Gas field water associated resource recovery method
The sulfide in the gas field water was degraded through blowing and oxidation method, and combined with ozone catalytic oxidation and adsorption method, lithium, barium, potassium, chloride and bromine resources were recovered, solving the problem that resources in the prior art were not fully recovered and utilized. Achieved the effect of near-zero emissions.
Patent Information
- Application Number
- CN202311112725.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-31
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The prior art lacks effective methods for recycling and utilization of associated resources when treating gas field water, resulting in the failure to fully utilize valuable resources and the realization of near-zero emissions.
The sulfide degradation method is used to degrade sulfides, remove COD through ozone catalytic oxidation, extract lithium by adsorption method, and recover barium, potassium, chloride and bromine resources through a series of reactions and precipitation processes to achieve full recovery and close retrieval of resources. Zero emissions.
The full recycling and utilization of associated resources in the water of gas fields has been achieved, not only recycled valuable resources, but also achieved the effect of near-zero emissions, improving resource utilization efficiency and environmental protection.
Abstract
Description
Technical Field
[0001] The invention relates to a method for recycling wastewater resources, in particular to a method for recycling gas field water resources. Background Art
[0002] Gas field water refers to the water source of aquifers produced by exploiting oil and gas fields. In the process of oil and gas exploration and production, gas field water is an important by-product. Gas field water is mainly composed of water in underground aquifers, containing certain dissolved gases, suspended particles and dissolved solids.
[0003] At present, the treatment of gas field water is mainly based on post-treatment discharge, which aims to reduce environmental pollution, and there is little recycling of valuable resources. Summary of the invention
[0004] The technical problem to be solved by the present invention is to overcome the above-mentioned defects of the prior art and provide a method for recovering gas field water associated resources which can fully recover the associated resources.
[0005] The technical solution adopted by the present invention to solve the technical problem is as follows: A method for recovering gas field water associated resources comprises the following steps:
[0006] (1) Desulfurization treatment: Use stripping and oxidation methods to reduce the sulfide in gas field water to below 5 mg / L;
[0007] (2) COD removal: The COD in the gas field water is removed to below 50 mg / L through ozone catalytic oxidation;
[0008] (3) Lithium recovery: lithium is extracted by adsorption, and the remaining solution is the lithium extraction adsorption tail liquid;
[0009] (4) Barium recovery and hardness removal: adding sulfate to the lithium extraction adsorption tail liquid for reaction, after the reaction is complete, solid-liquid separation is performed to obtain filter residue 1 and filtrate 1; filter residue 1 is barium sulfate precipitate; adding alkali to filtrate 1 to a pH value of 10-12, after the reaction is complete, solid-liquid separation is performed to obtain filter residue 2 and filtrate 2; adding carbonate to filtrate 2, after the reaction is complete, solid-liquid separation is performed to obtain filter residue 3 and filtrate 3;
[0010] (5) Potassium and sodium recovery: the filtrate 3 is evaporated and concentrated to precipitate sodium chloride, and solid-liquid separation is performed to obtain sodium chloride precipitate and mother liquor 1. The concentration endpoint is determined based on the ion concentration and the K, Na / Cl- ternary phase diagram; the mother liquor 1 is cooled and crystallized, and solid-liquid separation is performed to obtain potassium chloride precipitate and mother liquor 2;
[0011] (6) Bromine resource recovery: Acidification of the mother liquor 2 to a pH value of 2-5 is introduced, chlorine gas is introduced for oxidation, hot air is blown out, and the mixture is absorbed by an aqueous sulfur dioxide solution to obtain an absorption liquid; chlorine gas is introduced into the absorption liquid for oxidation, hot air is blown out, and crude bromine and bromine extraction tail liquid are obtained.
[0012] By adopting the above technical solution, the associated resources in the gas field water are fully recycled and utilized; not only are valuable resources recovered, but also near-zero emissions are achieved.
[0013] Preferably, in step (1), air is introduced into the gas field water to blow out the sulfide in the water in the form of hydrogen sulfide to obtain a primary desulfurization liquid; an oxidant is added to the primary desulfurization liquid to oxidize the sulfide into a single substance, and the solid and liquid are separated to obtain a secondary desulfurization liquid, thereby completing the desulfurization.
[0014] The blown hydrogen sulfide can be absorbed by alkaline solution and then further refined or recycled; after stripping, the sulfide in the gas field water can be reduced to below 50 mg / L; after further oxidation treatment, the sulfide can be reduced to below 5 mg / L. By adopting the above technical solution, the sulfide content can be well reduced, which is conducive to subsequent processing and extraction.
[0015] Preferably, in step (1), the ratio of the gas field water to the air is 1L:25-150L.
[0016] By adopting the above technical solution, a better stripping and desulfurization effect is achieved.
[0017] Preferably, in step (1), the oxidant is sodium hypochlorite or sodium hypochlorite solution; the added amount is 25-100 mg / L of effective chlorine.
[0018] By adopting the above technical solution, a better oxidation desulfurization effect is achieved.
[0019] Preferably, in step (2), the ozone introduction rate is 0.5-1 L / min.
