A resin bonded solidified filter element and its preparation method and application

By controlling the expansion uniformity of the binder and gas flow solidification technology in the filter element, the problem of filter element performance damage caused by uneven solidification of the binder is solved, and efficient organic coating filtration performance is achieved.

CN114515457BActive Publication Date: 2024-10-18HANGZHOU COBETTER FILTRATION EQUIPMENT CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202111682557.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-31
Publication Date
2024-10-18
Estimated Expiration
2041-12-31

AI Technical Summary

Technical Problem

In the existing filter element, due to uneven solidification of the binder during the filtration process of organic coatings, the performance of the filter element is damaged and the interception rate is reduced. It cannot effectively prevent the dissolution of small molecules of the binder and affect the filtration effect.

Method used

By dividing the filter element into four areas along the radial cross-section, the standard deviation and average ratio of the expansion degree of the adhesive are controlled within the range of 0.01-0.5. The gas flow curing method is used to ensure uniform solidification of the adhesive and form a uniform skin. Core structure to improve the strength and solvent resistance of the filter element.

Benefits of technology

It achieves a uniform solidification degree of the filter element's binder, improves the interception rate and stability of the filter element, reduces the dissolution of small molecules of the binder, and enhances the filtration performance of organic coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003452472960000461
    Figure BDA0003452472960000461
Patent Text Reader

Abstract

The invention discloses a resin bonded solidified filter element and a preparation method and application thereof, and relates to the technical field of filter elements. The filter element comprises resin fibers, which are provided with a permeable liquid inlet surface and a liquid outlet surface, and an axial hollow flow channel is formed at the same time. The resin fibers are coated with a binder to form a skin-core structure, and the binder is cured and bonded. The filter element is immersed in an organic solvent, and the volume of the organic solvent swollen and absorbed by the binder in the filter element per unit weight is used to represent the expansion degree. In the radial cross section of the filter element, the first region is at 0-25% of the filter element thickness from the liquid inlet side, the second region is at 25-50%, the third region is at 50-75%, and the fourth region is at 75-100%. The ratio between the standard deviation of the expansion degree of each region and the average expansion degree is 0.01-0.5. The invention has a small difference in expansion degree between each region, can effectively prevent small molecules of the binder from mixing into the filtrate during the coating filtration process, has good bonding between fibers, and is stable in filtration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of filter elements, in particular to a resin-bonded and cured filter element and a preparation method and application thereof. Background Art

[0002] The filter element is the heart of the filter and the main principle of the filter operation. It is a purification device for purifying resources and increasing resource reuse. The filter element is generally used in oil, water, air filtration, etc. to remove impurities in the medium and protect the normal operation of the equipment or the cleanliness of the air.

[0003] Paint is applied to the surface of a specific object and can form a film that plays a protective or decorative role. Therefore, if the paint contains too many particulate impurities, it will seriously affect the uniformity of the paint, thereby affecting the subsequent coating effect. Therefore, filtering the paint before using it is also an essential step. However, since the paint contains a high solid content, especially for organic paints, it often has a high consistency or viscosity, and the filtering pressure is high, which ordinary filter elements often cannot withstand.

[0004] However, filter elements that are impregnated with adhesives and then cured and bonded are widely used in the filtration of organic coatings due to their excellent strength and rigidity. When preparing the filter element, the adhesive must first be impregnated on the fiber and then the adhesive must be cured at high temperature. In the prior art, in the preparation process of the filter element, the adhesive is usually cured and dried in an oven. Due to uneven temperature transfer and heating, the degree of curing of the adhesive in different areas of the filter element is uneven. Among them, the part with too low a degree of curing will cause too much neutralization and dissolution in the filter element, and the purity of the filtrate cannot be guaranteed during the filtration process. If the degree of curing is too high, the performance of the filter element will be impaired. Similarly, due to the uneven curing of the adhesive, the bonding force of the resin fibers in each area of ​​the filter element is damaged, and the filter element cannot withstand the filtration pressure during the filtration of organic coatings. Summary of the invention

[0005] The object of the present invention is to provide a filter element with uniform curing degree of binder in different regions, so as to prevent binder dissolution or damage to the overall performance of the filter element in organic coating filtration applications due to uneven curing during use.

[0006] In order to achieve the above object, the present invention adopts the following technical solution:

[0007] A resin bonded solidified filter element, the filter element comprising resin fibers, having a permeable liquid inlet surface and a liquid outlet surface remote from the liquid inlet surface and also permeable, and forming an axial hollow flow channel;

[0008] The resin fiber is coated with a binder to form a skin-core structure, and the binder is cured and bonded;

[0009] The filter element is immersed in an organic solvent, and the volume of the organic solvent absorbed by the binder in the filter element per unit weight is used to represent the expansion degree. In the radial section of the filter element:

[0010] The first area is 0-25% of the filter element thickness from the liquid inlet side.

[0011] The second area is 25-50% of the filter element thickness from the liquid inlet side.

[0012] The third area is 50-75% of the filter element thickness from the liquid inlet side.

[0013] The fourth area is 75-100% of the filter element thickness from the liquid inlet side.

[0014] The ratio between the standard deviation of the expansion degree and the average expansion degree of each region is 0.01-0.5.

[0015] In the resin bonded and cured filter element of the present invention, the resin fibers are coated with an adhesive to form a skin-core structure. After the adhesive is cured and bonded, it can not only increase the bonding firmness between the resin fibers, thereby increasing the strength and rigidity of the entire filter element, but also the skin layer formed by the adhesive can prevent the organic solvents in the coating from dissolving and corroding the resin fibers during the long-term filtration of organic coatings by the filter element, thereby increasing the overall solvent resistance of the filter element.

[0016] In addition, the invention team discovered in experiments that in the prior art, the filter element using binder to coat resin fibers has different degrees of binder curing in different areas in the cross-sectional direction. During the filtration process of the organic coating, due to the low degree of cross-linking in the incompletely cured part, the uncured small molecules in the binder cortex are easily dissolved, resulting in residual binder small molecules in the filtrate, affecting the overall filtration effect. At the same time, the incompletely cured part has a low degree of cross-linking and many small molecules, which are easily dissolved by the organic coating, resulting in a decrease in the bonding strength between the resin fibers in the filter element. During the filtration process, due to the presence of a certain pressure in the fluid, if the resin fiber bonding is not firm, the pressure will easily squeeze and deform the fibers, thereby affecting the interception rate (i.e., accuracy) of the filter element, and thus affecting the final filtration effect.

[0017] In the present invention, the filter element is divided into four regions along the radial cross-section direction, wherein the first, second, third and fourth regions are located at 0-25%, 25-50%, 50-75% and 75-100% of the filter element thickness from the liquid inlet side, respectively, and the ratio between the standard deviation of the expansion degree and the average expansion degree in each region is 0.01-0.5, wherein the expansion degree is the volume of organic solvent absorbed by the binder per unit weight in the filter element when the filter element is immersed in an organic solvent, and the higher the expansion degree, the lower the curing degree of the binder, and the easier it is to absorb the organic solvent and swell, while the solid A low degree of curing also means that the content of uncured small molecules in the binder is high; the smaller the ratio between the standard deviation of the expansion and the average expansion, the smaller the difference in expansion between each area and the more uniform it is. Therefore, when the ratio is 0.01-0.5, the difference in expansion between each area of ​​the filter element is small, the binder is completely cured, and there are few small molecules of binder, which prevents small molecules of binder from mixing into the filtrate during the filtration process and affecting the quality of the coating. At the same time, complete curing can also give good adhesion between fibers, prevent the interception rate of the filter element from being affected when the filtration is under pressure, and ensure filtration stability.

[0018] Furthermore, the ratio between the standard deviation of the expansion degree in each region and the average expansion degree is 0.05-0.3.

[0019] Furthermore, after the filter element is fully impregnated with the organic solvent, the interception rate of particles with a particle size of 10 μm is reduced by 0.1-1%.

[0020] The curing degree of the binder in the filter element of the present invention is uniform and relatively complete. After being fully impregnated with an organic solvent, few small molecules are dissolved, while still ensuring good bonding strength. Therefore, the internal fiber interweaving structure is not easily deformed under pressure, and the overall interception rate of the filter element is reduced.

[0021] Furthermore, the filter element has an interception rate of 99% for particles with a particle size of 10 μm.

[0022] The filter element of the present invention has a good interception rate.

[0023] Furthermore, the binder accounts for 20-70% of the overall mass of the filter element.

[0024] The binder is coated on the outside of the resin fiber as a cortical structure. On the one hand, it can ensure the bonding strength between the resin fibers, and on the other hand, it can improve the resin fiber's tolerance to solvents in the coating. If the binder content is too low, it cannot be well coated on the outside of the resin fiber to form a cortical structure. If the content is too high, the resin fiber content as the core layer is too low. Although the bonding strength between the resin fibers can be guaranteed, the overall strength will be low due to the small amount of core layer.

[0025] Furthermore, the standard deviation of the expansion degree of each area in the radial cross section of the filter element is 0.1-1.5 mL / kg; the average expansion degree of the filter element is 1-10 mL / kg.

[0026] When the average expansion degree of the filter element of the present invention is within the range of 1-10mL / kg, the binder is cured more completely. If the average expansion degree is too large and the curing is incomplete, more uncured small molecules will be dissolved and mixed into the filtrate during the filtration process. At the same time, the bonding strength between the resin fibers decreases, which can easily affect the overall interception rate of the filter element under the pressure of the filtering fluid, thereby affecting the filtration quality. At the same time, when the standard deviation of the expansion degree in each region is within the range of 0.1-1.5mL / kg, it has better curing uniformity and the overall filtration performance of the filter element is more stable.

[0027] Furthermore, the diameter of the resin fiber is 1-100 μm.

[0028] Different fiber diameters can be selected according to different flow rate requirements of the filter element.

[0029] Furthermore, the filter element is obtained by winding at least one non-woven fabric, and the non-woven fabric contains resin fibers.

[0030] Furthermore, the thickness of the non-woven fabric is h1, the radial distance between the liquid inlet surface and the liquid outlet surface is h2, and h1:h2 is 1:10-25; and / or, h2=(1.1-1.5)*n*h1, wherein n is the number of winding layers of the non-woven fabric.

[0031] The filter element of the present invention can be wound with a non-woven fabric during preparation, wherein the ratio between the thickness h1 of the non-woven fabric and the radial distance h2 between the liquid inlet surface and the liquid outlet surface of the filter element is 1:10-25. If the ratio is too small and the thickness of the non-woven fabric is too thin, the number of winding layers is too large, and the resin fibers between the contact surfaces of the layers can only be bonded by a binder. Compared with the resin fibers in the layers that are relatively perpendicular to the thickness direction, the contact surfaces between the layers are weak areas for the bonding of the resin fibers of the filter element. Therefore, if the number of layers is too large, the contact surfaces between the layers increase. If the non-woven fabric layers are not firmly bonded during filtration, the interception rate may vary greatly. If the ratio is too large, the non-woven fabric is too thick, and the number of winding layers is too small, especially for filter elements using multiple non-woven fabrics, the interception rate and flow rate of the prepared filter element may be uneven. When the number of non-woven fabric winding layers is n, in order to achieve better adhesion between layers, the present invention sets h2 = (1.1-1.5) * n * h1, that is, a certain thickness of adhesive layer is set between layers.

