Phenylphosphinothiophene thermally excited delayed fluorescence host material, synthesis method and application thereof

By synthesizing phenylphosphonthiophene-type thermal excitation delayed fluorescent host materials, the carrier transmission ability is enhanced by using thiophene groups, the problems of exciton quenching and carrier transmission imbalance in OLED devices are solved, and efficient electrogenesis is achieved Luminous effect.

CN114524848BActive Publication Date: 2024-12-03HEILONGJIANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011323203.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-11-23
Publication Date
2024-12-03
Estimated Expiration
2040-11-23

AI Technical Summary

Technical Problem

In existing OLED devices, the large concentration of guest molecules leads to imbalance and incomplete exciton quenching and carrier transport, and it is difficult to effectively inhibit the self-quenching effect of molecules and the interaction between molecules.

Method used

Synthesize heat excitation delayed fluorescent host materials of phenylphosphonthiophene. By introducing thiophenyl groups, enhance the spin-orbit coupling of molecules and the transmission capacity of carriers, weaken the interaction between molecules and within molecules, and prepare good comprehensive performance Electrophosphorescence devices.

Benefits of technology

Effectively inhibit the quenching effect of molecules, ensure the balance of energy transfer between the main body and the guest molecule, reduce the driving voltage of the electroluminescent device, improve the luminescence efficiency and brightness, and prepare an excellent organic electroluminescent diode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002793518400000021
    Figure BDA0002793518400000021
  • Figure BDA0002793518400000061
    Figure BDA0002793518400000061
  • Figure BDA0002793518400000131
    Figure BDA0002793518400000131
Patent Text Reader

Abstract

The present invention provides a phenylphosphine thiophene thermally excited delayed fluorescence host material, which is a cyclic compound formed by introducing a thiophene group into phenylphosphine. The material can introduce a thiophene group, enhance the spin-orbit coupling of the molecule, enhance the carrier transmission capacity, have good thermodynamic stability, and effectively improve the comprehensive performance of the organic electroluminescent material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electroluminescent materials, and in particular relates to a phenylphosphinothiophene-type thermally excited delayed fluorescent aromatic phosphine oxide material. Background Art

[0002] At the beginning of the 20th century, one of the major scientific breakthroughs that affected people's daily lives on a global scale was the discovery of solid-state lighting (SSL). SSL is based on the concept of electroluminescence, where light is generated by the radiative transition of excitons, which are generated due to the efficient electron-hole recombination present in most semiconductor materials. SSL technology is divided into light-emitting diodes (LEDs), organic light-emitting diodes (OLEDs) and light-emitting electrochemical cells (LECs).

[0003] In OLED devices, light emission is mainly achieved through electrical excitation of the device. When an external voltage is applied to the OLED device, holes and electrons are injected from the anode and cathode sides respectively, transferred through the transport layer, and recombined in the light-emitting layer. The electrons are excited to generate 25% singlet excitons (S1) and 75% triplet excitons (T1). In order to reduce the self-quenching effect of the guest due to excessive exciton concentration, it is usually selected to dope the guest at a smaller concentration into a host material with energy level matching as the light-emitting layer of the organic electroluminescent device. Therefore, the main function of the host material is to transfer energy and disperse the guest. At present, the high molecular concentration in the guest material leads to the quenching of excitons and the unbalanced and incomplete carrier transfer.

[0004] Therefore, it is necessary to further develop host materials that can be used in conjunction with guest materials to obtain light-emitting devices with good comprehensive performance. Summary of the invention

[0005] In order to solve the above problems, the inventors have conducted intensive research and synthesized a type of thermally excited delayed fluorescence host material of phenylphosphine thiophene. The introduction of thiophene groups into phenylphosphine enhances the spin-orbit coupling of the molecule and the carrier transmission capacity, weakens the interaction between molecules and within molecules, and can effectively inhibit the quenching effect of the molecule. By using this type of compound as a thermally excited delayed fluorescence host material, an electrophosphorescent device with good comprehensive performance can be prepared, thereby completing the present invention.

[0006] The first aspect of the present invention aims to provide a phenylphosphine thiophene thermally excited delayed fluorescence host material, wherein the material is a cyclic compound formed by introducing a thiophene group into phenylphosphine. Preferably, the material is a phenylphosphine thiophene cyclic compound or a phenylphosphine oxythiophene cyclic compound.

[0007] In one embodiment of the present invention, the cyclic compound is:

[0008]

[0009] Wherein, X is oxygen or sulfur.

[0010] In another embodiment of the present invention, the cyclic compound further comprises a cyclic compound of Formula I or Formula II having a substituent at the hydrogen-containing position, and the substituent is selected from an alkyl group or an alkoxy group.

[0011] The phenylphosphinothiophene thermally excited delayed fluorescent host material is prepared using a thiophene compound and a phenylphosphine compound as raw materials, and preferably comprises the following steps:

[0012] Step 1, adding a thiophene compound and a lithium reagent into a solvent, and reacting to obtain a reaction solution I;

[0013] Step 2, adding a phenylphosphine compound to the reaction solution I to react to obtain an intermediate product I;

[0014] Step 3, adding the intermediate product I to the solvent again, adding a lithium reagent to react, and then adding a phenylphosphine compound to react to obtain an intermediate product II;

[0015] Step 4: adding the intermediate product II into a solvent, adding an oxidizing agent or a sulfurizing agent, and performing post-treatment to obtain a phenylphosphinothiophene-based thermally excited delayed fluorescent host material.

[0016] The second aspect of the present invention aims to provide a method for synthesizing the phenylphosphinothiophene thermally excited delayed fluorescent host material, which is prepared using a thiophene compound and a phenylphosphine compound as raw materials, and preferably comprises the following steps:

[0017] Step 1, adding a thiophene compound and a lithium reagent into a solvent, and reacting to obtain a reaction solution I;

[0018] Step 2, adding a phenylphosphine compound to the reaction solution I to react to obtain an intermediate product I;

[0019] Step 3, adding the intermediate product I to the solvent again, adding a lithium reagent to react, and then adding a phenylphosphine compound to react to obtain an intermediate product II;

[0020] Step 4: adding the intermediate product II into a solvent, adding an oxidizing agent or a sulfurizing agent, and performing post-treatment to obtain a phenylphosphinothiophene-based thermally excited delayed fluorescent host material.

[0021] The third aspect of the present invention aims to provide the use of the phenylphosphinothiophene thermally excited delayed fluorescent host material for preparing an electrophosphorescent device.

[0022] The phenylphosphinothiophene thermally excited delayed fluorescent host material and the synthesis method thereof provided by the present invention have the following beneficial effects:

[0023] (1) The phenylphosphinothiophene-based thermally excited delayed fluorescence host material provided in the present invention utilizes the introduction of thiophene groups to enhance the spin-orbit coupling of the molecule, enhance the carrier transport capability, weaken the intermolecular and intramolecular interactions, and effectively inhibit the quenching effect of the molecule.

[0024] (2) The phenylphosphinothiophene-based thermally excited delayed fluorescence host material provided in the present invention has a high triplet energy level, which can ensure the energy transfer between the host molecule and the guest molecule, and can solve the problems of exciton quenching and unbalanced and incomplete carrier transmission caused by high concentration of guest molecules.