[0020] By adopting the above technical solution, a better effect of oxidative COD removal is achieved.
[0021] Preferably, in step (2), the time of ozone catalytic oxidation treatment is 0.5-2h.
[0022] By adopting the above technical solution, a better effect of oxidative COD removal is achieved.
[0023] The catalyst used for ozone catalytic oxidation may be the product in CN102872884B, or other catalysts used for ozone catalytic oxidation may be used.
[0024] Preferably, in step (3), an adsorbent for lithium extraction is used to extract lithium, and water is used to desorb to obtain a lithium-rich desorption solution. An ion exchange resin is used to remove calcium, magnesium, barium and boron in the lithium-rich desorption solution, and the solution is concentrated. Sodium carbonate solution is added to carry out lithium precipitation reaction to obtain lithium carbonate precipitate.
[0025] By adopting the above technical solution, lithium resources in gas field water can be recovered.
[0026] Preferably, in step (3), the adsorption rate is 2-6 BV / h.
[0027] By adopting the above technical solution, a better adsorption and extraction effect is achieved.
[0028] Preferably, in step (3), the desorption rate is 1-3 BV / h.
[0029] By adopting the above technical solution, a better desorption effect is achieved.
[0030] The adsorbent for lithium extraction by adsorption may be the product in CN111905700B, or other adsorbents for lithium extraction by adsorption may be used.
[0031] The adsorption process can adopt a continuous ion exchange process, and the required equipment can be purchased from the market.
[0032] Ion exchange resins for removing calcium, magnesium, barium and boron are commercially available.
[0033] Preferably, in step (3), the concentration is carried out by reverse osmosis concentration and / or evaporation concentration.
[0034] By adopting the above technical solution, the lithium ion concentration is increased, which is convenient for further processing.
[0035] Preferably, in step (3), the Li in the concentrated solution after concentration is ≥ 20 g / L.
[0036] By adopting the above technical solution, the lithium ion concentration is more suitable, which is convenient for further processing.
[0037] Preferably, in step (3), the temperature of the lithium precipitation reaction is 80-90° C., and the reaction time is 0.5-2 h.
[0038] By adopting the above technical solution, a better lithium deposition effect is achieved.
[0039] Preferably, in step (3), the concentration of the sodium carbonate solution is 15-25% by mass.
[0040] By adopting the above technical solution, a better lithium deposition effect is achieved.
[0041] The obtained lithium carbonate precipitate is an industrial-grade lithium carbonate product after ordinary washing and drying.
[0042] Preferably, in step (4), the amount of sulfate added is 1.05-1.3 times the molar amount of barium in the solution.
[0043] By adopting the above technical solution, the barium ions are completely precipitated.
[0044] Preferably, in step (4), the amount of the base added is 1.05-1.3 times the molar amount of magnesium in the solution.
[0045] By adopting the above technical solution, magnesium ions are completely precipitated.
[0046] Preferably, in step (4), the amount of carbonate added is 1.05-1.3 times the molar amount of calcium in the solution.
[0047] By adopting the above technical solution, calcium ions are completely precipitated.
[0048] Preferably, in step (4), the sulfate is potassium sulfate and / or sodium sulfate.
[0049] By adopting the above technical solution, a better barium deposition effect is achieved.
[0050] Preferably, in step (4), the base is potassium hydroxide and / or sodium hydroxide.
[0051] By adopting the above technical solution, a better magnesium deposition effect is achieved.
[0052] Preferably, in step (4), the carbonate is potassium carbonate and / or sodium carbonate.
[0053] By adopting the above technical solution, a better calcium precipitation effect is achieved.
[0054] The barium sulfate precipitate is an industrial-grade barium sulfate product after ordinary washing and drying.
[0055] The filter residue 2 is magnesium hydroxide, and the filter residue 3 is calcium hydroxide, which can be further refined or recycled. Removing calcium and magnesium ions from water reduces water hardness, which is beneficial to avoiding subsequent evaporator scaling.
[0056] The filtrate 3 is a high-sodium, low-potassium mother liquor. According to the phase diagram, after evaporation and concentration to sodium chloride saturation, evaporation and crystallization are continued to precipitate sodium chloride crystals; the mother liquor 1 is the mother liquor that evaporates and crystallizes sodium chloride until potassium chloride begins to be saturated, and then the temperature is lowered and crystallized to precipitate potassium chloride.
[0057] The sodium chloride precipitate obtained in step (5) can be dried to obtain a first-grade industrial salt; the potassium chloride precipitate can be dried to obtain a first-grade potassium chloride product.
[0058] Preferably, in step (6), the calculation formula for the amount of chlorine introduced into the chlorine oxidation is as follows:
[0059] Chlorine consumption (g) = bromine content (g) × 0.444 × chlorine ratio (%)
[0060] The chlorine ratio ranges from 110% to 130%.
[0061] By adopting the above technical solution, a better oxidation effect is achieved.
[0062] Preferably, in step (6), the temperature of the hot air is 60-90°C; and the gas-liquid ratio of the hot air blown out is 100-160L:1L.
[0063] By adopting the above technical solution, a better blowing effect is achieved.