[0032] Furthermore, the resin fiber includes a mixture of one or more of polyester fiber, nylon fiber, polypropylene fiber, cellulose fiber, and acrylonitrile fiber.

[0033] Furthermore, the binder includes phenolic resin.

[0034] Furthermore, the organic solvent includes one or more of ethanol, acetone, butanone, ethyl acetate, and xylene.

[0035] A method for preparing a resin-bonded and cured filter element comprises the following steps:

[0036] S1: Material selection: select resin fiber non-woven fabric;

[0037] S2: Winding: Winding the non-woven fabric to obtain a wound filter element;

[0038] S3: Impregnation: prepare a binder solution, and immerse the wound filter element in the binder solution to obtain a primary filter element;

[0039] S4: Debonding: removing excess binder solution;

[0040] S5: Curing: Use gas to circulate and cure the debonded filter element to prepare a resin-bonded and cured filter element.

[0041] When preparing the resin-bonded and cured filter element of the present invention, it is first necessary to select a non-woven fabric with a suitable fiber diameter according to actual needs, and then wind it to obtain a wound filter element. Then, a binder solution is prepared, and the wound filter element is immersed in the binder solution so that the binder fills the filter element and fully covers the surface of the resin fiber. Subsequently, the filter element is degummed to remove excess binder solution in the pores of the filter element. Finally, the degummed filter element is cured by the binder by gas circulation. The advantage of using the gas circulation method is that the adhesive between each area of ​​the filter element cross section can be uniformly cured. This is because the binder is only coated on the surface of the resin fiber after the degummed filter element, and the gas used for curing can quickly pass through the entire filter element through the pores of the filter element, thereby ensuring that each area of ​​the filter element cross section is evenly heated and the degree of curing is uniform.

[0042] Furthermore, in step S2, a binder solution is sprayed on the surface of the non-woven fabric during winding, and the spraying amount is 20-70% of the gram weight.

[0043] In the present invention, the adhesive solution can be sprayed on the surface of the non-woven fabric when it is wound, so that the prepared wound filter element has good initial bonding strength and prevents the loosening of the non-woven fabric layers in the wound filter element.

[0044] Furthermore, the winding tension in step S2 is 3-20N.

[0045] Under this winding tension, the prepared wound filter element has good overall performance; if the winding tension is too small, the prepared wound filter element is too loose, and if the winding tension is too large, the non-woven fabric is not only easily torn during preparation, but the filtration interception rate or the overall flow rate of the filter element is difficult to control.

[0046] Furthermore, in step S3, the concentration of the binder solution is 50-500wt%.

[0047] The binder solution at this concentration is easier to cover the resin fiber during impregnation, is not easy to fall off, and is easy to solidify.

[0048] Furthermore, the immersion in step S3 is performed at 15-30° C. for 5-60 min.

[0049] When immersed within this temperature and time range, the binder solution can fill the filter element and well cover the outside of the resin fiber.

[0050] Furthermore, the degumming in step S4 is a multi-stage flushing with compressed gas, and the compressed gas passes through the filter element.

[0051] And the wind pressure decreases:

[0052] S41: The wind pressure of compressed gas is 50-100kpa, and the flushing time is 2-5s;

[0053] S42: The wind pressure of compressed gas is 10-50kpa, and the flushing time is 5-20s;

[0054] S43: The wind pressure of compressed gas is 2-15kpa, and the flushing time is 15-40s.

[0055] In the present invention, degumming can be performed by multi-stage flushing with compressed gas. During degumming, compressed gas passes through the filter element and the wind pressure decreases. In the S41 stage, the wind pressure is relatively large and the flushing time is relatively short. This stage is mainly used to flush out the binder filling the pores of the filter element. In the S42 stage, the wind pressure decreases and the time is prolonged. While flushing the binder in the pores of the filter element, the filter element coated on the resin fiber is prevented from being flushed away. In the S43 stage, the wind pressure further decreases and the time is further prolonged, which can ensure that the binder solution in the pores of the filter element is cleaned, and the binder solution coated on the surface of the resin fiber can form a skin-core structure after curing, thereby ensuring good bonding performance between the resin fibers.

[0056] Furthermore, the degumming in step S4 is centrifugal degumming, and the centrifugal speed is 1500-3000r / min.

[0057] The filter element can also be degummed by centrifugation. However, if the centrifugal speed is too low, the binder in the gaps of the filter element may not be completely removed, and it is easy to get clogged after curing. If the speed is too high, there will be too little binder solution coated on the resin fiber after degumming, and the resin fiber cannot be well bonded after curing.

[0058] Furthermore, the curing in step S5 is a multi-stage curing, during which the gas passes through the filter element and the pressure and temperature increase gradually:

[0059] S51: pressure 2-50kpa; curing temperature 100-120℃;

[0060] S52: pressure 2-50kpa; curing temperature 150-170℃;

[0061] S53: pressure 5-100kpa; curing temperature 190-210℃.

[0062] In the present invention, the filter element is cured by a multi-stage, gas-through-filtration method after degumming. In the S51 stage, the gas pressure is relatively small and the gas temperature used for curing is also relatively low. At this time, the adhesive cures relatively slowly. Subsequently, in the S52 and S53 stages, the pressure and curing temperature are gradually increased, so that the adhesive is heated more evenly and completely cured under uniform heating, which can ensure that the degree of curing is the same in each area.

[0063] The invention discloses an application of a resin-bonded solidified filter element in coating filtration.

[0064] The resin bonded and cured filter element of the present invention has a small difference in expansion degree between various regions in the cross-sectional direction, the binder is completely cured, and there are few uncured binder small molecules. During the coating filtration process, the binder small molecules can be effectively prevented from mixing into the filtrate and affecting the coating quality. At the same time, complete curing can also give good bonding between fibers, preventing the filter element interception rate from being affected when the filtration is under pressure, thereby ensuring filtration stability. DETAILED DESCRIPTION

[0065] In order to more clearly understand the above-mentioned purpose, features and advantages of the present invention, the present invention is further described in detail below in conjunction with specific embodiments. It should be noted that the embodiments of the present application and the features in the embodiments can be combined with each other without conflict.

[0066] In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited to the specific embodiments disclosed below.

[0067] Embodiment 1:

[0068] A resin bonded solidified filter element, the filter element comprising PET resin fibers, having a permeable liquid inlet surface and a liquid outlet surface away from the liquid inlet surface and also permeable, and forming an axial hollow flow channel; wherein the outer diameter of the filter element is 64 mm, the diameter of the axial hollow flow channel is 28 mm, the radial distance h2 between the liquid inlet surface and the liquid outlet surface is 18 mm, and the length of the filter element is 254 mm;

[0069] The PET resin fiber is coated with a phenolic resin binder to form a skin-core structure, and the phenolic resin binder is cured and bonded;

[0070] The filter element is immersed in the organic solvent ethanol, and the volume of the organic solvent absorbed by the phenolic resin binder in the filter element per unit weight is used to represent the expansion degree. In the radial section of the filter element:

[0071] The first area is 0-25% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 4.8 mL / kg;

[0072] The second area is 25-50% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 5.3 mL / kg;

[0073] The third area is 50-75% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 6.9 mL / kg;

[0074] The fourth area is 75-100% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 5.9 mL / kg;

[0075] The standard deviation of the swelling degree of each region is 0.78 mL / kg, and the ratio between the standard deviation of the swelling degree and the average swelling degree of the first region is 0.16, the ratio between the standard deviation of the swelling degree and the average swelling degree of the second region is 0.15, the ratio between the standard deviation of the swelling degree and the average swelling degree of the third region is 0.11, and the ratio between the standard deviation of the swelling degree and the average swelling degree of the fourth region is 0.13;

[0076] The phenolic resin binder in the filter element accounts for 55%; the interception rate for particles with a particle size of 10 μm is 99%; the flow rate is 7.5 kPa;

[0077] A method for preparing a resin-bonded and cured filter element comprises the following steps:

[0078] S1: Material selection: Select fiber with a diameter of 15-25μm, a thickness of 1mm, and a weight of 100g / m 2 PET resin fiber non-woven fabric;

[0079] S2: Winding: Prepare a phenolic resin binder solution with a concentration of 300wt%, spray the phenolic resin binder solution on the surface of the non-woven fabric, the spraying amount is 70% of the gram weight, and then wind it under a tension of 6N to obtain a wound filter element, and the number of winding layers n is 12 layers;

[0080] S3: Immersing: Immersing the wound filter element in a phenolic resin binder solution at 25° C. for 50 minutes to obtain a primary filter element;

[0081] S4: Debonding: Use compressed gas for multi-stage flushing. The compressed gas passes through the filter element, and the wind pressure decreases gradually to remove excess binder solution:

[0082] S41: The compressed gas pressure is 68kpa and the flushing time is 3s;

[0083] S42: The compressed gas pressure is 25 kPa and the flushing time is 15 s;

[0084] S43: The wind pressure of the compressed gas is 6 kPa, and the flushing time is 27 seconds;

[0085] S5: Curing: Use gas to circulate and cure the debonded filter element. The curing is a multi-stage curing. During the curing, the gas passes through the filter element, and the pressure and temperature increase gradually to prepare a resin-bonded cured filter element.

[0086] S51: pressure 11kpa; curing temperature 110℃;

[0087] S52: pressure 12kpa; curing temperature 155℃;

[0088] S53: pressure 27kpa; curing temperature 205℃.

[0089] Expansion test method: first weigh the weight G0 of the filter element in different areas, then soak it in water, take it out and dry the surface. At this time, the water fills the gaps in the filter element, and weigh the weight G1; after drying, soak it in ethanol at 50°C for 24 hours. At this time, the binder is completely swollen by ethanol, dry the surface and weigh G2, and calculate the expansion rate ((G2-G0) / ρ2-(G1-G0) / ρ1) / G0.

[0090] Interception rate test method: refer to standard DLT 1357-2014, where the powder adopts ISO 12103-1A4 test powder, the medium is water, and the flow rate is 65L / min.

[0091] Flow rate test method: Reference standard JIS K 3831-1990, where the medium is water and the flow rate is 65L / min.

