Preparation method of SGT-MOSFET semiconductor device
By forming an increasingly dense film layer structure on the sidewalls and bottom of the deep trench of the SGT-MOSFET device, and using ion implantation and barrier layer etching technology, the problems of limited BV improvement and complicated preparation processes in the existing technology are solved. Improvement of device performance and optimization of preparation efficiency are achieved.
Patent Information
- Application Number
- CN202011302582.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-11-19
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2040-11-19
AI Technical Summary
Existing SGT-MOSFET devices have limitations in increasing the breakdown voltage (BV), and the EPI concentration gradient is easily weakened in high-temperature processes, affecting device performance, and the preparation process is complex and time-consuming.
By forming an increasingly dense film structure on the sidewalls and bottom of the deep trench, using an ion implantation process to form a covering layer, and using the barrier layer as a mask to remove part of the sacrificial layer, the thickness and surface shape of the sidewalls of the deep trench are adjusted. Optimize the vertical exhaustion effect to improve BV.
It achieves an increase in BV of SGT-MOSFET devices, simplifies the preparation process, reduces R&D time and silicon wafer usage, and improves the voltage resistance and performance of the device.
Smart Images

Figure CN114520147B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of power semiconductors, and more specifically, to a method for preparing a SGT-MOSFET semiconductor device. Background Art
[0002] SGT-MOSFET is a new type of power semiconductor device, which has the advantages of low conduction loss of traditional deep trench MOSFET and lower switching loss. As a switching device, SGT-MOSFET is used in motor drive systems, inverter systems and power management systems in the fields of new energy electric vehicles, new photovoltaic power generation, energy-saving home appliances, etc. It is a core power control component.
[0003] SGT-MOSFET is a MOSFET with a deep trench longitudinal structure. The depletion electric field of an ordinary power MOSFET is a triangle, while the depletion electric field of the shielding gate region of the deep trench of SGT-MOSFET is approximately rectangular, so SGT-MOSFET has better device withstand voltage. The shielding gate between adjacent deep trenches of the SGT-MOSFET of the prior art can play a role of lateral depletion, and the charge coupling effect causes the peak value of the electric field in the bottom area of the deep trench to be pulled up, and the projection area of the electric field along the depth increases. Under the condition of achieving the same BV, a lower resistivity EPI (Epitaxy, referred to as EPI) is used to achieve a reduction in Rdson (on-state resistance). Since the shielding gate is formed by doped polysilicon, there is a voltage drop when the current passes through the shielding gate, and the potential decreases from deep to shallow along the depth of the deep trench. Although the electric field strength at the bottom of the deep trench can be pulled up, the entire electric field distribution cannot be completely flattened, thereby limiting the improvement of the BV of the SGT-MOSFET device.
[0004] At present, the problem can be compensated by adjusting the EPI concentration along the depth of the deep trench, but the disadvantages are: first, it requires professional EPI equipment manufacturers to complete it through multiple batches, and each batch of silicon wafers must have at least one piece of silicon wafer and multiple attempts, which takes a long time to develop and use a large number of silicon wafers; second, the high temperature in the EPI process weakens the EPI concentration gradient, and the temperature and time of the high-temperature process in the later SGT-MOSFET device process will affect the diffusion rate from high concentration to low concentration in the EPI and the final concentration distribution, thereby affecting the BV improvement effect. Summary of the invention
[0005] The purpose of the present invention is to overcome the above-mentioned defects in the prior art and provide a method for preparing a SGT-MOSFET semiconductor device.
[0006] To achieve the above object, the present invention provides a method for preparing a SGT-MOSFET semiconductor device, which is characterized by comprising:
[0007] Providing a semiconductor substrate having a deep trench;
[0008] forming an initial first sacrificial layer on the semiconductor substrate, wherein the initial first sacrificial layer also covers the sidewalls and the bottom of the deep trench;
[0009] Performing ion implantation on the initial first sacrificial layer by an implantation process to form a first sacrificial layer covering the sidewalls and bottom of the deep trench and a second sacrificial layer located on the first sacrificial layer on the semiconductor substrate;
[0010] forming a third sacrificial layer on the second sacrificial layer;
[0011] forming a barrier layer filling the deep trench;
[0012] Using the barrier layer as a mask, removing the second sacrificial layer, the third sacrificial layer, and a portion of the first sacrificial layer located on the sidewall of the deep trench, wherein the thickness of the remaining first sacrificial layer located on the sidewall of the deep trench gradually increases along the sidewall of the deep trench toward the bottom of the deep trench;
[0013] The barrier layer is removed.