[0025] (3) The host material molecules have a large steric hindrance effect, which can effectively inhibit the interaction between molecules and weaken the interaction between the host and the guest; it can also disperse the guest molecules and weaken the quenching effect between the guest molecules.

[0026] (4) The polarization effect of the phosphine oxide and phosphine sulfur groups in the host material can improve the electron injection and transmission capabilities of the material and reduce the driving voltage of the electroluminescent device. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The ultraviolet spectrum and fluorescence spectrum of compound (I) in Example 1 of the present invention are shown (■ in the figure represents the ultraviolet spectrum, and □ represents the fluorescence spectrum);

[0028] Figure 2 The thermogravimetric analysis diagram of compound (I) in Example 1 of the present invention is shown;

[0029] Figure 3 The ultraviolet spectrum and fluorescence spectrum of compound (II) in Example 2 of the present invention are shown (■ in the figure represents the ultraviolet spectrum, and □ represents the fluorescence spectrum);

[0030] Figure 4 The thermogravimetric analysis diagram of compound (II) in Example 2 of the present invention is shown;

[0031] Figure 5The ultraviolet spectrum and fluorescence spectrum of compound (III) in Example 3 of the present invention are shown (■ in the figure represents the ultraviolet spectrum, and □ represents the fluorescence spectrum);

[0032] Figure 6 The thermogravimetric analysis diagram of compound (III) in Example 3 of the present invention is shown;

[0033] Figure 7 The ultraviolet spectrum and fluorescence spectrum of compound (IV) in Example 4 of the present invention are shown (■ in the figure represents the ultraviolet spectrum, and □ represents the fluorescence spectrum);

[0034] Figure 8 The thermogravimetric analysis diagram of compound (IV) in Example 4 of the present invention is shown;

[0035] Fig. 9 The ultraviolet spectrum and fluorescence spectrum of compound (V) in Example 5 of the present invention are shown (■ in the figure represents the ultraviolet spectrum, and □ represents the fluorescence spectrum);

[0036] Fig.10 The thermogravimetric analysis diagram of compound (V) in Example 5 of the present invention is shown;

[0037] Fig.11 The ultraviolet spectrum and fluorescence spectrum of compound (VI) in Example 6 of the present invention are shown (■ in the figure represents the ultraviolet spectrum, and □ represents the fluorescence spectrum);

[0038] Fig.12 The thermogravimetric analysis diagram of compound (VI) in Example 6 of the present invention is shown;

[0039] Fig.13 The voltage-current density relationship curve of the electrophosphorescent device prepared in Example 1 of the present invention is shown;

[0040] Fig.14 The voltage-brightness relationship curve of the electrophosphorescent device prepared in Example 1 of the present invention is shown;

[0041] Fig.15 The brightness-current efficiency relationship curve of the electrophosphorescent device prepared in Example 1 of the present invention is shown;

[0042] Fig.16 The brightness-power efficiency relationship curve of the electrophosphorescent device prepared in Example 1 of the present invention is shown;

[0043] Fig.17 The brightness-external quantum efficiency relationship curve of the electrophosphorescent device prepared in Example 1 of the present invention is shown;

[0044] Fig.18 The electroluminescence spectrum of the electrophosphorescent device prepared in Example 1 of the present invention is shown;

[0045] Fig.19 The voltage-current density relationship curve of the electrophosphorescent device prepared in Example 2 of the present invention is shown;

[0046] Fig. 20 The voltage-brightness relationship curve of the electrophosphorescent device prepared in Example 2 of the present invention is shown;

[0047] Fig.21 The brightness-current efficiency relationship curve of the electrophosphorescent device prepared in Example 2 of the present invention is shown;

[0048] Fig. 22 The brightness-power efficiency relationship curve of the electrophosphorescent device prepared in Example 2 of the present invention is shown;

[0049] Fig.23 The brightness-external quantum efficiency relationship curve of the electrophosphorescent device prepared in Example 2 of the present invention is shown;

[0050] Fig.24 The electroluminescence spectrum of the electrophosphorescent device prepared in Example 2 of the present invention is shown;

[0051] Fig.25 The voltage-current density relationship curve of the electrophosphorescent device prepared in Example 3 of the present invention is shown;

[0052] Fig.26 The voltage-brightness relationship curve of the electrophosphorescent device prepared in Example 3 of the present invention is shown;

[0053] Fig. 27 The brightness-current efficiency relationship curve of the electrophosphorescent device prepared in Example 3 of the present invention is shown;

[0054] Fig.28 The brightness-power efficiency relationship curve of the electrophosphorescent device prepared in Example 3 of the present invention is shown;

[0055] Fig.29 The relationship curve between brightness and external quantum efficiency of the electrophosphorescent device prepared in Example 3 of the present invention is shown;

[0056] Fig.30 The electroluminescence spectrum of the electrophosphorescent device prepared in Example 3 of the present invention is shown;

[0057] Fig.31 The voltage-current density relationship curve of the electrophosphorescent device prepared in Example 4 of the present invention is shown;

[0058] Fig.32 The voltage-brightness relationship curve of the electrophosphorescent device prepared in Example 4 of the present invention is shown;

[0059] Fig.33 The brightness-current efficiency relationship curve of the electrophosphorescent device prepared in Example 4 of the present invention is shown;

[0060] Fig.34 The brightness-power efficiency relationship curve of the electrophosphorescent device prepared in Example 4 of the present invention is shown;

[0061] Fig.35 The relationship curve between brightness and external quantum efficiency of the electrophosphorescent device prepared in Example 4 of the present invention is shown;

[0062] Fig.36 The electroluminescence spectrum of the electrophosphorescent device prepared in Example 4 of the present invention is shown;

[0063] Fig.37 The voltage-current density relationship curve of the electrophosphorescent device prepared in Example 5 of the present invention is shown;

[0064] Fig.38 The voltage-brightness relationship curve of the electrophosphorescent device prepared in Example 5 of the present invention is shown;

[0065] Fig.39 The brightness-current efficiency relationship curve of the electrophosphorescent device prepared in Example 5 of the present invention is shown;

[0066] Fig.40 The brightness-power efficiency relationship curve of the electrophosphorescent device prepared in Example 5 of the present invention is shown;

[0067] Fig.41 The brightness-external quantum efficiency relationship curve of the electrophosphorescent device prepared in Example 5 of the present invention is shown;

[0068] Fig.42 The electroluminescence spectrum of the electrophosphorescent device prepared in Example 5 of the present invention is shown.

[0069] Fig.43 The voltage-current density relationship curve of the electrophosphorescent device prepared in Example 6 of the present invention is shown;

[0070] Fig.44 The voltage-brightness relationship curve of the electrophosphorescent device prepared in Example 6 of the present invention is shown;

[0071] Fig.45 The brightness-current efficiency relationship curve of the electrophosphorescent device prepared in Example 6 of the present invention is shown;

[0072] Fig.46 The brightness-power efficiency relationship curve of the electrophosphorescent device prepared in Example 6 of the present invention is shown;

[0073] Fig.47The brightness-external quantum efficiency relationship curve of the electrophosphorescent device prepared in Example 6 of the present invention is shown;

[0074] Fig.48 The electroluminescence spectrum of the electrophosphorescent device prepared in Example 6 of the present invention is shown. DETAILED DESCRIPTION

[0075] The present invention is described in detail below through specific implementation modes, and the characteristics and advantages of the present invention will become clearer and more specific with these descriptions.