[0092] Embodiment 2:

[0093] A resin bonded solidified filter element, the filter element comprising PET resin fibers, having a permeable liquid inlet surface and a liquid outlet surface away from the liquid inlet surface and also permeable, and forming an axial hollow flow channel; wherein the outer diameter of the filter element is 64 mm, the diameter of the axial hollow flow channel is 28 mm, the radial distance h2 between the liquid inlet surface and the liquid outlet surface is 18 mm, and the length of the filter element is 254 mm;

[0094] The PET resin fiber is coated with a phenolic resin binder to form a skin-core structure, and the phenolic resin binder is cured and bonded;

[0095] The filter element is immersed in the organic solvent ethanol, and the volume of the organic solvent absorbed by the phenolic resin binder in the filter element per unit weight is used to represent the expansion degree. In the radial section of the filter element:

[0096] The first area is 0-25% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 7.2 mL / kg;

[0097] The second area is 25-50% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 5.1 mL / kg;

[0098] The third area is 50-75% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 6.8 mL / kg;

[0099] The fourth area is 75-100% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 5.9 mL / kg;

[0100] The standard deviation of the swelling degree of each region is 0.81 mL / kg, and the ratio between the standard deviation of the swelling degree and the average swelling degree of the first region is 0.11, the ratio between the standard deviation of the swelling degree and the average swelling degree of the second region is 0.16, the ratio between the standard deviation of the swelling degree and the average swelling degree of the third region is 0.12, and the ratio between the standard deviation of the swelling degree and the average swelling degree of the fourth region is 0.14;

[0101] The phenolic resin binder in the filter element accounts for 59%; the interception rate for particles with a particle size of 10 μm is 99%; the flow rate is 7.8 kPa;

[0102] A method for preparing a resin-bonded and cured filter element comprises the following steps:

[0103] S1: Material selection: Select fiber with a diameter of 15-20μm, a thickness of 1mm, and a weight of 100g / m 2 PET resin fiber non-woven fabric;

[0104] S2: Winding: Prepare a phenolic resin binder solution with a concentration of 300wt%, spray the phenolic resin binder solution on the surface of the non-woven fabric, the spraying amount is 62% of the gram weight, and then wind it under a tension of 7N to obtain a wound filter element, and the number of winding layers n is 12 layers;

[0105] S3: Immersing: Immersing the wound filter element in a phenolic resin binder solution at 25° C. for 50 minutes to obtain a primary filter element;

[0106] S4: Debonding: Use compressed gas for multi-stage flushing. The compressed gas passes through the filter element, and the wind pressure decreases gradually to remove excess binder solution:

[0107] S41: The compressed gas pressure is 63kpa and the flushing time is 3s;

[0108] S42: The compressed gas pressure is 22kpa and the flushing time is 18s;

[0109] S43: The wind pressure of the compressed gas is 5kpa and the flushing time is 30s;

[0110] S5: Curing: Use gas to circulate and cure the debonded filter element. The curing is a multi-stage curing. During the curing, the gas passes through the filter element, and the pressure and temperature increase gradually to prepare a resin-bonded cured filter element.

[0111] S51: pressure 12kpa; curing temperature 110℃;

[0112] S52: pressure 13kpa; curing temperature 150℃;

[0113] S53: pressure 30kpa; curing temperature 195℃.

[0114] Embodiment 3:

[0115] A resin bonded solidified filter element, the filter element comprising PET resin fibers, having a permeable liquid inlet surface and a liquid outlet surface away from the liquid inlet surface and also permeable, and forming an axial hollow flow channel; wherein the outer diameter of the filter element is 64 mm, the diameter of the axial hollow flow channel is 28 mm, the radial distance h2 between the liquid inlet surface and the liquid outlet surface is 18 mm, and the length of the filter element is 254 mm;

[0116] The PET resin fiber is coated with a phenolic resin binder to form a skin-core structure, and the phenolic resin binder is cured and bonded;

[0117] The filter element is immersed in the organic solvent ethanol, and the volume of the organic solvent absorbed by the phenolic resin binder in the filter element per unit weight is used to represent the expansion degree. In the radial section of the filter element:

[0118] The first area is 0-25% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 7.7 mL / kg;

[0119] The second area is 25-50% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 6.9 mL / kg;

[0120] The third area is 50-75% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 6.3 mL / kg;

[0121] The fourth area is 75-100% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 5.8 mL / kg;

[0122] The standard deviation of the swelling degree of each region is 0.71 mL / kg, and the ratio between the standard deviation of the swelling degree of the first region and the average swelling degree is 0.09, the ratio between the standard deviation of the swelling degree of the second region and the average swelling degree is 0.1, the ratio between the standard deviation of the swelling degree of the third region and the average swelling degree is 0.11, and the ratio between the standard deviation of the swelling degree of the fourth region and the average swelling degree is 0.12;

[0123] The phenolic resin binder in the filter element accounts for 61%; the interception rate for particles with a particle size of 10 μm is 99%; the flow rate is 8.9 kPa;

[0124] A method for preparing a resin-bonded and cured filter element comprises the following steps:

[0125] S1: Material selection: Select fiber with a diameter of 10-20μm, a thickness of 1mm, and a weight of 100g / m 2 PET resin fiber non-woven fabric;

[0126] S2: Winding: Prepare a phenolic resin binder solution with a concentration of 300wt%, spray the phenolic resin binder solution on the surface of the non-woven fabric, the spraying amount is 16% of the gram weight, and then wind it under a tension of 22N to obtain a wound filter element, and the number of winding layers n is 17 layers;

[0127] S3: Immersing: Immersing the wound filter element in a phenolic resin binder solution at 25° C. for 50 minutes to obtain a primary filter element;

[0128] S4: Debonding: Use compressed gas for multi-stage flushing. The compressed gas passes through the filter element, and the wind pressure decreases gradually to remove excess binder solution:

[0129] S41: The compressed gas pressure is 63kpa and the flushing time is 2s;

[0130] S42: The compressed gas pressure is 19 kPa and the flushing time is 15 seconds;

[0131] S43: The wind pressure of the compressed gas is 5kpa and the flushing time is 32s;

[0132] S5: Curing: Use gas to circulate and cure the debonded filter element. The curing is a multi-stage curing. During the curing, the gas passes through the filter element, and the pressure and temperature increase gradually to prepare a resin-bonded cured filter element.

[0133] S51: pressure 11kpa; curing temperature 108℃;

[0134] S52: pressure 10kpa; curing temperature 163℃;

[0135] S53: pressure 29kpa; curing temperature 199℃.

[0136] Embodiment 4:

[0137] A resin bonded solidified filter element, the filter element comprising PET resin fibers, having a permeable liquid inlet surface and a liquid outlet surface away from the liquid inlet surface and also permeable, and forming an axial hollow flow channel; wherein the outer diameter of the filter element is 64 mm, the diameter of the axial hollow flow channel is 28 mm, the radial distance h2 between the liquid inlet surface and the liquid outlet surface is 18 mm, and the length of the filter element is 254 mm;

[0138] The PET resin fiber is coated with a phenolic resin binder to form a skin-core structure, and the phenolic resin binder is cured and bonded;

[0139] The filter element is immersed in the organic solvent ethanol, and the volume of the organic solvent absorbed by the phenolic resin binder in the filter element per unit weight is used to represent the expansion degree. In the radial section of the filter element:

[0140] The first area is 0-25% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 7.3 mL / kg;

[0141] The second area is 25-50% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 5.1 mL / kg;

[0142] The third area is 50-75% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 4.2 mL / kg;

[0143] The fourth area is 75-100% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 6.2 mL / kg;

[0144] The standard deviation of the swelling degree of each region is 1.16 mL / kg, and the ratio between the standard deviation of the swelling degree and the average swelling degree of the first region is 0.16, the ratio between the standard deviation of the swelling degree and the average swelling degree of the second region is 0.23, the ratio between the standard deviation of the swelling degree and the average swelling degree of the third region is 0.28, and the ratio between the standard deviation of the swelling degree and the average swelling degree of the fourth region is 0.19;

[0145] The phenolic resin binder in the filter element accounts for 52%; the interception rate for particles with a particle size of 10 μm is 99%; the flow rate is 8.3 kpa;

[0146] A method for preparing a resin-bonded and cured filter element comprises the following steps:

[0147] S1: Material selection: Select fiber with a diameter of 15-25μm, a thickness of 1mm, and a weight of 100g / m 2 PET resin fiber non-woven fabric;

[0148] S2: Winding: Prepare a phenolic resin binder solution with a concentration of 300wt%, spray the phenolic resin binder solution on the surface of the non-woven fabric, the spraying amount is 45% of the gram weight, and then wind it under a tension of 130N to obtain a wound filter element, and the number of winding layers n is 14 layers;

[0149] S3: Immersing: Immersing the wound filter element in a phenolic resin binder solution at 25° C. for 50 minutes to obtain a primary filter element;

[0150] S4: Debonding: Use compressed gas for multi-stage flushing. The compressed gas passes through the filter element, and the wind pressure decreases gradually to remove excess binder solution:

[0151] S41: The compressed gas pressure is 60 kPa and the flushing time is 3 s;

[0152] S42: The compressed gas pressure is 18kpa and the flushing time is 16s;

[0153] S43: The wind pressure of the compressed gas is 4kpa and the flushing time is 35s;

[0154] S5: Curing: Use gas to circulate and cure the debonded filter element. The curing is a multi-stage curing. During the curing, the gas passes through the filter element, and the pressure and temperature increase gradually to prepare a resin-bonded cured filter element.

[0155] S51: pressure 10kpa; curing temperature 110℃;

[0156] S52: pressure 12kpa; curing temperature 165℃;

[0157] S53: pressure 28kpa; curing temperature 197℃.

[0158] Embodiment 5:

[0159] A resin bonded solidified filter element, the filter element comprising PET resin fibers, having a permeable liquid inlet surface and a liquid outlet surface away from the liquid inlet surface and also permeable, and forming an axial hollow flow channel; wherein the outer diameter of the filter element is 64 mm, the diameter of the axial hollow flow channel is 28 mm, the radial distance h2 between the liquid inlet surface and the liquid outlet surface is 18 mm, and the length of the filter element is 254 mm;

[0160] The PET resin fiber is coated with a phenolic resin binder to form a skin-core structure, and the phenolic resin binder is cured and bonded;

[0161] The filter element is immersed in the organic solvent ethanol, and the volume of the organic solvent absorbed by the phenolic resin binder in the filter element per unit weight is used to represent the expansion degree. In the radial section of the filter element:

[0162] The first area is 0-25% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 6.1 mL / kg;

[0163] The second area is 25-50% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 6.1 mL / kg;

[0164] The third area is 50-75% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 5.3 mL / kg;

[0165] The fourth area is 75-100% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 7.9 mL / kg;

[0166] The standard deviation of the swelling degree of each region is 0.94 mL / kg, and the ratio between the standard deviation of the swelling degree and the average swelling degree of the first region is 0.15, the ratio between the standard deviation of the swelling degree and the average swelling degree of the second region is 0.14, the ratio between the standard deviation of the swelling degree and the average swelling degree of the third region is 0.19, and the ratio between the standard deviation of the swelling degree and the average swelling degree of the fourth region is 0.12;

[0167] The phenolic resin binder in the filter element accounts for 64%; the interception rate for particles with a particle size of 10 μm is 99%; the flow rate is 15 kPa;

[0168] A method for preparing a resin-bonded and cured filter element comprises the following steps:

[0169] S1: Material selection: Select fiber with a diameter of 5-15μm, a thickness of 1mm, and a weight of 100g / m 2 PET resin fiber non-woven fabric;

[0170] S2: Winding: Prepare a phenolic resin binder solution with a concentration of 300wt%, spray the phenolic resin binder solution on the surface of the non-woven fabric, the spraying amount is 35% of the gram weight, and then wind it under a tension of 20N to obtain a wound filter element, and the number of winding layers n is 15 layers;

[0171] S3: Immersing: Immersing the wound filter element in a phenolic resin binder solution at 25° C. for 50 minutes to obtain a primary filter element;

[0172] S4: Debonding: Use compressed gas for multi-stage flushing. The compressed gas passes through the filter element, and the wind pressure decreases gradually to remove excess binder solution:

[0173] S41: The compressed gas pressure is 55 kPa and the flushing time is 5 seconds;

[0174] S42: The compressed gas pressure is 13kpa and the flushing time is 18s;

[0175] S43: The wind pressure of the compressed gas is 2kpa, and the flushing time is 40s;

[0176] S5: Curing: Use gas to circulate and cure the debonded filter element. The curing is a multi-stage curing. During the curing, the gas passes through the filter element, and the pressure and temperature increase gradually to prepare a resin-bonded cured filter element.