[0014] Preferably, the angle between the sidewall and the bottom of the deep trench is 86.5° to 89.5°.
[0015] Preferably, the semiconductor substrate is a silicon substrate, the material of the initial first sacrificial layer is silicon oxide, the formation process of the first sacrificial layer includes a thermal oxidation method, and the thickness of the initial first sacrificial layer is 2000 angstroms to 8000 angstroms.
[0016] Preferably, the ions implanted are argon ions, the implantation energy of the implantation process is 30KeV to 100KeV, the implantation depth of the ion implantation is 300 angstroms to 500 angstroms, the thickness of the second sacrificial layer is 300 angstroms to 500 angstroms, and the density of the second sacrificial layer is lower than the density of the first sacrificial layer.
[0017] Preferably, the density of the third sacrificial layer is lower than that of the second sacrificial layer, the thickness of the third sacrificial layer is 200 angstroms to 800 angstroms, and the formation process of the third sacrificial layer includes chemical vapor deposition.
[0018] Preferably, the barrier layer comprises one of a photoresist layer and a BARC layer, and a height of the barrier layer is lower than or equal to a surface of a third sacrificial layer located on the semiconductor substrate.
[0019] Preferably, an isotropic etching process is used to remove the second sacrificial layer, the third sacrificial layer, and a portion of the first sacrificial layer located on the sidewall of the deep trench; the isotropic etching process includes one or a combination of an isotropic wet etching process or an isotropic dry etching process; the etching removal rate of the third sacrificial layer is greater than the etching removal rate of the second sacrificial layer; the etching removal rate of the second sacrificial layer is greater than the etching removal rate of the first sacrificial layer.
[0020] Preferably, the implantation process is a single continuous ion implantation process, and the remaining first sacrificial layer located on the sidewall of the deep trench has an inclined surface intersecting the sidewall of the deep trench at an acute angle, and the inclined surface is a continuous and smooth surface.
[0021] Preferably, the remaining first sacrificial layer located on the sidewall of the deep trench also has a vertical surface parallel to the sidewall of the deep trench, and the first sacrificial layer with the inclined surface is connected to the first sacrificial layer located at the bottom of the deep trench through the first sacrificial layer with the vertical surface.
[0022] Preferably, the implantation process is a single step ion implantation process, the implantation energy of which is reduced stepwise, and the remaining first sacrificial layer located on the sidewall of the deep trench has a step surface that gradually decreases along the sidewall of the deep trench toward the bottom of the deep trench.
[0023] It can be seen from the above technical scheme that the present invention provides a method for preparing an SGT-MOSFET semiconductor device, by ion implanting the initial first sacrificial layer on the sidewall of the deep trench, thereby forming a first sacrificial layer covering the sidewall and bottom of the deep trench and a second sacrificial layer located on the first sacrificial layer on the semiconductor substrate, the second sacrificial layer having a lower density than the first sacrificial layer; forming a third sacrificial layer on the second sacrificial layer, the third sacrificial layer having a lower density than the second sacrificial layer, thereby forming a film layer structure with a density increasing from the outside to the inside on the sidewall of the deep trench, by filling a barrier layer in the deep trench, and then using the barrier layer as a mask to remove the second sacrificial layer, the third sacrificial layer, and part of the first sacrificial layer located on the sidewall of the deep trench, the thickness of the remaining first sacrificial layer located on the sidewall of the deep trench gradually increases along the sidewall of the deep trench toward the bottom of the deep trench, and the surface shape of the remaining first sacrificial layer located on the sidewall of the deep trench can be adjusted by the implantation process, thereby adjusting the SGT longitudinal depletion, and then optimizing the BV improvement, which has significant significance. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0025] Figures 1 to 7 A schematic diagram of the process steps of a method for preparing a SGT-MOSFET semiconductor device according to an embodiment of the present invention is shown. DETAILED DESCRIPTION
[0026] To make the content of the present invention more clear and understandable, the content of the present invention is further described below in conjunction with the accompanying drawings of the specification. Of course, the present invention is not limited to this specific embodiment, and general replacements known to those skilled in the art are also covered within the protection scope of the present invention.