[0076] The invention provides a phenylphosphine thiophene thermally excited delayed fluorescence host material, wherein the material is a cyclic compound formed by introducing a thiophene group into phenylphosphine.

[0077] Preferably, the material is a phenylphosphinethiophene cyclic compound or a phenylphosphineoxythiophene cyclic compound.

[0078] In one embodiment of the present invention, the cyclic compound is:

[0079]

[0080] Wherein, X is oxygen or sulfur.

[0081] In another embodiment of the present invention, the cyclic compound also includes a cyclic compound of Formula I or Formula II having a substituent at the hydrogen-containing position, wherein the substituent is selected from an alkyl group or an alkoxy group. The alkyl group is selected from a C1-C5 alkyl group, and the alkoxy group is selected from a C1-C5 alkoxy group.

[0082] Oxygen and sulfur heteroatoms have the ability to enhance spin-orbit coupling, change the transport capacity of carriers, and regulate the interaction within or between molecules. Introducing heteroatom-containing materials into organic electroluminescent devices as host materials can regulate the balance of carrier transport between the host and the guest. Therefore, the thiophene group is introduced into the phosphine oxygen or phosphine sulfur host with a rigid ring to adjust the molecular configuration and electrical properties of the material, thereby obtaining higher triplet and frontier orbital energy levels. By regulating the molecular configuration, coordinating the interaction between molecular structures, and developing host materials with strong transport capabilities, efficient electroluminescent devices can be prepared.

[0083] The phenylphosphinothiophene thermally excited delayed fluorescent host material provided by the present invention is prepared using a thiophene compound and a phenylphosphine compound as raw materials, and specifically comprises the following steps:

[0084] Step 1: Add a thiophene compound and a lithium reagent into a solvent, and react to obtain a reaction solution I.

[0085] The thiophene compound is selected from dihalogenated thiophene compounds, preferably selected from 2,3-halogenated thiophene compounds or 3,4-halogenated thiophene compounds, more preferably selected from 2,3-halogenated thiophene, 3,4-halogenated thiophene, alkyl-substituted 2,3-halogenated thiophene, alkoxy-substituted 2,3-halogenated thiophene, alkyl-substituted 3,4-halogenated thiophene or alkoxy-substituted 3,4-halogenated thiophene. The alkyl group is selected from C1-C5 alkyl, and the alkoxy group is selected from C1-C5 alkoxy. The halo is selected from chloro, bromo or iodo, preferably selected from bromo or iodo, such as bromo.

[0086] The lithium reagent is selected from alkyl lithium, preferably selected from n-butyl lithium, isobutyl lithium, tert-butyl lithium, and more preferably n-butyl lithium.

[0087] The solvent is selected from ethers, such as diethyl ether or tetrahydrofuran, and alkanes, such as n-hexane, preferably selected from diethyl ether, tetrahydrofuran or n-hexane, more preferably diethyl ether or tetrahydrofuran.

[0088] In a preferred embodiment of the present invention, the thiophene compound is first added to a solvent, stirred to dissolve, and then a lithium reagent is added dropwise to carry out a stirring reaction.

[0089] The molar ratio of the thiophene compound to the lithium reagent is 1:(1.05-1.5), preferably 1:(1.2-1.2). In the invention, the amount of phenylphosphine groups in the product can be adjusted by controlling the usage ratio of the thiophene compound to the lithium reagent.

[0090] The molar volume ratio of the thiophene compound to the solvent is 1 mmol:(5-28) mL, preferably 1 mmol:(7-20) mL, and more preferably 1 mmol:(9-12) mL.

[0091] The reaction temperature is -90 to -150°C, preferably -105 to -135°C, more preferably -115 to -125°C; the reaction time is 0.5 to 5h, preferably 1 to 4h, more preferably 1.5 to 3h. The reaction is carried out under a protective gas atmosphere, such as a nitrogen atmosphere. After the reaction is completed, a reaction solution I is obtained.

[0092] Step 2: Add a phenylphosphine compound to the reaction solution I to obtain an intermediate product I.

[0093] The phenylphosphine compound is selected from phenyl dihalophosphine compounds, preferably selected from phenyl dihalophosphine, alkyl substituted phenyl dihalophosphine or alkoxy substituted phenyl dihalophosphine. The alkyl is selected from C1-C5 alkyl, and the alkoxy is selected from C1-C5 alkoxy. The halo is selected from chloro, bromo or iodo, preferably selected from bromo or iodo, such as bromo.

[0094] The molar ratio of the phenylphosphine compound to the thiophene compound is 1:(0.45-0.65), preferably 1:(0.51-0.55).

[0095] The reaction temperature is 5-45°C, preferably 15-35°C, more preferably 20-25°C; the reaction time is 9-24h, preferably 12-21h, more preferably 15-18h.

[0096] In a preferred embodiment of the present invention, at the reaction temperature in step 1, a phenylphosphine compound is added, and the reaction is stirred for 1.5-2.5 hours, such as 2 hours, and then the temperature is raised to the reaction temperature in step 2 to react, so that the reaction system proceeds smoothly.

[0097] The reaction is carried out under a protective atmosphere, such as nitrogen.

[0098] After the reaction is completed, the reaction solution is poured into ice water for quenching. After the quenching is completed, the reaction solution is post-treated to obtain the intermediate product I.

[0099] The post-treatment process includes extraction, drying and purification.

[0100] The extraction is to extract the reaction solution with an extractant to obtain an organic phase. The extractant is selected from acetone and dichloromethane, preferably dichloromethane.

[0101] The drying is to use a desiccant to dry the organic phase to remove moisture. The desiccant is not specifically limited in the present invention, such as anhydrous sodium sulfate.

[0102] The purification is to purify the dried organic phase by column chromatography, and the eluent of the column chromatography is a mixed solvent of petroleum ether and dichloromethane.

[0103] Step 3: Add the intermediate product I into the solvent again, add a lithium reagent to react, then add a phenylphosphine compound to react to obtain the intermediate product II.

[0104] In step 3, the solvent, lithium reagent and phenylphosphine compound are preferably the solvent, lithium reagent and phenylphosphine compound in step 1, respectively.

[0105] The amounts of the solvent, lithium reagent and phenylphosphine compound used are preferably the same as those used in step 1, respectively.

[0106] After adding the lithium reagent, the reaction temperature is -90 to -150°C, preferably -105 to -135°C, more preferably -115 to -125°C; the reaction time is 0.5-5h, preferably 1-4h, more preferably 1.5-3h.

[0107] After adding the phenylphosphine compound, the above temperature is maintained for reaction for 1.5-2.5h, such as 2h, and then the temperature is raised to react. The reaction temperature is 5-45°C, preferably 15-35°C, and more preferably 20-25°C. After heating, the reaction time is 6-24h, preferably 8-20h, and more preferably 10-16h, so that the reaction system proceeds smoothly.

[0108] The reaction is carried out under a protective atmosphere, such as nitrogen.

[0109] After the reaction is completed, the reaction solution is poured into ice water for quenching. After the quenching is completed, the reaction solution is post-treated to obtain the intermediate product II.

[0110] The post-treatment process includes extraction, drying and purification.

[0111] The extraction is to extract the reaction solution with an extractant to obtain an organic phase. The extractant is selected from acetone and dichloromethane, preferably dichloromethane.