[0177] S51: pressure 4kpa; curing temperature 105℃;

[0178] S52: pressure 6kpa; curing temperature 170℃;

[0179] S53: pressure 23kpa; curing temperature 190℃.

[0180] Embodiment 6:

[0181] A resin bonded solidified filter element, the filter element comprising PET resin fibers, having a permeable liquid inlet surface and a liquid outlet surface away from the liquid inlet surface and also permeable, and forming an axial hollow flow channel; wherein the outer diameter of the filter element is 64 mm, the diameter of the axial hollow flow channel is 28 mm, the radial distance h2 between the liquid inlet surface and the liquid outlet surface is 18 mm, and the length of the filter element is 254 mm;

[0182] The PET resin fiber is coated with a phenolic resin binder to form a skin-core structure, and the phenolic resin binder is cured and bonded;

[0183] The filter element is immersed in the organic solvent ethanol, and the volume of the organic solvent absorbed by the phenolic resin binder in the filter element per unit weight is used to represent the expansion degree. In the radial section of the filter element:

[0184] The first area is 0-25% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 4.1 mL / kg;

[0185] The second area is 25-50% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 5.9 mL / kg;

[0186] The third area is 50-75% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 5.5 mL / kg;

[0187] The fourth area is 75-100% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 4.4 mL / kg;

[0188] The standard deviation of the swelling degree of each region is 0.73 mL / kg, and the ratio between the standard deviation of the swelling degree and the average swelling degree of the first region is 0.18, the ratio between the standard deviation of the swelling degree and the average swelling degree of the second region is 0.12, the ratio between the standard deviation of the swelling degree and the average swelling degree of the third region is 0.13, and the ratio between the standard deviation of the swelling degree and the average swelling degree of the fourth region is 0.16;

[0189] The phenolic resin binder in the filter element accounts for 45%; the interception rate for particles with a particle size of 10 μm is 99%; the flow rate is 6 kPa;

[0190] A method for preparing a resin-bonded and cured filter element comprises the following steps:

[0191] S1: Material selection: Select fiber with a diameter of 35-45μm, a thickness of 2mm, and a weight of 190g / m 2 PET resin fiber non-woven fabric;

[0192] S2: Winding: Prepare a phenolic resin binder solution with a concentration of 300wt%, spray the phenolic resin binder solution on the surface of the non-woven fabric, the spraying amount is 50% of the gram weight, and then wind it under a tension of 10N to obtain a wound filter element;

[0193] S3: Immersing: Immersing the wound filter element in a phenolic resin binder solution at 20° C. for 30 minutes to obtain a primary filter element;

[0194] S4: Debonding: Use compressed gas for multi-stage flushing. The compressed gas passes through the filter element, and the wind pressure decreases gradually to remove excess binder solution:

[0195] S41: The compressed gas pressure is 71 kPa and the flushing time is 3 s;

[0196] S42: The compressed gas pressure is 27 kPa and the flushing time is 13 s;

[0197] S43: The wind pressure of the compressed gas is 8kpa and the flushing time is 35s;

[0198] S5: Curing: Use gas to circulate and cure the debonded filter element. The curing is a multi-stage curing. During the curing, the gas passes through the filter element, and the pressure and temperature increase gradually to prepare a resin-bonded cured filter element.

[0199] S51: pressure 18kpa; curing temperature 110℃;

[0200] S52: pressure 23kpa; curing temperature 155℃;

[0201] S53: pressure 50kpa; curing temperature 205℃.

[0202] Embodiment 7:

[0203] A resin bonded solidified filter element, the filter element comprising PET resin fibers, having a permeable liquid inlet surface and a liquid outlet surface away from the liquid inlet surface and also permeable, and forming an axial hollow flow channel; wherein the outer diameter of the filter element is 64 mm, the diameter of the axial hollow flow channel is 28 mm, the radial distance h2 between the liquid inlet surface and the liquid outlet surface is 18 mm, and the length of the filter element is 254 mm;

[0204] The PET resin fiber is coated with a phenolic resin binder to form a skin-core structure, and the phenolic resin binder is cured and bonded;

[0205] The filter element is immersed in the organic solvent ethanol, and the volume of the organic solvent absorbed by the phenolic resin binder in the filter element per unit weight is used to represent the expansion degree. In the radial section of the filter element:

[0206] The first area is 0-25% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 5.2 mL / kg;

[0207] The second area is 25-50% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 3.8 mL / kg;

[0208] The third area is 50-75% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 4.7 mL / kg;

[0209] The fourth area is 75-100% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 4.4 mL / kg;

[0210] The standard deviation of the swelling degree of each region is 0.51 mL / kg, and the ratio between the standard deviation of the swelling degree and the average swelling degree of the first region is 0.10, the ratio between the standard deviation of the swelling degree and the average swelling degree of the second region is 0.13, the ratio between the standard deviation of the swelling degree and the average swelling degree of the third region is 0.11, and the ratio between the standard deviation of the swelling degree and the average swelling degree of the fourth region is 0.12;

[0211] The phenolic resin binder in the filter element accounts for 38%; the interception rate for particles with a particle size of 10 μm is 99%; the flow rate is 5 kPa;

[0212] A method for preparing a resin-bonded and cured filter element comprises the following steps:

[0213] S1: Material selection: Select fiber with a diameter of 40-50μm, a thickness of 2mm, and a weight of 190g / m 2 PET resin fiber non-woven fabric;

[0214] S2: Winding: Prepare a phenolic resin binder solution with a concentration of 300wt%, spray the phenolic resin binder solution on the surface of the non-woven fabric, the spraying amount is 50% of the gram weight, and then wind it under a tension of 10N to obtain a wound filter element;

[0215] S3: Immersing: Immersing the wound filter element in a phenolic resin binder solution at 20° C. for 30 minutes to obtain a primary filter element;

[0216] S4: Debonding: Use compressed gas for multi-stage flushing. The compressed gas passes through the filter element, and the wind pressure decreases gradually to remove excess binder solution:

[0217] S41: The compressed gas pressure is 71 kPa and the flushing time is 2 s;

[0218] S42: The compressed gas pressure is 27kpa and the flushing time is 8s;

[0219] S43: The wind pressure of the compressed gas is 7kpa and the flushing time is 28s;

[0220] S5: Curing: Use gas to circulate and cure the debonded filter element. The curing is a multi-stage curing. During the curing, the gas passes through the filter element, and the pressure and temperature increase gradually to prepare a resin-bonded cured filter element.

[0221] S51: pressure 21kpa; curing temperature 108℃;

[0222] S52: pressure 28kpa; curing temperature 162℃;

[0223] S53: pressure 54kpa; curing temperature 205℃.

[0224] Embodiment 8:

[0225] A resin bonded solidified filter element, the filter element comprising PET resin fibers, having a permeable liquid inlet surface and a liquid outlet surface away from the liquid inlet surface and also permeable, and forming an axial hollow flow channel; wherein the outer diameter of the filter element is 64 mm, the diameter of the axial hollow flow channel is 28 mm, the radial distance h2 between the liquid inlet surface and the liquid outlet surface is 18 mm, and the length of the filter element is 254 mm;

[0226] The PET resin fiber is coated with a phenolic resin binder to form a skin-core structure, and the phenolic resin binder is cured and bonded;

[0227] The filter element is immersed in the organic solvent ethanol, and the volume of the organic solvent absorbed by the phenolic resin binder in the filter element per unit weight is used to represent the expansion degree. In the radial section of the filter element:

[0228] The first area is 0-25% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 4 mL / kg;

[0229] The second area is 25-50% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 4.9 mL / kg;

[0230] The third area is 50-75% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 4.4 mL / kg;

[0231] The fourth area is 75-100% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 5.8 mL / kg;

[0232] The standard deviation of the swelling degree of each region is 0.67 mL / kg, and the ratio between the standard deviation of the swelling degree and the average swelling degree of the first region is 0.17, the ratio between the standard deviation of the swelling degree and the average swelling degree of the second region is 0.14, the ratio between the standard deviation of the swelling degree and the average swelling degree of the third region is 0.15, and the ratio between the standard deviation of the swelling degree and the average swelling degree of the fourth region is 0.12;

[0233] The phenolic resin binder in the filter element accounts for 42%; the interception rate for particles with a particle size of 10 μm is 99%; the flow rate is 5.2 kPa;

[0234] A method for preparing a resin-bonded and cured filter element comprises the following steps:

[0235] S1: Material selection: Select fiber with a diameter of 40-45μm, a thickness of 2mm, and a weight of 190g / m 2 PET resin fiber non-woven fabric;

[0236] S2: Winding: Prepare a phenolic resin binder solution with a concentration of 300wt%, spray the phenolic resin binder solution on the surface of the non-woven fabric, the spraying amount is 50% of the gram weight, and then wind it under a tension of 10N to obtain a wound filter element;

[0237] S3: Immersing: Immersing the wound filter element in a phenolic resin binder solution at 20° C. for 30 minutes to obtain a primary filter element;

[0238] S4: Debonding: Use compressed gas for multi-stage flushing. The compressed gas passes through the filter element, and the wind pressure decreases gradually to remove excess binder solution:

[0239] S41: The compressed gas pressure is 76 kPa and the flushing time is 3 s;

[0240] S42: The compressed gas pressure is 29 kPa and the flushing time is 14 seconds;

[0241] S43: The wind pressure of the compressed gas is 7 kpa and the flushing time is 31 s;

[0242] S5: Curing: Use gas to circulate and cure the debonded filter element. The curing is a multi-stage curing. During the curing, the gas passes through the filter element, and the pressure and temperature increase gradually to prepare a resin-bonded cured filter element.

[0243] S51: pressure 20kpa; curing temperature 105℃;

[0244] S52: pressure 26kpa; curing temperature 162℃;

[0245] S53: pressure 61kpa; curing temperature 197℃.