[0064] Acidification can be carried out using acids that do not participate in other reactions, such as hydrochloric acid, sulfuric acid, and nitric acid.
[0065] When the absorption liquid is oxidized and blown out again, the chlorine gas introduced into the absorption liquid reacts with the hydrobromic acid in the absorption liquid to generate hydrogen chloride and free bromine. The hydrogen chloride turns into hydrochloric acid when it meets water. The free bromine is evaporated in the heating process (heating with hot air) to form bromine vapor. The bromine vapor becomes crude bromine after cooling.
[0066] Industrial secondary bromine can be obtained after distillation of crude bromine: the crude bromine is heated to the boiling point of bromine (58.5°C) to convert chlorine and bromine into a mixed gas. Then, by controlling the reflux condensation temperature of the distillation (controlled at 30-40°C), the bromine is purified to obtain industrial secondary bromine.
[0067] The present invention first performs desulfurization treatment, and sulfide in water is easy to generate hydrogen sulfide gas, which has great safety hazards; COD is removed before adsorption, mainly because COD is easy to affect the adsorption effect of the adsorbent; alkali needs to be added in the barium recovery and hardness removal process, and lithium extraction before this can reduce the amount of reagents and improve production efficiency; calcium and magnesium are removed before potassium and sodium are recovered to prevent scaling of the evaporator; the mother liquor obtained after bromine extraction by air blowing method is strongly acidic, so bromine recovery is finally performed to reduce the amount of reagents and improve production efficiency.
[0068] The present invention can fully recycle the associated resources in the gas field water to achieve near-zero emissions: in step (1) of the present invention, the desulfurization treatment blows out the sulfide in the water in the form of hydrogen sulfide, and the blown hydrogen sulfide can be absorbed by alkaline solutions such as sodium hydroxide and potassium hydroxide, and then further refined or recycled; the sulfur element produced by oxidation can be recycled after solid-liquid separation. In step (3), the eluent collected from the resin column for removing calcium, magnesium and barium and the resin for removing boron during lithium extraction can be further recycled. In step (4), the filter residue 1 is a barium sulfate precipitate, which is an industrial-grade barium sulfate product after ordinary washing and drying; the filter residue 2 is magnesium hydroxide, and the filter residue 3 is calcium hydroxide, which can be further refined or recycled. In step (5), the sodium chloride precipitate obtained can be dried to obtain a first-grade industrial salt; the potassium chloride precipitate can be dried to obtain a first-grade potassium chloride product. In step (6), the bromine extraction tail liquid and the acidified mother liquor remaining after the bromine resource recovery can be returned to the bromine resource recovery process for utilization.
[0069] Beneficial effects of the present invention:
[0070] 1. The associated resources in the gas field water were fully recycled and utilized;
[0071] 2. The present invention not only recycles valuable resources, but also achieves near-zero emissions. BRIEF DESCRIPTION OF THE DRAWINGS DETAILED DESCRIPTION
[0072] The present invention will be further described below with reference to the embodiments.
[0073] Unless otherwise specified, the raw materials, products and equipment used in the embodiments of the present invention are obtained through conventional commercial channels.
[0074] Example 1
[0075] The main component data of the gas field water in this embodiment are shown in the following table.
[0076] Table 1 Main components of gas field water extraction lithium tail liquid
[0077] index <![CDATA[Li + ]]> <![CDATA[Na + ]]> <![CDATA[K + ]]> <![CDATA[Ca 2+ ]]> <![CDATA[Mg 2+ ]]> <![CDATA[Ba 2+ ]]> content(%) 0.01438 2.5310 0.2447 0.1607 0.0305 0.1109 index <![CDATA[Sr 2+ ]]> <![CDATA[B2O3]]> <![CDATA[Cl - ]]> <![CDATA[Br - ]]> Sulfide COD content(%) 0.0193 0.0387 4.8194 0.0231 0.0174 185
[0078] The catalyst used for ozone catalytic oxidation in this embodiment is the product in CN102872884B; the adsorbent used for lithium adsorption extraction is the product in CN111905700B.
[0079] The method for recovering gas field water-associated resources in this embodiment comprises the following steps:
[0080] (1) Desulfurization treatment: 15 kg of lithium tail liquid extracted from gas field water was taken and subjected to primary desulfurization by air stripping method. Air was introduced into the gas field water at a liquid-to-gas ratio of 1:50 (L / L) to blow out the sulfide in the water in the form of hydrogen sulfide. The blown hydrogen sulfide was absorbed by sodium hydroxide solution, and the sulfide in the water was reduced to 35.2 mg / L to obtain a primary desulfurization liquid. Then, 12.36 g of 10% sodium hypochlorite was added to the primary desulfurization liquid to deeply remove the remaining sulfide, and the solution was filtered to obtain a secondary desulfurization liquid with a sulfide content of 3.25 mg / L.