[0027] It should be noted that in the following specific embodiments, when describing the embodiments of the present invention in detail, in order to clearly represent the structure of the present invention for the convenience of explanation, the structures in the accompanying drawings are not drawn according to general proportions, and are partially enlarged, deformed and simplified. Therefore, it should be avoided to understand this as a limitation of the present invention.
[0028] In order to make the purpose, technical solutions and advantages of the present invention more clear, the specific embodiments of the present invention are further described in detail below with reference to the accompanying drawings. Figures 1 to 7 A schematic diagram of the process steps of a method for preparing a SGT-MOSFET semiconductor device according to an embodiment of the present invention is shown.
[0029] like Figure 1 As shown, a semiconductor substrate 100 is provided, wherein the semiconductor substrate 100 has a deep trench 101 .
[0030] The provided semiconductor substrate 100 may be a Si substrate, a Ge substrate, a SiGe substrate, a SiC substrate, a SOI (Silicon On Insulator) substrate or a GOI (Germanium On Insulator) substrate, etc. It may also be a substrate including other element semiconductors or compound semiconductors, such as a glass substrate or a III-V compound substrate (such as a gallium nitride substrate or a gallium arsenide substrate, etc.), and may also be a stacked structure, such as Si / SiGe, etc., and may also be other epitaxial structures, such as SGOI (Silicon Germanium On Insulator), etc. In one embodiment, the semiconductor substrate 100 is a silicon substrate, an epitaxial layer is deposited on the silicon substrate, and then the epitaxial layer is patterned to form a deep trench 101 in the epitaxial layer. In the present embodiment, the semiconductor substrate 100 is a silicon substrate, and a patterned photoresist layer is formed on the semiconductor substrate 100 by a photolithography process, and the patterned photoresist layer defines the position and shape of the deep trench 101. The patterned photoresist layer is used as a mask to etch the semiconductor substrate 100, and a plurality of deep trenches 101 are formed in the semiconductor substrate 100. Then, the patterned photoresist layer is removed, and the angle between the sidewall and the bottom of the deep trench 101 is 86.5° to 89.5°. In the present embodiment, after the deep trench 101 is formed, the corners of the bottom of the deep trench 101 are rounded to form a U-shaped deep trench 101. The cross-sectional shape of the deep trench 101 also includes one of the group consisting of a rectangle and a square, or two or more of a rectangle, a square, a positive "V" shape, and a reverse "V" shape. Since the process is known in the art, the details are not repeated here.
[0031] like Figure 2 As shown, an initial first sacrificial layer 110 is formed on the semiconductor substrate 100 , and the initial first sacrificial layer 110 also covers the sidewalls and the bottom of the deep trench 101 .
[0032] After standard surface cleaning, an initial first sacrificial layer 110 is formed on the semiconductor substrate 100 by using techniques known in the art, including but not limited to physical deposition, chemical deposition such as low pressure chemical vapor deposition (LPCVD), plasma deposition such as plasma enhanced chemical vapor deposition (PECVD), combined deposition of physical and chemical deposition, pulsed laser deposition, thermal evaporation, electron beam evaporation, sputtering deposition such as DC sputtering and RF sputtering, atomic alignment, wet oxidation, dry oxidation, chemical solution oxidation and other well-known techniques to form the initial first sacrificial layer 110. In this embodiment, the formation process of the initial first sacrificial layer 110 is thermal oxidation, the semiconductor substrate 100 is a silicon substrate, the initial first sacrificial layer 110 is formed on the semiconductor substrate 100 by thermal oxidation, the material of the initial first sacrificial layer 110 is silicon oxide, a dense layer of silicon oxide is formed on the sidewall and bottom of the deep trench 101 by thermal oxidation, and the thickness of the initial first sacrificial layer 110 is 2000 angstroms to 8000 angstroms.
[0033] like Figure 3 As shown, the initial first sacrificial layer 110 is ion implanted by an implantation process to form a first sacrificial layer (not shown) covering the sidewall and bottom of the deep trench 101 and a second sacrificial layer (not shown) located on the first sacrificial layer on the semiconductor substrate 100.