[0246] Embodiment 9:

[0247] A resin bonded solidified filter element, the filter element comprising PET resin fibers, having a permeable liquid inlet surface and a liquid outlet surface away from the liquid inlet surface and also permeable, and forming an axial hollow flow channel; wherein the outer diameter of the filter element is 64 mm, the diameter of the axial hollow flow channel is 28 mm, the radial distance h2 between the liquid inlet surface and the liquid outlet surface is 18 mm, and the length of the filter element is 254 mm;

[0248] The PET resin fiber is coated with a phenolic resin binder to form a skin-core structure, and the phenolic resin binder is cured and bonded;

[0249] The filter element is immersed in the organic solvent ethanol, and the volume of the organic solvent absorbed by the phenolic resin binder in the filter element per unit weight is used to represent the expansion degree. In the radial section of the filter element:

[0250] The first area is 0-25% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 5.1 mL / kg;

[0251] The second area is 25-50% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 4.6 mL / kg;

[0252] The third area is 50-75% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 5.7 mL / kg;

[0253] The fourth area is 75-100% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 4.1 mL / kg;

[0254] The standard deviation of the swelling degree of each region is 0.59 mL / kg, and the ratio between the standard deviation of the swelling degree and the average swelling degree of the first region is 0.12, the ratio between the standard deviation of the swelling degree and the average swelling degree of the second region is 0.13, the ratio between the standard deviation of the swelling degree and the average swelling degree of the third region is 0.1, and the ratio between the standard deviation of the swelling degree and the average swelling degree of the fourth region is 0.14;

[0255] The phenolic resin binder in the filter element accounts for 46%; the interception rate for particles with a particle size of 10 μm is 99%; the flow rate is 5.4 kPa;

[0256] A method for preparing a resin-bonded and cured filter element comprises the following steps:

[0257] S1: Material selection: Select fiber with a diameter of 35-40μm, a thickness of 2mm, and a weight of 190g / m 2 PET resin fiber non-woven fabric;

[0258] S2: Winding: Prepare a phenolic resin binder solution with a concentration of 300wt%, spray the phenolic resin binder solution on the surface of the non-woven fabric, the spraying amount is 50% of the gram weight, and then wind it under a tension of 10N to obtain a wound filter element;

[0259] S3: Immersing: Immersing the wound filter element in a phenolic resin binder solution at 20° C. for 30 minutes to obtain a primary filter element;

[0260] S4: Debonding: Use compressed gas for multi-stage flushing. The compressed gas passes through the filter element, and the wind pressure decreases gradually to remove excess binder solution:

[0261] S41: The compressed gas pressure is 75 kPa and the flushing time is 4 seconds;

[0262] S42: The compressed gas pressure is 30 kPa and the flushing time is 13 s;

[0263] S43: The wind pressure of the compressed gas is 8kpa and the flushing time is 27s;

[0264] S5: Curing: Use gas to circulate and cure the debonded filter element. The curing is a multi-stage curing. During the curing, the gas passes through the filter element, and the pressure and temperature increase gradually to prepare a resin-bonded cured filter element.

[0265] S51: pressure 22kpa; curing temperature 108℃;

[0266] S52: pressure 25kpa; curing temperature 155℃;

[0267] S53: pressure 60kpa; curing temperature 205℃.

[0268] Embodiment 10:

[0269] A resin bonded solidified filter element, the filter element comprising PET resin fibers, having a permeable liquid inlet surface and a liquid outlet surface away from the liquid inlet surface and also permeable, and forming an axial hollow flow channel; wherein the outer diameter of the filter element is 64 mm, the diameter of the axial hollow flow channel is 28 mm, the radial distance h2 between the liquid inlet surface and the liquid outlet surface is 18 mm, and the length of the filter element is 254 mm;

[0270] The PET resin fiber is coated with a phenolic resin binder to form a skin-core structure, and the phenolic resin binder is cured and bonded;

[0271] The filter element is immersed in the organic solvent ethanol, and the volume of the organic solvent absorbed by the phenolic resin binder in the filter element per unit weight is used to represent the expansion degree. In the radial section of the filter element:

[0272] The first area is 0-25% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 4.2 mL / kg;

[0273] The second area is 25-50% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 5 mL / kg;

[0274] The third area is 50-75% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 4.8 mL / kg;

[0275] The fourth area is 75-100% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 3.6 mL / kg;

[0276] The standard deviation of the swelling degree of each region is 0.55 mL / kg, and the ratio between the standard deviation of the swelling degree and the average swelling degree of the first region is 0.13, the ratio between the standard deviation of the swelling degree and the average swelling degree of the second region is 0.11, the ratio between the standard deviation of the swelling degree and the average swelling degree of the third region is 0.11, and the ratio between the standard deviation of the swelling degree and the average swelling degree of the fourth region is 0.15;

[0277] The phenolic resin binder in the filter element accounts for 34%; the interception rate for particles with a particle size of 10 μm is 99%; the flow rate is 4.5 kPa;

[0278] A method for preparing a resin-bonded and cured filter element comprises the following steps:

[0279] S1: Material selection: Select fiber with a diameter of 45-60μm, a thickness of 2mm, and a weight of 190g / m 2 PET resin fiber non-woven fabric;

[0280] S2: Winding: Prepare a phenolic resin binder solution with a concentration of 300wt%, spray the phenolic resin binder solution on the surface of the non-woven fabric, the spraying amount is 50% of the gram weight, and then wind it under a tension of 10N to obtain a wound filter element;

[0281] S3: Immersing: Immersing the wound filter element in a phenolic resin binder solution at 20° C. for 30 minutes to obtain a primary filter element;

[0282] S4: Debonding: Use compressed gas for multi-stage flushing. The compressed gas passes through the filter element, and the wind pressure decreases gradually to remove excess binder solution:

[0283] S41: The compressed gas pressure is 77 kpa and the flushing time is 4 seconds;

[0284] S42: The compressed gas pressure is 31 kPa and the flushing time is 16 seconds;

[0285] S43: The wind pressure of the compressed gas is 8kpa and the flushing time is 35s;

[0286] S5: Curing: Use gas to circulate and cure the debonded filter element. The curing is a multi-stage curing. During the curing, the gas passes through the filter element, and the pressure and temperature increase gradually to prepare a resin-bonded cured filter element.

[0287] S51: pressure 23kpa; curing temperature 105℃;

[0288] S52: pressure 29kpa; curing temperature 155℃;

[0289] S53: pressure 63kpa; curing temperature 200℃.

[0290] Embodiment 11:

[0291] A resin bonded solidified filter element, the filter element comprising PET resin fibers, having a permeable liquid inlet surface and a liquid outlet surface away from the liquid inlet surface and also permeable, and forming an axial hollow flow channel; wherein the outer diameter of the filter element is 64 mm, the diameter of the axial hollow flow channel is 28 mm, the radial distance h2 between the liquid inlet surface and the liquid outlet surface is 18 mm, and the length of the filter element is 254 mm;

[0292] The PET resin fiber is coated with a phenolic resin binder to form a skin-core structure, and the phenolic resin binder is cured and bonded;

[0293] The filter element is immersed in the organic solvent ethanol, and the volume of the organic solvent absorbed by the phenolic resin binder in the filter element per unit weight is used to represent the expansion degree. In the radial section of the filter element:

[0294] The first area is 0-25% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 4.2 mL / kg;

[0295] The second area is 25-50% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 4.5 mL / kg;

[0296] The third area is 50-75% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 3.1 mL / kg;

[0297] The fourth area is 75-100% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 3.8 mL / kg;

[0298] The standard deviation of the swelling degree of each region is 0.52 mL / kg, and the ratio between the standard deviation of the swelling degree and the average swelling degree of the first region is 0.12, the ratio between the standard deviation of the swelling degree and the average swelling degree of the second region is 0.12, the ratio between the standard deviation of the swelling degree and the average swelling degree of the third region is 0.17, and the ratio between the standard deviation of the swelling degree and the average swelling degree of the fourth region is 0.14;

[0299] The phenolic resin binder in the filter element accounts for 29%; the interception rate for particles with a particle size of 10 μm is 99%; the flow rate is 3 kPa;

[0300] A method for preparing a resin-bonded and cured filter element comprises the following steps:

[0301] S1: Material selection: Select fiber with a diameter of 70-80μm, a thickness of 3.5mm, and a weight of 280g / m 2 PET resin fiber non-woven fabric;

[0302] S2: Winding: Prepare a phenolic resin binder solution with a concentration of 300wt%, spray the phenolic resin binder solution on the surface of the non-woven fabric, the spraying amount is 50% of the gram weight, and then wind it under a tension of 10N to obtain a wound filter element;

[0303] S3: Immersing: Immersing the wound filter element in a phenolic resin binder solution at 20° C. for 20 minutes to obtain a primary filter element;

[0304] S4: Debonding: Use compressed gas for multi-stage flushing. The compressed gas passes through the filter element, and the wind pressure decreases gradually to remove excess binder solution:

[0305] S41: The wind pressure of the compressed gas is 80kpa and the flushing time is 4s;

[0306] S42: The wind pressure of the compressed gas is 35kpa, and the flushing time is 12s;

[0307] S43: The wind pressure of the compressed gas is 9 kPa and the flushing time is 33 s;

[0308] S5: Curing: Use gas to circulate and cure the debonded filter element. The curing is a multi-stage curing. During the curing, the gas passes through the filter element, and the pressure and temperature increase gradually to prepare a resin-bonded cured filter element.

[0309] S51: pressure 31kpa; curing temperature 110℃;

[0310] S52: pressure 35kpa; curing temperature 165℃;

[0311] S53: pressure 80kpa; curing temperature 203℃.

[0312] Embodiment 12:

[0313] A resin bonded solidified filter element, the filter element comprising PET resin fibers, having a permeable liquid inlet surface and a liquid outlet surface away from the liquid inlet surface and also permeable, and forming an axial hollow flow channel; wherein the outer diameter of the filter element is 64 mm, the diameter of the axial hollow flow channel is 28 mm, the radial distance h2 between the liquid inlet surface and the liquid outlet surface is 18 mm, and the length of the filter element is 254 mm;

[0314] The PET resin fiber is coated with a phenolic resin binder to form a skin-core structure, and the phenolic resin binder is cured and bonded;

[0315] The filter element is immersed in the organic solvent ethanol, and the volume of the organic solvent absorbed by the phenolic resin binder in the filter element per unit weight is used to represent the expansion degree. In the radial section of the filter element:

[0316] The first area is 0-25% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 3.8 mL / kg;

[0317] The second area is 25-50% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 3.4 mL / kg;

[0318] The third area is 50-75% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 4.1 mL / kg;

[0319] The fourth area is 75-100% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 4.4 mL / kg;

[0320] The standard deviation of the swelling degree of each region is 0.37 mL / kg, and the ratio between the standard deviation of the swelling degree of the first region and the average swelling degree is 0.1, the ratio between the standard deviation of the swelling degree of the second region and the average swelling degree is 0.11, the ratio between the standard deviation of the swelling degree of the third region and the average swelling degree is 0.09, and the ratio between the standard deviation of the swelling degree of the fourth region and the average swelling degree is 0.08;

[0321] The phenolic resin binder in the filter element accounts for 28%; the interception rate for particles with a particle size of 10 μm is 99%; the flow rate is 2 kPa;

[0322] A method for preparing a resin-bonded and cured filter element comprises the following steps:

[0323] S1: Material selection: Select fiber with a diameter of 75-85μm, a thickness of 3.5mm, and a weight of 280g / m 2 PET resin fiber non-woven fabric;

[0324] S2: Winding: Prepare a phenolic resin binder solution with a concentration of 300wt%, spray the phenolic resin binder solution on the surface of the non-woven fabric, the spraying amount is 50% of the gram weight, and then wind it under a tension of 10N to obtain a wound filter element;

[0325] S3: Immersing: Immersing the wound filter element in a phenolic resin binder solution at 20° C. for 20 minutes to obtain a primary filter element;

[0326] S4: Debonding: Use compressed gas for multi-stage flushing. The compressed gas passes through the filter element, and the wind pressure decreases gradually to remove excess binder solution:

[0327] S41: The compressed gas pressure is 82 kPa and the flushing time is 3 s;

[0328] S42: The compressed gas pressure is 37 kPa and the flushing time is 11 s;

[0329] S43: The compressed gas pressure is 11 kPa and the flushing time is 25 seconds;

[0330] S5: Curing: Use gas to circulate and cure the debonded filter element. The curing is a multi-stage curing. During the curing, the gas passes through the filter element, and the pressure and temperature increase gradually to prepare a resin-bonded cured filter element.