[0081] (2) COD removal: The secondary desulfurization liquid was subjected to ozone catalytic oxidation, with an ozone flow rate of 0.5 L / min and a catalytic oxidation time of 1 h. After oxidation, the COD was reduced to 35.64 mg / L;
[0082] (3) Lithium recovery: The solution obtained in step (2) was subjected to selective adsorption and lithium extraction by continuous ion exchange equipment, and the remaining solution was the lithium extraction adsorption tail liquid; the adsorbent loading amount was 3825 mL, the adsorption rate was 4 BV / h, pure water was used for desorption, and the desorption rate was 2 BV / h, and 3.946 kg of selectively adsorbed lithium-rich desorption liquid was obtained. The components of the lithium-rich desorption liquid are shown in the following table;
[0083] Table 2 Main components of lithium-rich desorption solution
[0084] Element <![CDATA[Ca 2+ ]]> <![CDATA[K + ]]> <![CDATA[Mg 2+ ]]> <![CDATA[Na + ]]> <![CDATA[Ba 2+ ]]> <![CDATA[Li + ]]> <![CDATA[Sr 2+ ]]> <![CDATA[B2O3]]> content(%) 0.0162 0.0014 0.0033 0.105 0.0239 0.044 0.0027 0.0225
[0085] The lithium-rich desorption liquid is respectively passed through ion exchange resin to remove calcium, magnesium, barium and boron in the solution, wherein the feed rate of the resin column for removing calcium, magnesium and barium is 2BV / h, the calcium ion concentration in the effluent is 3.56mg / L, the magnesium ion concentration is 2.39mg / L, and the barium ion concentration is 3.64mg / L. The feed rate of the boron removal resin is 1.5BV / h, and the boron concentration in the boron removal effluent is 2.87mg / L. After boron removal, reverse osmosis concentration is performed, and the first-level reverse osmosis pressure is 2.5MPa to obtain 0.809kg of first-level reverse osmosis concentrated water, and then secondary reverse osmosis is performed, and the secondary reverse osmosis pressure is 3.6MPa to obtain 0.382kg of secondary reverse osmosis concentrated liquid, with a lithium ion concentration of 4.23g / L. The secondary reverse osmosis concentrated liquid is evaporated and concentrated to obtain 0.083kg of concentrated liquid, with a lithium ion concentration of 20.39g / L, and then 73.11g 20% sodium carbonate solution, lithium precipitation reaction, reaction temperature 90 ° C, reaction time 1h, 7.36g of crude lithium carbonate was obtained, and then washed twice and dried to obtain 6.54g of industrial grade lithium carbonate product;
[0086] (4) Barium recovery and hardness removal: 15 kg of lithium adsorption tail liquid was taken, and the main component data are shown in the following table;
[0087] Table 3 Main components of gas field water extraction lithium tail liquid
[0088] Element <![CDATA[K + ]]> <![CDATA[Na + ]]> <![CDATA[Ca 2+ ]]> <![CDATA[Mg 2+ ]]> <![CDATA[Li + ]]> <![CDATA[Ba 2+ ]]> <![CDATA[Br - ]]> content(%) 2.0474 3.407 0.2141 0.0217 0.0031 0.1864 0.0349
[0089] 34.8 g of sodium sulfate was added to the lithium extraction adsorption tail liquid, and the mixture was stirred for reaction for 20 min and filtered to obtain filter residue 1 and filtrate 1. The filter residue 1 was washed twice with deionized water and dried to obtain 46.58 g of industrial precipitated barium sulfate (mass fraction 97.8%); sodium hydroxide was added to the filtrate 1 to adjust the pH value to 12, and the mixture was stirred for reaction for 20 min and filtered to obtain filter residue 2 and filtrate 2; then 102.1 g of sodium carbonate was added to the filtrate 2, and the mixture was stirred for reaction for 20 min and filtered to obtain filter residue 3 and filtrate 3;
[0090] (5) Potassium and sodium recovery: The filtrate 3 is evaporated and salt is precipitated, and the evaporation end point is determined based on the ion concentration and the K, Na / Cl-ternary phase diagram; after evaporating 12.3 kg of water, it is filtered to obtain 1.4 kg of mother liquor 1 and 1.3 kg of wet sodium chloride, and the wet sodium chloride is dried to obtain 1.1 kg of industrial salt; the mother liquor 1 is cooled and crystallized again, and the mother liquor temperature is stopped when it drops to 40° C., and filtered to obtain 180.3 g of wet potassium chloride and 1219.7 g of mother liquor 2, and the wet potassium chloride is dried to obtain 140.2 g of agricultural first-grade potassium chloride;
[0091] (6) Bromine resource recovery: adding acid to the mother liquor 2 (Br - The pH value of the mother liquor 2 (with a concentration of 0.3865%) was adjusted to 3.5, 2.5gCl2 was introduced into the mother liquor 2 for oxidation, hot air at 80-90°C was introduced at a gas-liquid ratio of 120:1 (L / L), and the blown bromine vapor was absorbed by an aqueous SO2 solution to form hydrogen bromide and sulfuric acid, with a bromine concentration of 59.95g / L in the absorption liquid; then 2.1gCl2 was introduced into the absorption liquid for oxidation, hot air at 80-90°C was introduced at a gas-liquid ratio of 120:1 (L / L), and blown bromine vapor and bromine extraction tail liquid were obtained, and 4.07g of a 94.05% crude bromine product was obtained after condensation of the bromine vapor.