[0034] The implantation process includes one of a single continuous ion implantation process or a single step ion implantation process, and the implantation energy of the single step ion implantation process is reduced stepwise. In this embodiment, an ion implantation process is used to implant argon ions into the initial first sacrificial layer 110, the ions implanted are argon ions, the implantation energy of the implantation process is 30KeV-100KeV, the implantation depth of the ion implantation is 300 angstroms-500 angstroms, the thickness of the second sacrificial layer is 300 angstroms-500 angstroms, and the density of the second sacrificial layer is lower than the density of the first sacrificial layer. In this embodiment, argon ions are implanted into dense silicon oxide, and the second sacrificial layer is a silicon oxide layer doped with argon ions, and the density of the silicon oxide layer doped with argon ions is lower than that of the undoped first sacrificial layer, thereby forming a silicon oxide layer whose density gradually increases from the surface to the bottom surface. When the first sacrificial layer of the side wall of the deep trench 101 is subsequently etched, the angle between the surface of the first sacrificial layer and the side wall of the deep trench 101 can be adjusted by the implantation energy and implantation angle of the implantation process. The implantation process is a single continuous ion implantation process, the surface density of the second sacrificial layer gradually increases toward the bottom surface, and the remaining first sacrificial layer located on the sidewall of the deep trench subsequently has an inclined surface intersecting the sidewall of the deep trench at an acute angle, and the inclined surface is a continuous and smooth surface; the implantation process is a single step ion implantation process, and the implantation energy of the single step ion implantation process is reduced stepwise, and the surface density of the second sacrificial layer increases stepwise toward the bottom surface. In another embodiment, the implantation process only performs ion implantation on the initial first sacrificial layer 110 on the sidewall and bottom of the deep trench 101.
[0035] like Figure 4 As shown, a third sacrificial layer 121 is formed on the second sacrificial layer 120 .
[0036] The thickness of the third sacrificial layer 121 is 200 angstroms to 800 angstroms. The formation process of the third sacrificial layer 121 includes chemical vapor deposition. The third sacrificial layer 121 is also located on the sidewall and bottom of the deep trench 101. The density of the third sacrificial layer 121 is lower than that of the second sacrificial layer 120. In one embodiment, the third sacrificial layer 121 is the silicon oxide layer formed by the HDPCVD method. The silicon oxide layer deposited by the HDPCVD method covers the surface of the second sacrificial layer 120, which can make the surface of the second sacrificial layer 120 formed by thermal oxidation and doping more flat, and the corner transition of the second sacrificial layer 120 located at the bottom of the deep trench 101 is smoother.
[0037] like Figure 5 As shown, a barrier layer 130 is formed to fill the deep trench 101 (not shown).
[0038] The barrier layer 130 includes one of a photoresist layer or a BARC layer. In the present embodiment, the barrier layer 130 is a photoresist layer, and the photoresist layer filling the deep trench 101 is coated on the semiconductor substrate 100, and then the photoresist layer is patterned by a photolithography process and a development process. In another embodiment, the barrier layer 130 is a BARC layer, and the BARC layer filling the deep trench 101 is coated on the semiconductor substrate 100, and then the BARC layer is patterned by a photolithography process and a dry etching process to form the barrier layer 130 filling the deep trench 101. The surface of the barrier layer 130 is lower than or flush with the surface of the third sacrificial layer 121 located on the semiconductor substrate 110. In this embodiment, the surface of the blocking layer 130 is flush with the surface of the third sacrificial layer 121 located on the semiconductor substrate 110. The surface position of the blocking layer 130 affects the subsequent etching time of the first sacrificial layer 111 of the side wall of the deep trench 101, thereby affecting the shape of the remaining first sacrificial layer 111 on the side wall of the deep trench 101.
[0039] like Figure 6 As shown, using the blocking layer 130 as a mask, the second sacrificial layer (not shown), the third sacrificial layer (not shown), and a portion of the first sacrificial layer 111 located on the sidewall of the deep trench (not shown) are removed, and the thickness of the remaining first sacrificial layer 111 located on the sidewall of the deep trench gradually increases along the sidewall of the deep trench toward the bottom of the deep trench.