[0331] S51: pressure 36kpa; curing temperature 105℃;

[0332] S52: pressure 39kpa; curing temperature 160℃;

[0333] S53: pressure 83kpa; curing temperature 200℃.

[0334] Embodiment 13:

[0335] A resin bonded solidified filter element, the filter element comprising PET resin fibers, having a permeable liquid inlet surface and a liquid outlet surface away from the liquid inlet surface and also permeable, and forming an axial hollow flow channel; wherein the outer diameter of the filter element is 64 mm, the diameter of the axial hollow flow channel is 28 mm, the radial distance h2 between the liquid inlet surface and the liquid outlet surface is 18 mm, and the length of the filter element is 254 mm;

[0336] The PET resin fiber is coated with a phenolic resin binder to form a skin-core structure, and the phenolic resin binder is cured and bonded;

[0337] The filter element is immersed in the organic solvent ethanol, and the volume of the organic solvent absorbed by the phenolic resin binder in the filter element per unit weight is used to represent the expansion degree. In the radial section of the filter element:

[0338] The first area is 0-25% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 3.4 mL / kg;

[0339] The second area is 25-50% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 3.1 mL / kg;

[0340] The third area is 50-75% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 3.2 mL / kg;

[0341] The fourth area is 75-100% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 2.8 mL / kg;

[0342] The standard deviation of the swelling degree of each region is 0.21 mL / kg, and the ratio between the standard deviation of the swelling degree and the average swelling degree of the first region is 0.06, the ratio between the standard deviation of the swelling degree and the average swelling degree of the second region is 0.07, the ratio between the standard deviation of the swelling degree and the average swelling degree of the third region is 0.07, and the ratio between the standard deviation of the swelling degree and the average swelling degree of the fourth region is 0.08;

[0343] The phenolic resin binder in the filter element accounts for 24%; the interception rate for particles with a particle size of 10 μm is 99%; the flow rate is 1 kPa;

[0344] A method for preparing a resin-bonded and cured filter element comprises the following steps:

[0345] S1: Material selection: Select fiber with a diameter of 75-90μm, a thickness of 3.5mm, and a weight of 280g / m 2 PET resin fiber non-woven fabric;

[0346] S2: Winding: Prepare a phenolic resin binder solution with a concentration of 300wt%, spray the phenolic resin binder solution on the surface of the non-woven fabric, the spraying amount is 50% of the gram weight, and then wind it under a tension of 10N to obtain a wound filter element;

[0347] S3: Immersing: Immersing the wound filter element in a phenolic resin binder solution at 20° C. for 20 minutes to obtain a primary filter element;

[0348] S4: Debonding: Use compressed gas for multi-stage flushing. The compressed gas passes through the filter element, and the wind pressure decreases gradually to remove excess binder solution:

[0349] S41: The wind pressure of the compressed gas is 88kpa, and the flushing time is 2s;

[0350] S42: The compressed gas pressure is 41 kPa and the flushing time is 16 seconds;

[0351] S43: The wind pressure of the compressed gas is 13kpa, and the flushing time is 20s;

[0352] S5: Curing: Use gas to circulate and cure the debonded filter element. The curing is a multi-stage curing. During the curing, the gas passes through the filter element, and the pressure and temperature increase gradually to prepare a resin-bonded cured filter element.

[0353] S51: pressure 40kpa; curing temperature 105℃;

[0354] S52: pressure 45kpa; curing temperature 160℃;

[0355] S53: pressure 88kpa; curing temperature 195℃.

[0356] Embodiment 14:

[0357] A resin bonded solidified filter element, the filter element comprising PET resin fibers, having a permeable liquid inlet surface and a liquid outlet surface away from the liquid inlet surface and also permeable, and forming an axial hollow flow channel; wherein the outer diameter of the filter element is 64 mm, the diameter of the axial hollow flow channel is 28 mm, the radial distance h2 between the liquid inlet surface and the liquid outlet surface is 18 mm, and the length of the filter element is 254 mm;

[0358] The PET resin fiber is coated with a phenolic resin binder to form a skin-core structure, and the phenolic resin binder is cured and bonded;

[0359] The filter element is immersed in the organic solvent ethanol, and the volume of the organic solvent absorbed by the phenolic resin binder in the filter element per unit weight is used to represent the expansion degree. In the radial section of the filter element:

[0360] The first area is 0-25% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 4.1 mL / kg;

[0361] The second area is 25-50% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 3.5 mL / kg;

[0362] The third area is 50-75% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 3.4 mL / kg;

[0363] The fourth area is 75-100% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 4.6 mL / kg;

[0364] The standard deviation of the swelling degree of each region is 0.48 mL / kg, and the ratio between the standard deviation of the swelling degree and the average swelling degree of the first region is 0.12, the ratio between the standard deviation of the swelling degree and the average swelling degree of the second region is 0.14, the ratio between the standard deviation of the swelling degree and the average swelling degree of the third region is 0.14, and the ratio between the standard deviation of the swelling degree and the average swelling degree of the fourth region is 0.11;

[0365] The phenolic resin binder in the filter element accounts for 31%; the interception rate for particles with a particle size of 10 μm is 99%; the flow rate is 0.5 kpa;

[0366] A method for preparing a resin-bonded and cured filter element comprises the following steps:

[0367] S1: Material selection: Select fiber with a diameter of 70-75μm, a thickness of 3.5mm, and a weight of 280g / m 2 PET resin fiber non-woven fabric;

[0368] S2: Winding: Prepare a phenolic resin binder solution with a concentration of 300wt%, spray the phenolic resin binder solution on the surface of the non-woven fabric, the spraying amount is 50% of the gram weight, and then wind it under a tension of 10N to obtain a wound filter element;

[0369] S3: Immersing: Immersing the wound filter element in a phenolic resin binder solution at 20° C. for 20 minutes to obtain a primary filter element;

[0370] S4: Debonding: Use compressed gas for multi-stage flushing. The compressed gas passes through the filter element, and the wind pressure decreases gradually to remove excess binder solution:

[0371] S41: The wind pressure of the compressed gas is 90kpa, and the flushing time is 2s;

[0372] S42: The compressed gas pressure is 46 kPa and the flushing time is 15 seconds;

[0373] S43: The compressed gas pressure is 13kpa and the flushing time is 25s;

[0374] S5: Curing: Use gas to circulate and cure the debonded filter element. The curing is a multi-stage curing. During the curing, the gas passes through the filter element, and the pressure and temperature increase gradually to prepare a resin-bonded cured filter element.

[0375] S51: pressure 43kpa; curing temperature 110℃;

[0376] S52: pressure 47kpa; curing temperature 160℃;

[0377] S53: pressure 93kpa; curing temperature 205℃.

[0378] Embodiment 15:

[0379] A resin bonded solidified filter element, the filter element comprising PET resin fibers, having a permeable liquid inlet surface and a liquid outlet surface away from the liquid inlet surface and also permeable, and forming an axial hollow flow channel; wherein the outer diameter of the filter element is 64 mm, the diameter of the axial hollow flow channel is 28 mm, the radial distance h2 between the liquid inlet surface and the liquid outlet surface is 18 mm, and the length of the filter element is 254 mm;

[0380] The PET resin fiber is coated with a phenolic resin binder to form a skin-core structure, and the phenolic resin binder is cured and bonded;

[0381] The filter element is immersed in the organic solvent ethanol, and the volume of the organic solvent absorbed by the phenolic resin binder in the filter element per unit weight is used to represent the expansion degree. In the radial section of the filter element:

[0382] The first area is 0-25% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 2.8 mL / kg;

[0383] The second area is 25-50% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 3 mL / kg;

[0384] The third area is 50-75% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 3.1 mL / kg;

[0385] The fourth area is 75-100% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 2.5 mL / kg;

[0386] The standard deviation of the swelling degree of each region is 0.23 mL / kg, and the ratio between the standard deviation of the swelling degree of the first region and the average swelling degree is 0.08, the ratio between the standard deviation of the swelling degree of the second region and the average swelling degree is 0.08, the ratio between the standard deviation of the swelling degree of the third region and the average swelling degree is 0.07, and the ratio between the standard deviation of the swelling degree of the fourth region and the average swelling degree is 0.09;

[0387] The phenolic resin binder in the filter element accounts for 22%; the interception rate for particles with a particle size of 10 μm is 99%; the flow rate is 0.1 kPa;

[0388] A method for preparing a resin-bonded and cured filter element comprises the following steps:

[0389] S1: Material selection: Select fiber with a diameter of 80-100μm, a thickness of 3.5mm, and a weight of 280g / m 2 PET resin fiber non-woven fabric;

[0390] S2: Winding: Prepare a phenolic resin binder solution with a concentration of 300wt%, spray the phenolic resin binder solution on the surface of the non-woven fabric, the spraying amount is 50% of the gram weight, and then wind it under a tension of 10N to obtain a wound filter element;

[0391] S3: Immersing: Immersing the wound filter element in a phenolic resin binder solution at 20° C. for 20 minutes to obtain a primary filter element;

[0392] S4: Debonding: Use compressed gas for multi-stage flushing. The compressed gas passes through the filter element, and the wind pressure decreases gradually to remove excess binder solution:

[0393] S41: The wind pressure of the compressed gas is 90kpa, and the flushing time is 3s;

[0394] S42: The wind pressure of the compressed gas is 50kpa, and the flushing time is 15s;

[0395] S43: The wind pressure of the compressed gas is 15kpa and the flushing time is 30s;

[0396] S5: Curing: Use gas to circulate and cure the debonded filter element. The curing is a multi-stage curing. During the curing, the gas passes through the filter element, and the pressure and temperature increase gradually to prepare a resin-bonded cured filter element.

[0397] S51: pressure 45kpa; curing temperature 120℃;

[0398] S52: pressure 50kpa; curing temperature 170℃;

[0399] S53: pressure 100kpa; curing temperature 210℃.