[0092] The crude bromine was heated and vaporized, and the reflux condensation temperature was controlled between 30 and 35°C to obtain 3.65 g of 98.80% industrial secondary bromine.
[0093] The bromine extraction tail liquid is mixed with the acidified mother liquor and then oxidized and blown out.
[0094] Example 2
[0095] The main component data of the gas field water in this embodiment are shown in the following table.
[0096] Table 4 Main components of gas field water extraction lithium tail liquid
[0097] index <![CDATA[Li + ]]> <![CDATA[Na + ]]> <![CDATA[K + ]]> <![CDATA[Ca 2+ ]]> <![CDATA[Mg 2+ ]]> <![CDATA[Ba 2+ ]]> content(%) 0.0146 2.368 0.2569 0.1265 0.0334 0.1357 index <![CDATA[Sr 2+ ]]> <![CDATA[B2O3]]> <![CDATA[Cl - ]]> <![CDATA[Br - ]]> Sulfide COD content(%) 0.0187 0.0456 4.983 0.02291 0.0299 175
[0098] The catalyst used for ozone catalytic oxidation in this embodiment is the product in CN102872884B; the adsorbent used for lithium adsorption extraction is the product in CN111905700B.
[0099] The method for recovering gas field water-associated resources in this embodiment comprises the following steps:
[0100] (1) Desulfurization treatment: 15 kg of lithium tail liquid extracted from gas field water was taken and subjected to primary desulfurization by air stripping method. Air was introduced into the gas field water at a liquid-to-gas ratio of 1:100 (L / L) to blow out the sulfide in the water in the form of hydrogen sulfide. The blown hydrogen sulfide was absorbed by sodium hydroxide solution, and the sulfide in the water was reduced to 26.35 mg / L to obtain a primary desulfurization liquid. Then, 9.35 g of 10% sodium hypochlorite was added to the primary desulfurization liquid to deeply remove the remaining sulfide, and the liquid was filtered to obtain a secondary desulfurization liquid with a sulfide content of 2.34 mg / L.
[0101] (2) COD removal: The secondary desulfurization liquid was subjected to ozone catalytic oxidation, with an ozone flow rate of 0.5 L / min and a catalytic oxidation time of 1 h. After oxidation, the COD was reduced to 38.45 mg / L;
[0102] (3) Lithium recovery: The solution obtained in step (2) is subjected to selective adsorption and lithium extraction by continuous ion exchange equipment, and the remaining solution is the lithium extraction adsorption tail liquid; the adsorbent loading amount is 3825 ml, the adsorption rate is 4 BV / h, and pure water is used for desorption at a desorption rate of 2 BV / h to obtain 4.006 kg of selectively adsorbed lithium-rich desorption liquid, and the components of the lithium-rich desorption liquid are shown in the following table;
[0103] Table 5 Main components of lithium-rich desorption solution
[0104] Element <![CDATA[Ca 2+ ]]> <![CDATA[K + ]]> <![CDATA[Mg 2+ ]]> <![CDATA[Na + ]]> <![CDATA[Ba 2+ ]]> <![CDATA[Li + ]]> <![CDATA[Sr 2+ ]]> <![CDATA[B2O3]]> content(%) 0.0136 0.0026 0.0029 0.169 0.0251 0.045 0.0034 0.0236
[0105] The lithium-rich desorption liquid is respectively passed through ion exchange resin to remove calcium, magnesium, barium and boron in the solution, wherein the feed rate of the resin column for removing calcium, magnesium and barium is 2BV / h, the calcium ion concentration in the effluent is 2.87mg / L, the magnesium ion concentration is 2.13mg / L, and the barium ion concentration is 3.23mg / L. The feed rate of the boron removal resin is 1.5BV / h, and the boron concentration in the boron removal effluent is 2.36mg / L. After boron removal, reverse osmosis concentration is performed, the first-level reverse osmosis pressure is 2.5Mpa, and 0.821kg of first-level reverse osmosis concentrated water is obtained. Secondary reverse osmosis is then performed, and the secondary reverse osmosis pressure is 3.6Mpa to obtain 0.388kg of secondary reverse osmosis concentrated liquid with a lithium ion concentration of 4.34g / L. The secondary reverse osmosis concentrated liquid is evaporated and concentrated to obtain 0.122kg of concentrated liquid with a lithium ion concentration of 20.12g / L, and then 74.23g 20% sodium carbonate solution, lithium precipitation reaction, reaction temperature 90 ° C, reaction time 1h, 7.42g of crude lithium carbonate was obtained, and then washed twice and dried to obtain 6.79g of industrial grade lithium carbonate product;
[0106] (4) Barium recovery and hardness removal
[0107] 15kg of tail liquid from gas field water for lithium extraction and 15kg of tail liquid from lithium adsorption were taken, and the main component data are shown in the following table;
[0108] Table 6 Main components of gas field water extraction lithium tail liquid
[0109] Element <![CDATA[K + ]]> <![CDATA[Na + ]]> <![CDATA[Ca 2+ ]]> <![CDATA[Mg 2+ ]]> <![CDATA[Li + ]]> <![CDATA[Ba 2+ ]]> <![CDATA[Br - ]]> content(%) 1.6447 2.490 0.1607 0.0347 0.0036 0.1109 0.0230
[0110] Add 20.7 g of sodium sulfate to the lithium adsorption tail liquid, stir and react for 20 minutes, and then filter to obtain filter residue 1 and filtrate 1. Wash the filter residue 1 twice with deionized water and dry to obtain 28.3 g of industrial precipitated barium sulfate (mass fraction 97.5%). Add sodium hydroxide to the filtrate 1 to adjust the pH value to 12, stir and react for 20 minutes, and then filter to obtain filter residue 2 and filtrate 2. Then add 76.65 g of sodium carbonate to the filtrate 2, stir and react for 20 minutes, and then filter to obtain filter residue 3 and filtrate 3.