[0112] The drying is to use a desiccant to dry the organic phase to remove moisture. The desiccant is not specifically limited in the present invention, such as anhydrous sodium sulfate.

[0113] The purification is to purify the dried organic phase by column chromatography, and the eluent of the column chromatography is a mixed solvent of petroleum ether and dichloromethane.

[0114] Step 4: adding the intermediate product II into a solvent, adding an oxidizing agent or a sulfurizing agent, and performing post-treatment to obtain a phenylphosphinothiophene-based thermally excited delayed fluorescent host material.

[0115] The solvent is selected from halogenated hydrocarbon solvents, preferably halogenated alkane solvents, and more preferably dichloromethane.

[0116] The volume molar ratio of the solvent to the thiophene compound in step 1 is (4-18) mL:1 mmol, preferably (6-15) mL:1 mmol, and more preferably (8-12) mL:1 mmol.

[0117] When preparing the phenylphosphine oxythiophene cyclic compound, an oxidant is added, and the oxidant is selected from hydrogen peroxide or peracetic acid, preferably hydrogen peroxide, and more preferably a hydrogen peroxide aqueous solution with a mass fraction of 25%-35%.

[0118] The molar ratio of the oxidant to the thiophene compound in step 1 is (2-15):1, preferably (3-12):1, and more preferably (5-10):1.

[0119] When preparing phenylphosphinothiothiophene cyclic compounds, a vulcanizing agent is added, and the vulcanizing agent is selected from sulfur monochloride, benzoyl peroxide or elemental sulfur, preferably sulfur monochloride or elemental sulfur, and more preferably elemental sulfur.

[0120] The molar ratio of the sulfiding agent to the thiophene compound in step 1 is (2-15):1, preferably (3-12):1, more preferably (5-10):1, such as 5:1 or 10:1.

[0121] It is worth noting that when the molar amounts of the sulfiding agent and the thiophene compound in step 1 are different, the obtained phenylphosphinethiophene compound exists in cis-isomers and trans-isomers.

[0122] When the molar ratio of the vulcanizing agent to the thiophene compound in step 1 is less than or equal to 5:1, the obtained phenylphosphine thiophene thermally excited delayed fluorescence main material is a cis-phenylphosphine thiothiophene compound; when the molar ratio of the vulcanizing agent to the thiophene compound in step 1 is greater than or equal to 10:1, the obtained phenylphosphine thiophene thermally excited delayed fluorescence main material is a trans-phenylphosphine thiothiophene compound.

[0123] After the reaction is completed, the reaction solution is post-treated to obtain a phenylphosphinothiophene-based thermally excited delayed fluorescent host material.

[0124] The post-treatment process includes extraction, drying and purification.

[0125] The extraction is to extract the reaction solution with an extractant to obtain an organic phase.

[0126] When preparing phenylphosphineoxythiophene cyclic compounds, the extractant is selected from a mixed solvent of a saturated sodium bisulfite aqueous solution and a halogenated alkane, preferably a mixed solvent of a saturated sodium bisulfite aqueous solution and dichloromethane.

[0127] When preparing phenylphosphine-thiothiophene cyclic compounds, the extractant is selected from acetone and dichloromethane, preferably dichloromethane.

[0128] The drying is to use a desiccant to dry the organic phase to remove moisture. The desiccant is not specifically limited in the present invention, such as anhydrous sodium sulfate.

[0129] The purification is to purify the dried organic phase by column chromatography, and the eluent of the column chromatography is a mixed solvent of petroleum ether and ethyl acetate.

[0130] The invention provides an electrophosphorescent device prepared by using the phenylphosphinothiophene thermally excited delayed fluorescence main body material.

[0131] The electrophosphorescent device comprises a substrate layer, a conductive anode layer, a hole injection layer, a hole transport layer, an exciton blocking layer, a light emitting layer, a hole blocking layer, an electron transport layer, an electron injection layer and a cathode conductive layer.

[0132] The method for preparing the light-emitting device of the phenylphosphinothiophene thermally excited delayed fluorescent host material specifically comprises the following steps:

[0133] 1. preparing a conductive anode layer;

[0134] A glass or plastic substrate washed with deionized water is placed in a vacuum evaporator to prepare a conductive anode layer on the substrate layer. The conductive anode layer is selected from tin oxide conductive glass (ITO), transparent conductive polymers such as polyaniline, and semi-transparent metals such as Au, preferably ITO or semi-transparent metals, and more preferably ITO.

[0135] Preferably, the vacuum degree of vacuum evaporation is 1×10 -6 mbar, the evaporation rate is set to 0.1-0.3 nm / s, the evaporation material is indium tin oxide on the glass or plastic substrate, and the thickness of the anode conductive layer is 1-100 nm, preferably 8-20 nm, more preferably 10-15 nm, such as 10 nm.

[0136] Preferably, the hole injection layer, the hole transport layer, the exciton blocking layer, the light emitting layer, the hole blocking layer, the electron transport layer, the electron injection layer and the cathode conductive layer are prepared by vacuum evaporation.

[0137] 2. preparing a hole injection layer;

[0138] A hole injection layer is evaporated on the anode conductive layer, and the evaporated thickness is 2 to 20 nm, preferably 3 to 15 nm, more preferably 5 to 10 nm, such as 6 nm.

[0139] The hole injection layer material is selected from molybdenum oxide or poly (3,4-ethylenedioxythiophene): polystyrene sulfonate) (PEDOT:PSS), preferably molybdenum oxide, more preferably molybdenum oxide.

[0140] 3. Preparation of hole transport layer;

[0141] A hole transport layer is evaporated on the hole injection layer, and the evaporated thickness is 20-80 nm, preferably 30-70 nm, and more preferably 40-60 nm.

[0142] The hole transport layer material is selected from aromatic amine derivatives, such as N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine (NPB).

[0143] 4. preparing an exciton blocking layer;

[0144] The exciton blocking layer is evaporated on the hole transport layer, and the evaporated thickness is 1-20 nm, preferably 3-12 nm, more preferably 4-8 nm, such as 5 nm.

[0145] The exciton blocking layer material is selected from 9,9'-(1,3-phenyl)di-9H-carbazole (mCP) or bis[2-((oxy)diphenylphosphino)phenyl]ether (DPEPO), preferably 9,9'-(1,3-phenyl)di-9H-carbazole (mCP).

[0146] 5. preparing a light-emitting layer;

[0147] The light-emitting layer is evaporated on the exciton blocking layer, and the evaporated thickness is 10-50 nm, preferably 15-40 nm, and more preferably 20-30 nm.

[0148] The light-emitting layer material is a mixture of phenylphosphinothiophene thermally excited delayed fluorescent host material, 2CzPN (4,5-di(9-carbazolyl)-phthalonitrile) and 4CzTPN-Ph (2,3,5,6-tetrakis(3,6-diphenylcarbazol-9-yl)-1,4-dicyanobenzene).

[0149] 6. preparing a hole blocking layer;

[0150] The hole blocking layer is evaporated on the light-emitting layer, and the evaporated thickness is 1-16 nm, preferably 3-12 nm, more preferably 5-8 nm, such as 5 nm.

[0151] The hole blocking layer material is a phenylphosphinothiophene-based thermally excited delayed fluorescent host material.

[0152] 7. Preparing an electron transport layer;

[0153] The electron transport layer is evaporated on the hole blocking layer, and the evaporated thickness is 20-75 nm, preferably 30-65 nm, and more preferably 40-55 nm.