[0400] Embodiment 16:

[0401] A resin bonded solidified filter element, the filter element comprising PET resin fibers, having a permeable liquid inlet surface and a liquid outlet surface away from the liquid inlet surface and also permeable, and forming an axial hollow flow channel; wherein the outer diameter of the filter element is 64 mm, the diameter of the axial hollow flow channel is 28 mm, the radial distance h2 between the liquid inlet surface and the liquid outlet surface is 18 mm, and the length of the filter element is 254 mm;

[0402] The PET resin fiber is coated with a phenolic resin binder to form a skin-core structure, and the phenolic resin binder is cured and bonded;

[0403] The filter element is immersed in the organic solvent ethanol, and the volume of the organic solvent absorbed by the phenolic resin binder in the filter element per unit weight is used to represent the expansion degree. In the radial section of the filter element:

[0404] The first area is 0-25% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 2.1 mL / kg;

[0405] The second area is 25-50% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 2.6 mL / kg;

[0406] The third area is 50-75% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 2.4 mL / kg;

[0407] The fourth area is 75-100% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 2.7 mL / kg;

[0408] The standard deviation of the swelling degree of each region is 0.23 mL / kg, and the ratio between the standard deviation of the swelling degree of the first region and the average swelling degree is 0.11, the ratio between the standard deviation of the swelling degree of the second region and the average swelling degree is 0.09, the ratio between the standard deviation of the swelling degree of the third region and the average swelling degree is 0.1, and the ratio between the standard deviation of the swelling degree of the fourth region and the average swelling degree is 0.08;

[0409] The phenolic resin binder in the filter element accounts for 25%; the interception rate for particles with a particle size of 10 μm is 95%; the flow rate is 5.5 kPa;

[0410] A method for preparing a resin-bonded and cured filter element comprises the following steps:

[0411] S1: Material selection: Select fiber with a diameter of 15-25μm, a thickness of 1mm, and a weight of 100g / m 2 PET resin fiber non-woven fabric;

[0412] S2: Winding: Prepare a phenolic resin binder solution with a concentration of 300wt%, spray the phenolic resin binder solution on the surface of the non-woven fabric, the spraying amount is 50% of the gram weight, and then wind it under a tension of 10N to obtain a wound filter element;

[0413] S3: Immersing: Immersing the wound filter element in a phenolic resin binder solution at 25° C. for 50 minutes to obtain a primary filter element;

[0414] S4: Debonding: Use compressed gas for multi-stage flushing. The compressed gas passes through the filter element, and the wind pressure decreases gradually to remove excess binder solution:

[0415] S41: The compressed gas pressure is 120 kPa and the flushing time is 10 s;

[0416] S42: The wind pressure of the compressed gas is 60kpa, and the flushing time is 30s;

[0417] S43: The wind pressure of the compressed gas is 20kpa, and the flushing time is 50s;

[0418] S5: Curing: Use gas to circulate and cure the debonded filter element. The curing is a multi-stage curing. During the curing, the gas passes through the filter element, and the pressure and temperature increase gradually to prepare a resin-bonded cured filter element.

[0419] S51: pressure 11kpa; curing temperature 110℃;

[0420] S52: pressure 12kpa; curing temperature 155℃;

[0421] S53: pressure 27kpa; curing temperature 205℃.

[0422] Embodiment 17:

[0423] A resin bonded solidified filter element, the filter element comprising PET resin fibers, having a permeable liquid inlet surface and a liquid outlet surface away from the liquid inlet surface and also permeable, and forming an axial hollow flow channel; wherein the outer diameter of the filter element is 64 mm, the diameter of the axial hollow flow channel is 28 mm, the radial distance h2 between the liquid inlet surface and the liquid outlet surface is 18 mm, and the length of the filter element is 254 mm;

[0424] The PET resin fiber is coated with a phenolic resin binder to form a skin-core structure, and the phenolic resin binder is cured and bonded;

[0425] The filter element is immersed in the organic solvent ethanol, and the volume of the organic solvent absorbed by the phenolic resin binder in the filter element per unit weight is used to represent the expansion degree. In the radial section of the filter element:

[0426] The first area is 0-25% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 12.5 mL / kg;

[0427] The second area is 25-50% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 16.7 mL / kg;

[0428] The third area is 50-75% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 10.4 mL / kg;

[0429] The fourth area is 75-100% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 25.6 mL / kg;

[0430] The standard deviation of the swelling degree of each region is 5.83 mL / kg, and the ratio between the standard deviation of the swelling degree and the average swelling degree of the first region is 0.47, the ratio between the standard deviation of the swelling degree and the average swelling degree of the second region is 0.35, the ratio between the standard deviation of the swelling degree and the average swelling degree of the third region is 0.56, and the ratio between the standard deviation of the swelling degree and the average swelling degree of the fourth region is 0.23;

[0431] The phenolic resin binder in the filter element accounts for 55%; the interception rate for particles with a particle size of 10 μm is 99%; the flow rate is 7.5 kPa;

[0432] A method for preparing a resin-bonded and cured filter element comprises the following steps:

[0433] S1: Material selection: Select fiber with a diameter of 15-25μm, a thickness of 1mm, and a weight of 100g / m 2 PET resin fiber non-woven fabric;

[0434] S2: Winding: Prepare a phenolic resin binder solution with a concentration of 300wt%, spray the phenolic resin binder solution on the surface of the non-woven fabric, the spraying amount is 50% of the gram weight, and then wind it under a tension of 10N to obtain a wound filter element;

[0435] S3: Immersing: Immersing the wound filter element in a phenolic resin binder solution at 25° C. for 50 minutes to obtain a primary filter element;

[0436] S4: Debonding: Use compressed gas for multi-stage flushing. The compressed gas passes through the filter element, and the wind pressure decreases gradually to remove excess binder solution:

[0437] S41: The compressed gas pressure is 68kpa and the flushing time is 3s;

[0438] S42: The compressed gas pressure is 25 kPa and the flushing time is 15 s;

[0439] S43: The wind pressure of the compressed gas is 6 kPa, and the flushing time is 27 seconds;

[0440] S5: Curing: Use gas to circulate and cure the debonded filter element. The curing is a multi-stage curing. During the curing, the gas passes through the filter element, and the pressure and temperature increase gradually to prepare a resin-bonded cured filter element.

[0441] S51: pressure 3kpa; curing temperature 80℃;

[0442] S52: pressure 5kpa; curing temperature 130℃;

[0443] S53: pressure 10kpa; curing temperature 170℃.

[0444] Comparative Example 1:

[0445] A resin bonded solidified filter element, the filter element comprising PET resin fibers, having a permeable liquid inlet surface and a liquid outlet surface away from the liquid inlet surface and also permeable, and forming an axial hollow flow channel; wherein the outer diameter of the filter element is 64 mm, the diameter of the axial hollow flow channel is 28 mm, the radial distance h2 between the liquid inlet surface and the liquid outlet surface is 18 mm, and the length of the filter element is 254 mm;

[0446] The PET resin fiber is coated with a phenolic resin binder to form a skin-core structure, and the phenolic resin binder is cured and bonded;

[0447] The filter element is immersed in the organic solvent ethanol, and the volume of the organic solvent absorbed by the phenolic resin binder in the filter element per unit weight is used to represent the expansion degree. In the radial section of the filter element:

[0448] The first area is 0-25% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 75.6 mL / kg;

[0449] The second area is 25-50% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 33.4 mL / kg;

[0450] The third area is 50-75% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 12.2 mL / kg;

[0451] The fourth area is 75-100% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 9.3 mL / kg;

[0452] The standard deviation of the swelling degree of each region is 26.5 mL / kg, and the ratio between the standard deviation of the swelling degree and the average swelling degree of the first region is 0.35, the ratio between the standard deviation of the swelling degree and the average swelling degree of the second region is 0.8, the ratio between the standard deviation of the swelling degree and the average swelling degree of the third region is 2.17, and the ratio between the standard deviation of the swelling degree and the average swelling degree of the fourth region is 2.85;

[0453] The phenolic resin binder in the filter element accounts for 55%; the interception rate for particles with a particle size of 10 μm is 99%; the flow rate is 7.5 kPa;

[0454] A method for preparing a resin-bonded and cured filter element comprises the following steps:

[0455] S1: Material selection: Select fiber with a diameter of 15-25μm, a thickness of 1mm, and a weight of 100g / m 2 PET resin fiber non-woven fabric;

[0456] S2: Winding: Prepare a phenolic resin binder solution with a concentration of 300wt%, spray the phenolic resin binder solution on the surface of the non-woven fabric, the spraying amount is 50% of the gram weight, and then wind it under a tension of 10N to obtain a wound filter element;

[0457] S3: Immersing: Immersing the wound filter element in a phenolic resin binder solution at 25° C. for 50 minutes to obtain a primary filter element;

[0458] S4: Debonding: Use compressed gas for multi-stage flushing. The compressed gas passes through the filter element, and the wind pressure decreases gradually to remove excess binder solution:

[0459] S41: The compressed gas pressure is 68kpa and the flushing time is 3s;

[0460] S42: The compressed gas pressure is 25 kPa and the flushing time is 15 s;

[0461] S43: The wind pressure of the compressed gas is 6 kPa, and the flushing time is 27 seconds;

[0462] S5: Curing: Use an oven at 205°C until the curing is complete.

[0463] Comparative Example 2:

[0464] A resin bonded solidified filter element, the filter element comprising PET resin fibers, having a permeable liquid inlet surface and a liquid outlet surface away from the liquid inlet surface and also permeable, and forming an axial hollow flow channel; wherein the outer diameter of the filter element is 64 mm, the diameter of the axial hollow flow channel is 28 mm, the radial distance h2 between the liquid inlet surface and the liquid outlet surface is 18 mm, and the length of the filter element is 254 mm;

[0465] The PET resin fiber is coated with a phenolic resin binder to form a skin-core structure, and the phenolic resin binder is cured and bonded;

[0466] The filter element is immersed in the organic solvent ethanol, and the volume of the organic solvent absorbed by the phenolic resin binder in the filter element per unit weight is used to represent the expansion degree. In the radial section of the filter element:

[0467] The first area is 0-25% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 85.3 mL / kg;

[0468] The second area is 25-50% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 43.6 mL / kg;

[0469] The third area is 50-75% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 21.1 mL / kg;

[0470] The fourth area is 75-100% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 10.8 mL / kg;

[0471] The standard deviation of the swelling degree of each region is 28.61 mL / kg, and the ratio between the standard deviation of the swelling degree and the average swelling degree of the first region is 0.34, the ratio between the standard deviation of the swelling degree and the average swelling degree of the second region is 0.66, the ratio between the standard deviation of the swelling degree and the average swelling degree of the third region is 1.36, and the ratio between the standard deviation of the swelling degree and the average swelling degree of the fourth region is 2.65;

[0472] The phenolic resin binder in the filter element accounts for 55%; the interception rate for particles with a particle size of 10 μm is 99%; the flow rate is 7.3 kPa;

[0473] A method for preparing a resin-bonded and cured filter element comprises the following steps:

[0474] S1: Material selection: Select fiber with a diameter of 15-25μm, a thickness of 1mm, and a weight of 100g / m 2 PET resin fiber non-woven fabric;

[0475] S2: Winding: Prepare a phenolic resin binder solution with a concentration of 300wt%, spray the phenolic resin binder solution on the surface of the non-woven fabric, the spraying amount is 50% of the gram weight, and then wind it under a tension of 10N to obtain a wound filter element;

[0476] S3: Immersing: Immersing the wound filter element in a phenolic resin binder solution at 25° C. for 50 minutes to obtain a primary filter element;

[0477] S4: Debonding: Use compressed gas for multi-stage flushing. The compressed gas passes through the filter element, and the wind pressure decreases gradually to remove excess binder solution:

[0478] S41: The compressed gas pressure is 68kpa and the flushing time is 3s;

[0479] S42: The compressed gas pressure is 25 kPa and the flushing time is 15 s;

[0480] S43: The wind pressure of the compressed gas is 6 kPa, and the flushing time is 27 seconds;

[0481] S5: Curing: Use an oven at 205°C until the curing is complete.