[0111] (5) Potassium and sodium recovery: The filtrate 3 is evaporated and salt is precipitated, and the evaporation end point is determined based on the ion concentration and the K, Na / Cl-ternary phase diagram; after evaporating 12.7 kg of water, it is filtered to obtain 1.10 kg of mother liquor 1 and 1.2 kg of wet sodium chloride, and the wet sodium chloride is dried to obtain 0.95 kg of industrial salt; the mother liquor 1 is cooled and crystallized again, and the mother liquor temperature is stopped when it drops to 40° C., and filtered to obtain 164.8 g of wet potassium chloride and 935.2 g of mother liquor 2, and the wet potassium chloride is dried to obtain 119.5 g of agricultural first-grade potassium chloride;
[0112] (6) Bromine resource recovery: The mother liquor 2 (Br) obtained in step (5) is adjusted with sulfuric acid. - The pH value of the mother liquor 2 was raised to 3 with a concentration of 0.3205%), 2.1 g of Cl2 was introduced into the mother liquor 2 for oxidation, hot air at 80 to 90°C was introduced at a gas-liquid ratio of 120:1 (L / L), the blown bromine vapor was absorbed by an aqueous SO2 solution to form hydrogen bromide and sulfuric acid, the bromine concentration in the absorption liquid was 58.63 g / L, 1.8 g of Cl2 was introduced into the absorption liquid for oxidation, hot air at 80 to 90°C was introduced at a gas-liquid ratio of 120:1 (L / L), and blown bromine vapor and bromine extraction tail liquid were obtained. After the bromine vapor was condensed, 3.49 g of a 93.36% crude bromine product was obtained.
[0113] The crude bromine was heated and vaporized, and the reflux condensation temperature was controlled between 30 and 35°C to obtain 3.02 g of 98.83% industrial secondary bromine.
[0114] Example 3
[0115] The main component data of the gas field water in this embodiment are shown in the following table.
[0116] Table 7 Main components of gas field water extraction lithium tail liquid
[0117] index <![CDATA[Li + ]]> <![CDATA[Na + ]]> <![CDATA[K + ]]> <![CDATA[Ca 2+ ]]> <![CDATA[Mg 2+ ]]> <![CDATA[Ba 2+ <!-- 6 -->]]> content(%) 0.0132 2.45 0.2569 0.1265 0.0334 0.1357 index <![CDATA[Sr 2+ ]]> <![CDATA[B2O3]]> <![CDATA[Cl - ]]> <![CDATA[Br - ]]> Sulfide COD content(%) 0.0187 0.0456 4.983 0.0229 0.0299 205
[0118] The method for recovering gas field water-associated resources in this embodiment comprises the following steps:
[0119] (1) Desulfurization treatment: 15 kg of lithium tail liquid extracted from gas field water was taken and subjected to primary desulfurization by air stripping method. Air was introduced into the gas field water at a liquid-to-gas ratio of 1:100 (L / L) to blow out the sulfide in the water in the form of hydrogen sulfide. The blown hydrogen sulfide was absorbed by sodium hydroxide solution, and the sulfide in the water was reduced to 28.93 mg / L to obtain a primary desulfurization liquid. Then, 10.23 g of 10% sodium hypochlorite was added to the primary desulfurization liquid to deeply remove the remaining sulfide, and the secondary desulfurization liquid was obtained by filtering. The sulfide content was 3.28 mg / L.