[0154] The electron transport layer material is selected from tris(8-hydroxyquinoline)aluminum (Alq3), 1,3,5-tris(1-phenyl-1H-benzimidazol-2-yl)benzene (TPBi), 4,7-diphenyl-1,10-phenanthroline (Bphen), 3-(biphenyl-4-yl)-5-(4-tert-butylphenyl)-4-phenyl-4H-1,2,4-triazole (TAZ), preferably Bphen.

[0155] 8. preparing an electron injection layer;

[0156] The electron injection layer is evaporated on the electron transport layer, and the evaporated thickness is 0.1-8 nm, preferably 0.5-5 nm, more preferably 1-2 nm, such as 1 nm.

[0157] The electron injection layer material is selected from lithium tetrakis(8-hydroxyquinoline)borate (LiBq4) or LiF, preferably LiF.

[0158] 9. Prepare a cathode conductive layer, encapsulate it, and obtain a thermally excited delayed fluorescence electrophosphorescent device.

[0159] The cathode conductive layer is evaporated on the electron injection layer, and the evaporated thickness is 60-150 nm, preferably 80-130 nm, more preferably 100-110 nm, such as 100 nm.

[0160] The cathode conductive layer material is selected from a single metal cathode or an alloy cathode, preferably calcium, magnesium, silver, aluminum, a calcium alloy, a magnesium alloy, a silver alloy or an aluminum alloy, such as aluminum.

[0161] The phenylphosphinothiophene-based thermally excited delayed fluorescent host material provided by the present invention has good thermodynamic stability. The prepared electrophosphorescent device reduces the turn-on voltage to 2.5V and simultaneously improves the luminous efficiency and brightness of the organic electroluminescent material, thereby being able to prepare an organic electroluminescent diode with excellent performance.

[0162] Example

[0163] Example 1

[0164] Under nitrogen atmosphere, add 1mmol of 2,3-dibromothiophene to 10ml of ether, cool to -120℃, add 1.1mmol of n-butyl lithium dropwise, stir for 2 hours, then add 0.55mmol of phenylphosphine dichloride, continue stirring for 2 hours, slowly return to room temperature, and react for 16 hours. After the reaction is completed, pour into an appropriate amount of ice water. Then extract the reactant with dichloromethane to obtain an organic phase, and dry the organic phase with excess anhydrous Na2SO4. Purify the dried organic phase by column chromatography to obtain intermediate product I, and the column chromatography eluent is a mixed solution of petroleum ether and dichloromethane, and the volume ratio of the two is 5:1.

[0165] The intermediate product I was dissolved in 10 mL of ether, cooled to -120 ° C under a nitrogen atmosphere, and 1.1 mmol of n-butyl lithium was added dropwise. After stirring for 2 hours, the mixture was slowly restored to room temperature, and 0.55 mmol of phenylphosphine dichloride was added, and the mixture was reacted for another 16 hours. After the reaction was completed, the mixture was poured into an appropriate amount of ice water. The reactant was then extracted with a mixed solution of water and dichloromethane to obtain an organic phase, the volume ratio of water to dichloromethane was 10:1, and the organic phase was dried with excess anhydrous Na2SO4. The dried organic phase was purified by column chromatography to obtain the intermediate product II, and the column chromatography eluent was a mixed solution of petroleum ether and dichloromethane, the volume ratio of the two being 3:1.

[0166] The intermediate product II is dissolved in 10 ml of dichloromethane, and an aqueous solution containing 10 mmol of H2O2 with a mass fraction of 30% is added for oxidation. The mixture is reacted at 0°C for 15 to 16 hours, and extracted with a mixed solution of saturated sodium bisulfite aqueous solution and dichloromethane to obtain an organic phase, which is dried with excess anhydrous Na2SO4, and the dried organic phase is purified by column chromatography using a mixed solvent of petroleum ether and ethyl acetate as an eluent to obtain compound I, 4,8-diphenylphosphineoxy-benzo[1,2-b:5,4-b']dithiophene, having the structural formula:

[0167]

[0168] The obtained compound (I) was subjected to mass spectrometry test, and the time-of-flight mass spectrum data were: m / z (%): 411.99 (100%) [M + ].

[0169] The obtained compound (I) was subjected to a nuclear magnetic resonance test, and the data of the nuclear magnetic resonance hydrogen spectrum were as follows:

[0170] 1 H-NMR (400MHz, CDCl3): δ=8.022 (dd, J1=3.2Hz, J2=6.4Hz, 4H), 7.927-7.872 (m, 4H), 7.596-7.556 (m, 2H), 7.592-7.484 (m, 4H).

[0171] From the above H NMR spectrum data, it can be seen that compound (I) was prepared through the above experimental process.

[0172] The thermogravimetric analysis spectrum of the obtained compound (I) is as follows: Figure 2 As shown by Figure 2 It can be seen that the pyrolysis temperature of compound (I) reaches 365°C.

[0173] The obtained compound (I) was tested by UV spectrum and fluorescence spectrum. The test spectrum is as follows: Figure 1 shown.

[0174] An electrophosphorescent device is prepared using a mixture of compound (I), 2CzPN and 4CzTPN-Ph as a light-emitting layer material and compound (I) as a hole blocking layer material, as follows:

[0175] 1. Place the glass or plastic substrate washed with deionized water into a vacuum evaporator for evaporation at a vacuum degree of 1×10 -6 mbar, and the evaporation rate was set to 0.1 nm s -1 , the evaporation material is indium tin oxide (ITO), and an anode conductive layer with a thickness of 10 nm is obtained;

[0176] 2. Vapor-depositing the hole injection layer material MoOx on the anode conductive layer to obtain a hole injection layer with a thickness of 6 nm;

[0177] 3. Evaporating the hole transport layer material NPB on the hole injection layer to obtain a hole transport layer with a thickness of 50 nm;

[0178] 4. Vapor depositing a blocking layer material mCP on the hole transport layer to obtain an exciton blocking layer with a thickness of 5 nm;

[0179] 5. Evaporating a light-emitting layer material on the exciton blocking layer: the light-emitting layer material is a mixture of compound (I), 2CzPN and 4CzTPN-Ph, wherein the mass fraction of 2CzPN is 60%, and the mass fraction of 4CzTPN-Ph is 0.5%, to obtain a light-emitting layer with a thickness of 25 nm;

[0180] 6. Continue to evaporate compound (I) on the light-emitting layer to obtain a hole blocking layer with a thickness of 5 nm;

[0181] 7. Evaporating the electron transport layer material Bphen on the hole blocking layer to form an electron transport layer with a thickness of 55 nm;

[0182] 8. Vapor depositing the electron injection layer material LiF on the electron transport layer to form an electron injection layer with a thickness of 1 nm;

[0183] 9. A cathode conductive layer whose material is aluminum and whose thickness is 100 nm is evaporated on the electron injection layer to obtain an electrophosphorescent device.

[0184] The structure of the electrophosphorescent device in this embodiment is: ITO / MoOx(6nm) / NPB(50nm) / mCP(5nm) / (Ⅰ):2CzPN(60%):4CzTPN-Ph(0.5%):(25nm) / (Ⅰ)(5nm) / Bphen(55nm) / LiF(1nm) / Al.