[0040] The second sacrificial layer, the third sacrificial layer, and a portion of the first sacrificial layer 111 located on the sidewall of the deep trench are removed by an isotropic etching process; the isotropic etching process includes one or a combination of isotropic wet etching or isotropic dry etching processes; by ion implantation of the initial first sacrificial layer, a film structure is achieved in which the density gradually increases from the third sacrificial layer to the second sacrificial layer and then to the first sacrificial layer, and the etching removal rate of the third sacrificial layer is greater than the etching removal rate of the second sacrificial layer; the etching removal rate of the second sacrificial layer is greater than the etching removal rate of the first sacrificial layer. Moreover, with the barrier layer 130 as a mask, the etching process etches the second sacrificial layer, the third sacrificial layer, and the first sacrificial layer downward along the sidewall of the deep trench, and as the etching depth increases, the etching rate decreases, and finally the thickness of the remaining first sacrificial layer 111 located on the sidewall of the deep trench gradually increases along the sidewall of the deep trench to the bottom of the deep trench. In this embodiment, the etching process also removes the first sacrificial layer 111 and the second sacrificial layer 120 located on the semiconductor substrate 100. The implantation process is a single continuous ion implantation process, the density of the surface of the second sacrificial layer gradually increases toward the bottom surface, the remaining first sacrificial layer 111 located on the sidewall of the deep trench has an inclined surface intersecting the sidewall of the deep trench at an acute angle, the remaining first sacrificial layer 111 after etching has an inclined surface, and the inclined surface is a continuous and smooth surface, and the film thickness of the remaining first sacrificial layer 111 located on the sidewall of the deep trench 101 shows a trend of gradually thickening from the upper part of the sidewall of the deep trench 101 to the bottom of the deep trench 101. By adjusting the implantation energy of the single continuous ion implantation process, the inclination slope of the surface of the remaining first sacrificial layer 111 on the sidewall of the deep trench 101 can be adjusted, thereby adjusting the longitudinal depletion of SGT, and further optimizing the BV improvement. In one embodiment, the remaining first sacrificial layer 111 located on the sidewall of the deep trench also has a vertical surface parallel to the sidewall of the deep trench, and the first sacrificial layer 111 with the inclined surface is connected to the first sacrificial layer 111 located at the bottom of the deep trench through the first sacrificial layer 111 with the vertical surface, and the remaining first sacrificial layer 111 exposes a portion of the upper sidewall surface of the deep trench 101; in another embodiment, the remaining first sacrificial layer 111 completely covers the sidewall surface of the deep trench 101.In one embodiment, the implantation process is a single step ion implantation process, and the implantation energy of the single step ion implantation process is reduced stepwise. The single step ion implantation process forms a second sacrificial layer on the side wall of the deep trench 101, and the density of the second sacrificial layer gradually increases from the outside to the inside. The second sacrificial layer, the third sacrificial layer and the first sacrificial layer 111 are etched using the barrier layer 130 as a mask. The remaining first sacrificial layer 111 located on the side wall of the deep trench has a step surface that gradually descends along the side wall of the deep trench toward the bottom of the deep trench.
[0041] like Figure 7 As shown, the barrier layer 130 is removed.
[0042] Since this process is known in the art, the details are not repeated here.
[0043] In one embodiment, after removing the barrier layer 130, the method further includes: etching back the remaining first sacrificial layer 111 on the sidewall of the deep trench 101 to ensure that the second sacrificial layer 120 at the bottom of the deep trench 101 is completely removed; at the same time, by etching back the remaining first sacrificial layer 111 on the sidewall of the deep trench 101, a portion of the upper sidewall surface of the deep trench 101 is exposed, and the remaining first sacrificial layer has an inclined surface intersecting the sidewall of the deep trench at an acute angle and a horizontal surface located at the bottom of the deep trench and parallel to the surface of the semiconductor substrate.
[0044] According to the method for preparing an SGT-MOSFET semiconductor device prepared by the method of the present invention, the density of the second sacrificial layer is lower than that of the first sacrificial layer; a third sacrificial layer is formed on the second sacrificial layer, and the density of the third sacrificial layer is lower than that of the second sacrificial layer, so as to form a film layer structure with a density increasing from the outside to the inside on the sidewall of the deep trench, and a barrier layer is filled in the deep trench, and then the second sacrificial layer, the third sacrificial layer, and a part of the first sacrificial layer located on the sidewall of the deep trench are removed using the barrier layer as a mask, the thickness of the remaining first sacrificial layer located on the sidewall of the deep trench gradually increases along the sidewall of the deep trench to the bottom of the deep trench, and the surface shape of the remaining first sacrificial layer located on the sidewall of the deep trench can be adjusted by an injection process, thereby achieving optimization of BV improvement, which has significant significance.
[0045] The above-described embodiments are only preferred embodiments of the present invention, and the embodiments are not intended to limit the patent protection scope of the present invention. Therefore, any equivalent structural changes made using the description and drawings of the present invention should also be included in the protection scope of the present invention.