[0120] (2) COD removal: The secondary desulfurization liquid was subjected to ozone catalytic oxidation, with an ozone flow rate of 1 L / min and a catalytic oxidation time of 1 h. After oxidation, the COD was reduced to 25.31 mg / L;
[0121] (3) Lithium recovery: The solution obtained in step (2) is subjected to selective adsorption and lithium extraction by continuous ion exchange equipment, and the remaining solution is the lithium extraction adsorption tail liquid; the adsorbent loading amount is 3825 ml, the adsorption rate is 4 BV / h, pure water is used for desorption, and the desorption rate is 2 BV / h, and 3.622 kg of selectively adsorbed lithium-rich desorption liquid is obtained. The components of the lithium-rich desorption liquid are shown in the following table;
[0122] Table 8 Main components of lithium-rich desorption solution
[0123] Element <![CDATA[Ca 2+ ]]> <![CDATA[K + ]]> <![CDATA[Mg 2+ ]]> <![CDATA[Na + ]]> <![CDATA[Ba 2+ ]]> <![CDATA[Li + ]]> <![CDATA[Sr 2+ ]]> <![CDATA[B2O3]]> content(%) 0.0118 0.0023 0.0031 0.175 0.0151 0.043 0.0038 0.0253
[0124] The lithium-rich desorption liquid is respectively passed through ion exchange resin to remove calcium, magnesium, barium and boron in the solution, wherein the feed rate of the resin column for removing calcium, magnesium and barium is 2BV / h, the calcium ion concentration in the effluent is 3.17mg / L, the magnesium ion concentration is 2.54mg / L, and the barium ion concentration is 2.21mg / L. The feed rate of the boron removal resin is 1.5BV / h, and the boron concentration in the boron removal effluent is 3.25mg / L. After boron removal, reverse osmosis concentration is performed, the first-level reverse osmosis pressure is 2.5Mpa, and 0.742kg of first-level reverse osmosis concentrated water is obtained. Secondary reverse osmosis is then performed, and the secondary reverse osmosis pressure is 3.6Mpa to obtain 0.350kg of secondary reverse osmosis concentrated liquid with a lithium ion concentration of 4.56g / L. The secondary reverse osmosis concentrated liquid is evaporated and concentrated to obtain 0.073kg of concentrated liquid with a lithium ion concentration of 20.31g / L, and then 67.12g 20% sodium carbonate solution, lithium precipitation reaction, reaction temperature 90 ° C, reaction time 1h, 6.71g of crude lithium carbonate was obtained, and then washed twice and dried to obtain 6.08g of industrial grade lithium carbonate product;
[0125] (4) Barium recovery and hardness removal: 15 kg of lithium adsorption tail liquid was taken, and the main component data are shown in the following table;
[0126] Table 9 Main components of gas field water extraction lithium tail liquid
[0127] Element <![CDATA[K + ]]> <![CDATA[Na + ]]> <![CDATA[Ca 2+ ]]> <![CDATA[Mg 2+ ]]> <![CDATA[Li + ]]> <![CDATA[Ba 2+ ]]> <![CDATA[Br - ]]> content(%) 1.816 2.575 0.1555 0.03 0.0023 0.1052 0.036
[0128] 19.6 sodium sulfate was added to the lithium extraction adsorption tail liquid, and the mixture was stirred for reaction for 20 minutes and then filtered to obtain filter residue 1 and filtrate 1. The filter residue 1 was washed twice with deionized water and dried to obtain 26.57 barium sulfate (mass fraction 97.9%). Sodium hydroxide was added to the filtrate 1 to adjust the pH value to 12, and the mixture was stirred for reaction for 20 minutes and then filtered to obtain filter residue 2 and filtrate 2. Then 74.2 sodium carbonate was added to the filtrate 2 and the mixture was reacted for 20 minutes and then filtered to obtain filter residue 3 and filtrate 3.
[0129] (5) Potassium and sodium recovery: The filtrate 3 is evaporated and salt is precipitated. The evaporation end point is determined based on the ion concentration and the K, Na / Cl-ternary phase diagram. After evaporating 12.6 kg, the filtrate is filtered to obtain 0.94 kg of mother liquor 1 and 1.46 kg of wet sodium chloride. The wet sodium chloride is dried to obtain 0.75 kg of industrial salt. The mother liquor 1 is cooled and crystallized again. The crystallization is stopped when the liquid concentration drops to 40° C. and filtered to obtain 134.5 g of wet potassium chloride and 805.5 g of mother liquor 2. The wet potassium chloride is dried to obtain 94.2 g of agricultural first-grade potassium chloride.
[0130] (6) Bromine resource recovery: The mother liquor 2 (Br - The pH value of the mother liquor 2 (with a concentration of 0.3795%) was adjusted to 3.5, and then 2.4gCl2 was introduced into the mother liquor 2 for oxidation, and hot air at 80-90°C was introduced at a gas-liquid ratio of 120:1 (L / L). The blown bromine vapor was absorbed by an aqueous SO2 solution to form hydrogen bromide and sulfuric acid. The bromine concentration in the absorption liquid was 59.95g / L, and then 2gCl2 was introduced into the absorption liquid for oxidation, and hot air at 80-90°C was introduced at a gas-liquid ratio of 120:1 (L / L) to obtain blown bromine vapor and bromine extraction tail liquid. After the bromine vapor was condensed, 3.96g of a 94.05% crude bromine product was obtained.
[0131] The crude bromine was heated and vaporized, and the reflux condensation temperature was controlled between 30 and 35°C to obtain 3.48 g of 98.80% industrial secondary bromine.
[0132] The bromine extraction tail liquid is mixed with the acidified mother liquor and then oxidized and blown out.