[0185] In Example 1, the voltage-current density relationship curve of the electrophosphorescent device is as follows: Fig.13 As shown in the figure, it can be seen that compound (I) has semiconductor properties and its threshold voltage is 2.5V.

[0186] In Example 1, the voltage-brightness relationship curve of the electrophosphorescent device is as follows: Fig.14 As shown in the figure, we can see that the turn-on voltage of the device is 2.8V.

[0187] In Example 1, the brightness-current efficiency relationship curve of the electrophosphorescent device is as follows: Fig.15 As shown in the figure, it can be seen that the device has a brightness of 1.127cd·m -2 When the current efficiency reaches the maximum value of 22.86cd·A-1 .

[0188] In Example 1, the brightness-power efficiency relationship curve of the electrophosphorescent device is as follows: Fig.16 As shown in the figure, it can be seen that the device has a brightness of 1.127cd·m -2 When the power efficiency reaches the maximum value of 37.64lm·W -1 .

[0189] In Example 1, the relationship curve between brightness and external quantum efficiency of the electrophosphorescent device is as follows: Fig.17 As shown in the figure, it can be seen that the device has a brightness of 1.127cd·m -2 When , the maximum external quantum efficiency of 25.14% was obtained.

[0190] In Example 1, the electroluminescence spectrum of the electroluminescent blue phosphorescent device is as shown in Fig.18 As shown, it can be seen from this figure that the electroluminescence peak of the device is at 504nm.

[0191] Example 2

[0192] According to the synthesis method of compound (I) in Example 1, compound (II), cis-DPDPcDTS2, was prepared. The only difference was that the H2O2 aqueous solution containing 10 mmol H2O2 with a mass fraction of 30% was replaced by 5 mmol S8 (precipitated sulfur), and the final product was extracted with dichloromethane after the reaction. The structural formula of compound (II) is:

[0193]

[0194] The obtained compound (II) was subjected to mass spectrometry test, and the time-of-flight mass spectrum data were: m / z (%): 443.95 (100) [M + ];

[0195] The obtained compound (II) was subjected to a nuclear magnetic resonance test, and the data of the nuclear magnetic resonance hydrogen spectrum were as follows:

[0196] 1 H-NMR (400MHz, CDCl3): δ=8.016 (dd, J1=3.2Hz, J2=7.6Hz, 4H), 7.902-7.844 (m, 2H), 7.534-7.492 (m, 2H), 7.468-7.423 (m, 4H).

[0197] From the above H NMR spectrum data, it can be seen that compound (II) was prepared through the above experimental process.

[0198] The obtained compound (II) was tested by UV spectrum and fluorescence spectrum. The test spectrum is as follows: Figure 3 shown.

[0199] The thermogravimetric analysis spectrum of the obtained compound (II) is as follows: Figure 4 As shown in the figure, it can be seen that the cracking temperature of compound (II) reaches 301°C.

[0200] An electrophosphorescent device was prepared according to the preparation method of the electrophosphorescent device in Example 1. The only differences were that the hole transport layer had a thickness of 45 nm; the light-emitting layer material was a mixture of compound (II), 2CzPN and 4CzTPN-Ph, wherein the mass fraction of 2CzPN was 60%, the mass fraction of 4CzTPN-Ph was 0.5%, and the light-emitting layer thickness was 20 nm; the hole blocking layer material was compound (II); and the electron transport layer thickness was 40 nm.

[0201] The structure of the electrophosphorescent device in this embodiment is: ITO / MoOx(6nm) / NPB(45nm) / mCP(5nm) / (Ⅱ):2CzPN(60%):4CzTPN-Ph(0.5%):(20nm) / (Ⅱ)(5nm) / Bphen(40nm) / LiF(1nm) / Al.

[0202] In Example 2, the voltage-current density relationship curve of the electrophosphorescent device is as follows: Fig.19 As shown in the figure, it can be seen that compound (II) has semiconductor properties and its threshold voltage is 3.6V.

[0203] In Example 2, the voltage-brightness relationship curve of the electrophosphorescent device is as follows: Fig. 20 As shown in the figure, we can see that the turn-on voltage of the device is 2.5V.

[0204] In Example 2, the brightness-current efficiency relationship curve of the electrophosphorescent device is as follows: Fig.21 As shown in the figure, it can be seen that the device has a brightness of 0.665cd·m -2 When the current efficiency reaches the maximum value of 25.11cd·A -1 .

[0205] In Example 2, the brightness-power efficiency relationship curve of the electrophosphorescent device is as follows: Fig. 22 As shown in the figure, it can be seen that the device has a brightness of 0.665cd·m -2 When the power efficiency reaches the maximum value of 35.33lm·W -1 .

[0206] In Example 2, the relationship curve between brightness and external quantum efficiency of the electrophosphorescent device is as follows: Fig.23 As shown in the figure, it can be seen that the device has a brightness of 0.665cd·m -2 When , the maximum external quantum efficiency of 22.14% was obtained.

[0207] In Example 2, the electroluminescence spectrum of the electrophosphorescent device is as follows: Fig.24 As shown, it can be seen from this figure that the electroluminescence peak of the device is at 500nm.

[0208] Example 3

[0209] According to the synthesis method of compound (II) in Example 2, compound (III), trans-DPDPcDTS2, was prepared. The only difference was that the amount of S8 (precipitated sulfur) added was 10 mmol. The structural formula of compound (III) was:

[0210]

[0211] The obtained compound (III) was subjected to mass spectrometry test, and the time-of-flight mass spectrum data were: m / z (%): 443.95 (100) [M + ];

[0212] The obtained compound (III) was subjected to a nuclear magnetic resonance test, and the data of the nuclear magnetic resonance hydrogen spectrum were as follows:

[0213] 1 H-NMR (400MHz, CDCl3): δ=8.658 (dd, J1=3.6Hz, J2=6.4Hz, 4H), 7.080-7.047 (m, 2H), 6.886-6.833 (m, 8H).

[0214] From the above H NMR spectrum data, it can be seen that compound (III) was prepared through the above experimental process.

[0215] The obtained compound (III) was tested by UV spectrum and fluorescence spectrum. The test spectrum is as follows: Figure 5 shown.

[0216] The thermogravimetric analysis spectrum of the obtained compound (III) is as follows: Figure 6 As shown in the figure, it can be seen that the cracking temperature of compound (III) reaches 306°C.

[0217] An electrophosphorescent device was prepared according to the preparation method of the electrophosphorescent device in Example 1. The only differences were that the hole transport layer had a thickness of 60 nm; the luminescent layer material was a mixture of compound (III), 2CzPN and 4CzTPN-Ph, wherein the mass fraction of 2CzPN was 60%, the mass fraction of 4CzTPN-Ph was 0.5%, and the luminescent layer thickness was 20 nm; the hole blocking layer material was compound (III); and the electron transport layer thickness was 40 nm.

[0218] The structure of the electrophosphorescent device in this embodiment is: ITO / MoOx(6nm) / NPB(60nm) / mCP(5nm) / (Ⅲ):2CzPN(60%):4CzTPN-Ph(0.5%):(20nm) / (Ⅲ)(5nm) / Bphen(40nm) / LiF(1nm) / Al.

[0219] In Example 3, the voltage-current density relationship curve of the electrophosphorescent device is as follows: Fig.25 As shown in the figure, it can be seen that compound (III) has semiconductor properties and its threshold voltage is 3.6V.

