recovery of secondary fly ash according to claim 1, It is characterized in that In the primary alkali modulation step and the secondary alkali modulation step, the added alkali solution is sodium hydroxide or potassium hydroxide.
4. The method for harmless disposal and resource recovery of secondary fly ash according to claim 1, It is characterized in that The acid solution added in the first pickling, second pickling and evaporation crystallization steps is hydrochloric acid, nitric acid or a mixture thereof.
5. The method for harmless disposal and resource recovery of secondary fly ash according to claim 1, It is characterized in that The design value PH2 is further 9.3±0.
15.
6. The method for harmless disposal and resource recovery of secondary fly ash according to claim 1, It is characterized in that The design value PH3 is further 11.4±0.10.
Citation Information
Patent Citations
Method for recycling rare earths from cathode-ray tube fluorescent powder
CN102796872A
Treatment method of soot of copper smelting furnace
CN104388686A
Method for recycling copper smelting furnace soot
CN104451170A
Resourceful treatment method for waste incineration fly ash
CN107626714A
Cadmium telluride glass recovery method