Claims
1. A method for recovering gas field water-associated resources, characterized in that: The following steps are involved: (1) Desulfurization treatment: Use stripping and oxidation methods to reduce the sulfide in gas field water to below 5 mg / L; (2) COD removal: COD in gas field water is removed to below 50 mg / L through ozone catalytic oxidation; (3) Lithium recovery: lithium is extracted by adsorption method, and the remaining solution is the lithium extraction adsorption tail liquid; (4) Barium recovery and hardness removal: Sulfate is added to the tail liquid of lithium extraction adsorption for reaction. After the reaction is completed, solid-liquid separation is performed to obtain filter residue 1 and filtrate 1; filter residue 1 is barium sulfate precipitate; alkali is added to filtrate 1 to a pH value of 10-12. After the reaction is completed, solid-liquid separation is performed to obtain filter residue 2 and filtrate 2; carbonate is added to filtrate 2. After the reaction is completed, solid-liquid separation is performed to obtain filter residue 3 and filtrate 3; (5) Potassium and sodium recovery: the filtrate 3 is evaporated and concentrated to precipitate sodium chloride, and solid-liquid separation is performed to obtain sodium chloride precipitate and mother liquor 1. The concentration endpoint is determined based on the ion concentration and the K, Na / Cl- ternary phase diagram; the mother liquor 1 is cooled and crystallized, and solid-liquid separation is performed to obtain potassium chloride precipitate and mother liquor 2; (6) Bromine resource recovery: Acidification is added to the mother liquor 2 to a pH value of 2-5, chlorine gas is introduced for oxidation, hot air is blown out and the mixture is absorbed by an aqueous sulfur dioxide solution to obtain an absorption liquid; chlorine gas is introduced into the absorption liquid for oxidation, hot air is blown out and crude bromine and bromine extraction tail liquid are obtained.
2. The method for recovering gas field water associated resources according to claim 1, characterized in that: In step (1), air is introduced into the gas field water to blow out the sulfide in the water in the form of hydrogen sulfide to obtain a primary desulfurization liquid; an oxidant is added to the primary desulfurization liquid to oxidize the sulfide into a single substance, and the solid and liquid are separated to obtain a secondary desulfurization liquid, thereby completing the desulfurization.
3. The method for recovering gas field water associated resources according to claim 2, characterized in that: In step (1), the ratio of the gas field water to the air is 1 L: 25-150 L; the oxidant is sodium hypochlorite or sodium hypochlorite solution; and the added amount is an effective chlorine content of 25-100 mg / L.
4. The method for recovering gas field water associated resources according to any one of claims 1 to 3, characterized in that: In step (2), the ozone introduction rate is 0.5-1 L / min; and the ozone catalytic oxidation treatment time is 0.5-2 h.
5. The method for recovering gas field water associated resources according to any one of claims 1 to 4, characterized in that: In step (3), an adsorbent for lithium extraction is used to extract lithium, and a lithium-rich desorption solution is obtained after desorption with water. Calcium, magnesium, barium and boron in the lithium-rich desorption solution are removed by an ion exchange resin, and the solution is concentrated, and a sodium carbonate solution is added to react with lithium precipitation to obtain a lithium carbonate precipitate.
6. The method for recovering gas field water associated resources according to claim 5, characterized in that: In step (3), the adsorption rate is 2-6 BV / h; the desorption rate is 1-3 BV / h; the concentration is carried out by reverse osmosis concentration and / or evaporation concentration; the Li in the concentrated solution after concentration is ≥ 20 g / L; the temperature of the lithium precipitation reaction is 80-90° C., and the reaction time is 0.5-2 h; the concentration of the sodium carbonate solution is 15-25% by mass.
7. The method for recovering gas field water-associated resources according to any one of claims 1 to 6, characterized in that: In step (4), the amount of sulfate added is 1.05-1.3 times the molar amount of barium in the solution; the amount of alkali added is 1.05-1.3 times the molar amount of magnesium in the solution; and the amount of carbonate added is 1.05-1.3 times the molar amount of calcium in the solution.
8. The method for recovering gas field water-associated resources according to any one of claims 1 to 7, characterized in that: In step (4), the sulfate is potassium sulfate and / or sodium sulfate; the alkali is potassium hydroxide and / or sodium hydroxide; and the carbonate is potassium carbonate and / or sodium carbonate.
9. The method for recovering gas field water associated resources according to any one of claims 1 to 8, characterized in that: In step (6), the calculation formula for the chlorine gas input amount for chlorine oxidation is as follows: Chlorine consumption (g) = bromine content (g) × 0.444 × chlorine ratio (%) The chlorine ratio ranges from 110% to 130%.
10. The method for recovering gas field water associated resources according to any one of claims 1 to 9, characterized in that: In step (6), the temperature of the hot air is 60-90°C; the gas-liquid ratio of the hot air blown out is 100-160L:1L.
Citation Information
Patent Citations
Rejection processing technology for gas production wastewater in sulfur acid containing gas field
CN103880202A
Sulfur-containing gas field produced water treatment process
CN105174581A
Desulfuration and purification pre-treatment process for gas production wastewater
CN107265752A
Resin-based inorganic nanoparticle composite lithium extraction particle
CN111905700A
Production process for desalinating bromine in concentrated seawater
CN114933283A
Cited By
Method for recycling valuable resources of underground brine
CN120463379A
A method for recovering valuable resources from underground brine
CN120463379B
Method for preparing lithium carbonate by extracting lithium from gas field produced water