[0220] In Example 3, the voltage-brightness relationship curve of the electrophosphorescent device is as follows: Fig.26 As shown in the figure, we can see that the turn-on voltage of the device is 2.4V.

[0221] In Example 3, the brightness-current efficiency relationship curve of the electrophosphorescent device is as follows: Fig. 27 As shown in the figure, it can be seen that the device has a brightness of 0.637cd·m -2 When the current efficiency reaches the maximum value of 28.89cd·A -1 .

[0222] In Example 3, the brightness-power efficiency relationship curve of the electrophosphorescent device is as follows: Fig.28 As shown in the figure, it can be seen that the device has a brightness of 0.637cd·m -2 When the power efficiency reaches the maximum value of 34.9lm·W -1 .

[0223] In Example 3, the relationship curve between brightness and external quantum efficiency of the electrophosphorescent device is as follows: Fig.29 As shown in the figure, it can be seen that the device has a brightness of 0.637cd·m -2 When , the maximum external quantum efficiency of 22.14% was obtained.

[0224] In Example 3, the electroluminescence spectrum of the electrophosphorescent device is as follows: Fig.30 As shown, it can be seen from this figure that the electroluminescence peak of the device is at 504nm.

[0225] Example 4

[0226] Compound (IV), cis-DPDPbDTO2, was prepared according to the synthesis method of compound (I) in Example 1, except that 2,3-dibromothiophene was replaced by 3,4-dibromothiophene.

[0227] The structural formula of compound (IV) is:

[0228]

[0229] The obtained compound (IV) was subjected to mass spectrometry test, and the time-of-flight mass spectrum data were: m / z (%): 411.99 (100) [M + ];

[0230] The obtained compound (IV) was subjected to a nuclear magnetic resonance test, and the data of the nuclear magnetic resonance hydrogen spectrum were as follows:

[0231] δ=7.996-7.959(m,2H),7.767-7.739(m,2H),7.485-7.383(m,6H),7.331-7.739285(m,4H).

[0232] From the above H NMR spectrum data, it can be seen that compound (IV) was prepared through the above experimental process.

[0233] The obtained compound (IV) was tested by UV spectrum and fluorescence spectrum. The test spectrum is as follows: Figure 7 shown.

[0234] The thermogravimetric analysis spectrum of the obtained compound (Ⅳ) is as follows Figure 8 As shown in the figure, it can be seen that the cracking temperature of compound (Ⅳ) reaches 364°C.

[0235] An electrophosphorescent device was prepared according to the preparation method of the electrophosphorescent device in Example 1. The only differences were that the hole transport layer had a thickness of 40 nm; the luminescent layer material was a mixture of compound (IV), 2CzPN and 4CzTPN-Ph, wherein the mass fraction of 2CzPN was 60%, the mass fraction of 4CzTPN-Ph was 0.5%, and the luminescent layer thickness was 20 nm; the hole blocking layer material was compound (IV); and the electron transport layer thickness was 45 nm.

[0236] The structure of the electrophosphorescent device in this embodiment is: ITO / MoOx(6nm) / NPB(40nm) / mCP(5nm) / (Ⅳ):2CzPN(60%):4CzTPN-Ph(0.5%):(20nm) / (Ⅳ)(5nm) / Bphen(45nm) / LiF(1nm) / Al.

[0237] In Example 4, the voltage-current density relationship curve of the electrophosphorescent device is as follows: Fig.31 As shown in the figure, it can be seen that compound (IV) has semiconductor properties and its threshold voltage is 2.8V.

[0238] In Example 4, the voltage-brightness relationship curve of the electrophosphorescent device is as follows: Fig.32 As shown in the figure, we can see that the turn-on voltage of the device is 2.5V.

[0239] In Example 4, the brightness-current efficiency relationship curve of the electrophosphorescent device is as follows: Fig.33 As shown in the figure, it can be seen that the device has a brightness of 1.292cd·m -2 When the current efficiency reaches the maximum value of 27.48cd·A -1 .

[0240] In Example 4, the brightness-power efficiency relationship curve of the electrophosphorescent device is as follows: Fig.34 As shown in the figure, it can be seen that the device has a brightness of 1.292cd·m -2 When the power efficiency reaches the maximum value of 31.96lm·W -1 .

[0241] In Example 4, the relationship curve between brightness and external quantum efficiency of the electrophosphorescent device is as follows: Fig.35 As shown in the figure, it can be seen that the device has a brightness of 1.292cd·m -2 The maximum external quantum efficiency of 21.4% was obtained.

[0242] In Example 4, the electroluminescence spectrum of the electrophosphorescent device is as follows: Fig.36 As shown, it can be seen from this figure that the electroluminescence peak of the device is at 504nm.

[0243] Example 5

[0244] Compound (V), cis-DPDPbDTS2, was prepared according to the synthesis method of compound (II) in Example 2, except that 2,3-dibromothiophene was replaced by 3,4-dibromothiophene.

[0245] The structural formula of compound (V) is:

[0246]

[0247] The obtained compound (V) was subjected to mass spectrometry test, and the time-of-flight mass spectrum data were: m / z (%): 443.95 (100) [M + ];

[0248] The obtained compound (V) was subjected to a nuclear magnetic resonance test, and the data of the nuclear magnetic resonance hydrogen spectrum were as follows:

[0249] 1 H-NMR (400MHz, CDCl3): δ = 8.025 (dd, J1 = 6.8Hz, J2 = 16Hz, 2H), 7.897 (dd, J1 = 7.2Hz , J2=15.2Hz,2H),7.778-7.749(m,2H),7.551-7.458(m,6H),7.298-7.273(m,2H).

[0250] From the above H NMR spectrum data, it can be seen that compound (V) was prepared through the above experimental process.

[0251] The obtained compound (V) was tested by UV spectrum and fluorescence spectrum. The test spectrum is as follows: Fig. 9 shown.

[0252] The thermogravimetric analysis spectrum of the obtained compound (V) is as follows: Fig.10 As shown in the figure, it can be seen that the cracking temperature of compound (V) reaches 350°C.

[0253] An electrophosphorescent device was prepared according to the preparation method of the electrophosphorescent device in Example 1. The only differences were that the hole transport layer had a thickness of 50 nm; the luminescent layer material was a mixture of compound (V), 2CzPN and 4CzTPN-Ph, wherein the mass fraction of 2CzPN was 60%, the mass fraction of 4CzTPN-Ph was 0.5%, and the luminescent layer thickness was 25 nm; the hole blocking layer material was compound (V); and the electron transport layer thickness was 40 nm.

[0254] The structure of the electrophosphorescent device in this embodiment is: ITO / MoOx(6nm) / NPB(50nm) / mCP(5nm) / (V):2CzPN(60%):4CzTPN-Ph(0.5%):(25nm) / (V)(5nm) / Bphen(40nm) / LiF(1nm) / Al.

[0255] In Example 5, the voltage-current density relationship curve of the electrophosphorescent device is as follows: Fig.37 As shown in the figure, it can be seen that compound (V) has semiconductor properties and its threshold voltage is 2.7V.

[0256] In Example 5, the voltage-brightness relationship curve of the electrophosphorescent device is as follows: Fig.38 As shown in the figure, we can see that the turn-on voltage of the device is 2.6V.

[0257] In Example 5, the brightness-current efficiency relationship curve of the electrophosphorescent device is as follows: Fig.39 As shown in the figure, it can be seen that the device has a brightness of 0.665cd·m -2 When the current efficiency reaches the maximum value of 25.11cd·A -1 .