[0046] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing an SGT-MOSFET semiconductor device, characterized in that: include: Providing a semiconductor substrate having a deep trench; forming an initial first sacrificial layer on the semiconductor substrate, wherein the initial first sacrificial layer also covers the sidewalls and bottom of the deep trench; Performing ion implantation on the initial first sacrificial layer using an implantation process to form a first sacrificial layer covering the sidewalls and bottom of the deep trench and a second sacrificial layer located on the first sacrificial layer on the semiconductor substrate; forming a third sacrificial layer on the second sacrificial layer; forming a barrier layer filling the deep trench; Using the barrier layer as a mask, removing the second sacrificial layer, the third sacrificial layer, and a portion of the first sacrificial layer located on the sidewalls of the deep trench, wherein the thickness of the remaining first sacrificial layer located on the sidewalls of the deep trench gradually increases along the sidewalls of the deep trench toward the bottom of the deep trench; removing the barrier layer; The implantation energy of the implantation process is 30 KeV to 100 KeV, the implantation depth of the ion implantation is 300 angstroms to 500 angstroms, and the thickness of the second sacrificial layer is 300 angstroms to 500 angstroms; The third sacrificial layer has a lower density than the second sacrificial layer; The etching removal rate of the third sacrificial layer is greater than the etching removal rate of the second sacrificial layer; and the etching removal rate of the second sacrificial layer is greater than the etching removal rate of the first sacrificial layer.
2. The method for preparing the SGT-MOSFET semiconductor device according to claim 1, wherein: The angle between the sidewall and the bottom of the deep trench is 86.5° to 89.5°.
3. The method for preparing the SGT-MOSFET semiconductor device according to claim 1, wherein: The semiconductor substrate is a silicon substrate, the material of the initial first sacrificial layer is silicon oxide, the formation process of the first sacrificial layer includes a thermal oxidation method, and the thickness of the initial first sacrificial layer is 2000 angstroms to 8000 angstroms.
4. The method for preparing the SGT-MOSFET semiconductor device according to claim 1, wherein: The ions implanted are argon ions, and the density of the second sacrificial layer is lower than that of the first sacrificial layer.
5. The method for preparing the SGT-MOSFET semiconductor device according to claim 4, wherein: The thickness of the third sacrificial layer is 200 angstroms to 800 angstroms, and the formation process of the third sacrificial layer includes chemical vapor deposition.
6. The method for preparing the SGT-MOSFET semiconductor device according to claim 1, wherein: The barrier layer includes one of a photoresist layer and a BARC layer, and a surface of the barrier layer is lower than or flush with a surface of the third sacrificial layer located on the semiconductor substrate.
7. The method for preparing the SGT-MOSFET semiconductor device according to claim 1, wherein: An isotropic etching process is used to remove the second sacrificial layer, the third sacrificial layer, and a portion of the first sacrificial layer located on the sidewall of the deep trench; the isotropic etching process includes one or a combination of an isotropic wet etching process and an isotropic dry etching process.
8. The method for preparing the SGT-MOSFET semiconductor device according to claim 1, wherein: The implantation process is a single continuous ion implantation process. The remaining first sacrificial layer located on the sidewall of the deep trench has an inclined surface intersecting the sidewall of the deep trench at an acute angle, and the inclined surface is a continuous and smooth surface.
9. The method for preparing the SGT-MOSFET semiconductor device according to claim 8, wherein: The remaining first sacrificial layer located on the sidewall of the deep trench also has a vertical surface parallel to the sidewall of the deep trench. The first sacrificial layer with the inclined surface is connected to the first sacrificial layer located at the bottom of the deep trench through the first sacrificial layer with the vertical surface.
10. The method for preparing the SGT-MOSFET semiconductor device according to claim 1, wherein: The implantation process is a single step ion implantation process, in which the implantation energy is reduced stepwise, and the remaining first sacrificial layer located on the sidewall of the deep trench has a step surface that descends gradually along the sidewall of the deep trench toward the bottom of the deep trench.
Citation Information
Patent Citations
Manufacturing method of field oxide with gradually changed thickness in trench and manufacturing method of SGT device
CN111128706A
Shallow trench isolation structure and manufacturing method thereof
CN111223811A
Method for manufacturing semiconductor device
US20060166419A1
Method of Manufacturing a Trench Oxide in a Trench for a Gate Structure in a Semiconductor Substrate
US20200212203A1