[0482] Comparative Example 3:

[0483] A resin bonded solidified filter element, the filter element comprising PET resin fibers, having a permeable liquid inlet surface and a liquid outlet surface away from the liquid inlet surface and also permeable, and forming an axial hollow flow channel; wherein the outer diameter of the filter element is 64 mm, the diameter of the axial hollow flow channel is 28 mm, the radial distance h2 between the liquid inlet surface and the liquid outlet surface is 18 mm, and the length of the filter element is 254 mm;

[0484] The PET resin fiber is coated with a phenolic resin binder to form a skin-core structure, and the phenolic resin binder is cured and bonded;

[0485] The filter element is immersed in the organic solvent ethanol, and the volume of the organic solvent absorbed by the phenolic resin binder in the filter element per unit weight is used to represent the expansion degree. In the radial section of the filter element:

[0486] The first area is 0-25% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 108.6 mL / kg;

[0487] The second area is 25-50% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 53.8 mL / kg;

[0488] The third area is 50-75% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 25.4 mL / kg;

[0489] The fourth area is 75-100% of the filter element thickness from the liquid inlet side, and the average expansion degree of the filter element in this area is 11.5 mL / kg;

[0490] The standard deviation of the swelling degree of each region is 37.2 mL / kg, and the ratio between the standard deviation of the swelling degree and the average swelling degree of the first region is 0.34, the ratio between the standard deviation of the swelling degree and the average swelling degree of the second region is 0.69, the ratio between the standard deviation of the swelling degree and the average swelling degree of the third region is 1.46, and the ratio between the standard deviation of the swelling degree and the average swelling degree of the fourth region is 3.23;

[0491] The phenolic resin binder in the filter element accounts for 55%; the interception rate for particles with a particle size of 10 μm is 99%; the flow rate is 7.3 kPa;

[0492] A method for preparing a resin-bonded and cured filter element comprises the following steps:

[0493] S1: Material selection: Select fiber with a diameter of 15-25μm, a thickness of 1mm, and a weight of 100g / m 2 PET resin fiber non-woven fabric;

[0494] S2: Winding: Prepare a phenolic resin binder solution with a concentration of 300wt%, spray the phenolic resin binder solution on the surface of the non-woven fabric, the spraying amount is 50% of the gram weight, and then wind it under a tension of 10N to obtain a wound filter element;

[0495] S3: Immersing: Immersing the wound filter element in a phenolic resin binder solution at 25° C. for 50 minutes to obtain a primary filter element;

[0496] S4: Debonding: Use compressed gas for multi-stage flushing. The compressed gas passes through the filter element, and the wind pressure decreases gradually to remove excess binder solution:

[0497] S41: The compressed gas pressure is 68kpa and the flushing time is 3s;

[0498] S42: The compressed gas pressure is 25 kPa and the flushing time is 15 s;

[0499] S43: The wind pressure of the compressed gas is 6 kPa, and the flushing time is 27 seconds;

[0500] S5: Curing: Use an oven at 205°C until the curing is complete.

[0501] The filter elements prepared in Examples 1-5, 17 and Comparative Examples 1-3 were immersed in ethanol at 50°C for 24 hours, and then the interception rates of the filter elements after immersion were measured. The results are shown in the following table.

[0502]

[0503] It can be seen from the above-mentioned Examples 1-15 that the filter element prepared by the present invention has a relatively uniform expansion degree in each area of ​​the cross section and a high degree of curing. Therefore, when applied to organic coating filtration, small molecules dissolve less, and when the filter element is immersed in ethanol and then water is used as the medium to measure the interception rate, the interception rate decrease rate is low, indicating that the resin fiber of the filter element still has good adhesion. Compared with Example 1, Example 16 uses compressed gas for multi-stage flushing and degumming, and the flushing pressure is too high and the time is too long, resulting in too little binder solution coated on the resin fiber, and no good skin-core structure is formed after curing. Therefore, the expansion degree of each area is relatively low. When the interception rate is tested by the same method as Example 1, the interception rate decreases under water pressure due to the low adhesion between the resin fibers. Compared with Example 1, Example 17 uses gas for circulation curing. The gas pressure is low, so the curing uniformity of each area is poorer than that of Example 1. At the same time, due to the low curing temperature, the degree of curing is insufficient, and the expansion degree of each area is high. When the interception rate is tested with a water medium after ethanol immersion, the interception rate decreases. The difference between Comparative Examples 1-3 and Example 1 is that the degummed filter element primary product is not circulated and cured by gas, but is directly dried and cured in an oven. Although the fourth area is relatively completely cured, the overall degree of curing of the filter element is low, especially the inside of the filter element is not completely cured, resulting in a large difference in the expansion degree of each area. During the filtration of organic coatings, small molecules are easily dissolved. When the interception rate is tested with a water medium after ethanol immersion, the interception rate decreases significantly, indicating that the bonding force between the resin fibers in the filter element decreases after ethanol immersion, and the filter element cannot withstand the pressure during the interception rate test.

[0504] The preferred embodiments of the present invention have been described in detail above, but it should be understood that after reading the above teachings of the present invention, those skilled in the art may make various changes or modifications to the present invention. These equivalent forms also fall within the scope defined by the claims attached to this application.

Claims

1. A resin bonded cured filter element, the filter element comprising resin fibers, having a permeable liquid inlet surface and a liquid outlet surface remote from the liquid inlet surface and also permeable, and forming an axial hollow flow channel; Features: The resin fiber is coated with a binder to form a skin-core structure, and the binder is cured and bonded; The filter element is immersed in an organic solvent, and the volume of the organic solvent absorbed by the binder in the filter element per unit weight is used to represent the expansion degree. In the radial section of the filter element: The first area is 0-25% of the filter element thickness from the liquid inlet side. The second area is 25-50% of the filter element thickness from the liquid inlet side. The third area is 50-75% of the filter element thickness from the liquid inlet side. The fourth area is 75-100% of the filter element thickness from the liquid inlet side. The ratio between the standard deviation of the expansion degree and the average expansion degree of each region is 0.01-0.

5.

2. The resin bonded cured filter element according to claim 1, It is characterized in that After the filter element is fully impregnated with the organic solvent, the interception rate of particles with a particle size of 10 μm is reduced by 0.1-1%.

3. The resin bonded cured filter element according to claim 1, It is characterized in that The filter element has an interception rate of 99% for particles with a particle size of 10 μm.

4. The resin bonded cured filter element according to claim 1, It is characterized in that The binder accounts for 20-70% of the overall mass of the filter element.

5. The resin bonded cured filter element according to claim 1, It is characterized in that The standard deviation of the expansion degree of each area in the radial cross section of the filter element is 0.1-1.5 mL / kg; the average expansion degree of the filter element is 1-10 mL / kg.

6. The resin bonded cured filter element according to claim 1, It is characterized in that The resin fiber has a diameter of 1-100 μm.

7. The resin bonded cured filter element according to claim 1, It is characterized in that The filter element is obtained by winding at least one non-woven fabric, and the non-woven fabric contains resin fibers.

8. The resin bonded cured filter element according to claim 7, It is characterized in that The thickness of the non-woven fabric is h1, the radial distance between the liquid inlet surface and the liquid outlet surface is h2, h1:h2 is 1:10-25; and / or, h2=(1.1-1.5)*n*h1, wherein n is the number of winding layers of the non-woven fabric.

9. The resin bonded cured filter element according to claim 1, It is characterized in that The resin fiber includes a mixture of one or more of polyester fiber, nylon fiber, polypropylene fiber, cellulose fiber and acrylonitrile fiber.

10. The resin bonded cured filter element according to claim 1, It is characterized in that The binder includes a phenolic resin.

11. The resin bonded cured filter element according to claim 1, It is characterized in that The organic solvent includes one or more of ethanol, acetone, butanone, ethyl acetate and xylene.

12. A method for preparing a resin bonded and cured filter element according to any one of claims 1 to 11, It is characterized in that The method comprises the following preparation steps: S1: Material selection: select resin fiber non-woven fabric; S2: Winding: Winding the non-woven fabric to obtain a wound filter element; S3: Impregnation: prepare a binder solution, and immerse the wound filter element in the binder solution to obtain a primary filter element; S4: Debonding: removing excess binder solution; S5: Curing: Use gas to circulate and cure the debonded filter element to prepare a resin-bonded and cured filter element.

13. The method for preparing the resin-bonded and cured filter element according to claim 12, It is characterized in that In step S2, a binder solution is sprayed on the surface of the non-woven fabric during winding, and the spraying amount is 20-70% of the gram weight.

14. The method for preparing the resin-bonded and cured filter element according to claim 12, It is characterized in that The winding tension in step S2 is 3-20N.

15. The method for preparing the resin-bonded and cured filter element according to claim 12 or 13, It is characterized in that The concentration of the binder solution in step S3 is 50-500 wt %.

16. The method for preparing the resin-bonded and cured filter element according to claim 12, It is characterized in that The immersion in step S3 is carried out at 15-30° C. for 5-60 min.

17. The method for preparing the resin-bonded and cured filter element according to claim 12, It is characterized in that The degumming in step S4 is a multi-stage flushing with compressed gas, the compressed gas passes through the filter element, and the wind pressure decreases: S41: The wind pressure of compressed gas is 50-100kpa, and the flushing time is 2-5s; S42: The wind pressure of compressed gas is 10-50kpa, and the flushing time is 5-20s; S43: The wind pressure of compressed gas is 2-15kpa, and the flushing time is 15-40s.

18. The method for preparing the resin-bonded and cured filter element according to claim 12, It is characterized in that The degumming in step S4 is centrifugal degumming, and the centrifugal speed is 1500-3000r / min.

19. The method for preparing the resin-bonded and cured filter element according to claim 12, It is characterized in that The curing in step S5 is a multi-stage curing, during which the gas passes through the filter element and the pressure and temperature increase gradually: S51: pressure 2-50kpa; curing temperature 100-120℃; S52: pressure 2-50kpa; curing temperature 150-170℃; S53: pressure 5-100kpa; curing temperature 190-210℃.

20. Use of the resin bonded cured filter element as claimed in any one of claims 1 to 11 in coating filtration.

Citation Information

Patent Citations

  • Air filtration material and application thereof

    CN102794051A

  • Filter element and preparation method and application thereof

    CN104606802A