[0258] In Example 5, the brightness-power efficiency relationship curve of the electrophosphorescent device is as follows: Fig.40 As shown in the figure, it can be seen that the device has a brightness of 0.665cd·m -2 When the power efficiency reaches the maximum value of 35.33lm·W -1 .

[0259] In Example 5, the relationship curve between brightness and external quantum efficiency of the electrophosphorescent device is as follows: Fig.41 As shown in the figure, it can be seen that the device has a brightness of 0.665cd·m -2 When , the maximum external quantum efficiency of 22.14% was obtained.

[0260] In Example 5, the electroluminescence spectrum of the electrophosphorescent device is as follows: Fig.42 As shown, it can be seen from this figure that the electroluminescence peak of the device is at 504nm.

[0261] Example 6

[0262] According to the synthesis method of compound (III) in Example 3, compound (VI), trans-DPDPbDTS2, was prepared. The only difference was that 2,3-dibromothiophene was replaced by 3,4-dibromothiophene. The structural formula of compound (VI) is:

[0263]

[0264] The obtained compound (VI) was subjected to mass spectrometry test, and the time-of-flight mass spectrum data were: m / z (%): 443.95 (100) [M + ];

[0265] The obtained compound (VI) was subjected to a nuclear magnetic resonance test, and the data of the nuclear magnetic resonance hydrogen spectrum were as follows:

[0266] 1 H-NMR (400MHz, CDCl3): δ=7.962-9.933(m,2H), 7.893-7.863(m,2H), 7.340-7.213(m,6H), 7.161-7.113(m,4H).

[0267] From the above H NMR spectrum data, it can be seen that compound (VI) was prepared through the above experimental process.

[0268] The obtained compound (VI) was tested by UV spectrum and fluorescence spectrum. The test spectrum is as follows: Fig.11 shown.

[0269] The thermogravimetric analysis spectrum of the obtained compound (VI) is as follows: Fig.12 As shown in the figure, it can be seen that the pyrolysis temperature of compound (VI) reaches 343°C.

[0270] An electrophosphorescent device was prepared according to the preparation method of the electrophosphorescent device in Example 1. The only differences were that the hole transport layer had a thickness of 40 nm; the luminescent layer material was a mixture of compound (VI), 2CzPN and 4CzTPN-Ph, wherein the mass fraction of 2CzPN was 60%, the mass fraction of 4CzTPN-Ph was 0.5%, and the luminescent layer thickness was 30 nm; the hole blocking layer material was compound (VI); and the electron transport layer thickness was 40 nm.

[0271] The structure of the electrophosphorescent device in this embodiment is: ITO / MoOx(6nm) / NPB(40nm) / mCP(5nm) / (VI):2CzPN(60%):4CzTPN-Ph(0.5%):(30nm) / (VI)(5nm) / Bphen(40nm) / LiF(1nm) / Al.

[0272] In Example 6, the voltage-current density relationship curve of the electrophosphorescent device is as follows: Fig.43 As shown in the figure, it can be seen that compound (VI) has semiconductor properties and its threshold voltage is 2.9V.

[0273] In Example 6, the voltage-brightness relationship curve of the electrophosphorescent device is as follows: Fig.44 As shown in the figure, we can see that the turn-on voltage of the device is 2.5V.

[0274] In Example 6, the brightness-current efficiency relationship curve of the electrophosphorescent device is as follows: Fig.45 As shown in the figure, it can be seen that the device has a brightness of 0.6373cd·m -2 When the current efficiency reaches the maximum value of 28.89cd·A -1 .

[0275] In Example 6, the brightness-power efficiency relationship curve of the electrophosphorescent device is as follows: Fig.46 As shown in the figure, it can be seen that the device has a brightness of 0.6373cd·m -2 When the power efficiency reaches the maximum value of 34.9lm·W -1 .

[0276] In Example 6, the relationship curve between brightness and external quantum efficiency of the electrophosphorescent device is as follows: Fig.47 As shown in the figure, it can be seen that the device has a brightness of 0.6373cd·m -2 When , the maximum external quantum efficiency of 20.51% is obtained.

[0277] In Example 6, the electroluminescence spectrum of the electrophosphorescent device is as follows: Fig.48 As shown, it can be seen from this figure that the electroluminescence peak of the device is at 508nm.

[0278] The present invention is described in detail above in conjunction with specific embodiments and / or exemplary examples and drawings, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, various equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.

Claims

1. A phenylphosphinothiophene-based thermally excited delayed fluorescence host material, characterized in that: It is the following compound: Compound (III): The phenylphosphinothiophene thermally excited delayed fluorescent host material is used to prepare an electrophosphorescent device. The preparation method of the electrophosphorescent device comprises the following steps:

1. preparing a conductive anode layer; Putting a glass or plastic substrate cleaned with deionized water into a vacuum evaporator to prepare a conductive anode layer on the substrate layer; 2. preparing a hole injection layer; A hole injection layer is evaporated on the anode conductive layer, and the thickness of the evaporated layer is 2 to 20 nm; 3. Preparation of hole transport layer; A hole transport layer is evaporated on the hole injection layer, and the thickness of the evaporated layer is 20 to 80 nm; 4. preparing an exciton blocking layer; The exciton blocking layer is evaporated on the hole transport layer, the evaporation thickness is 1-20 nm, and the exciton blocking layer material is selected from 9,9'-(1,3-phenyl)di-9H-carbazole (mCP) or bis[2-((oxy)diphenylphosphino)phenyl]ether (DPEPO); 5. preparing a light-emitting layer; The light-emitting layer is evaporated on the exciton blocking layer, and the evaporation thickness is 10-50 nm. The light-emitting layer material is a mixture of phenylphosphinothiophene thermally excited delayed fluorescent host material, 2CzPN (4,5-di(9-carbazolyl)-phthalonitrile) and 4CzTPN-Ph (2,3,5,6-tetrakis(3,6-diphenylcarbazole-9-yl)-1,4-dicyanobenzene); 6. preparing a hole blocking layer; The hole blocking layer is evaporated on the light-emitting layer, and the thickness of the evaporated layer is 1-16 nm. The hole blocking layer material is a phenylphosphinothiophene-based thermally excited delayed fluorescent host material; 7. Preparing an electron transport layer; The electron transport layer is evaporated on the hole blocking layer, and the evaporation thickness is 20-75 nm. The electron transport layer material is selected from tris(8-hydroxyquinoline)aluminum (Alq3), 1,3,5-tris(1-phenyl-1H-benzimidazol-2-yl)benzene (TPBi), 4,7-diphenyl-1,10-phenanthroline (Bphen), 3-(biphenyl-4-yl)-5-(4-tert-butylphenyl)-4-phenyl-4H-1,2,4-triazole (TAZ); 8. preparing an electron injection layer; The electron injection layer is evaporated on the electron transport layer, the evaporation thickness is 0.1-8nm, and the electron injection layer material is selected from lithium tetrakis(8-hydroxyquinoline)borate (LiBq4) or LiF; 9. Prepare a cathode conductive layer, encapsulate it, and obtain a thermally excited delayed fluorescence electrophosphorescent device.

2. A method for synthesizing the phenylphosphinothiophene thermally excited delayed fluorescent host material according to claim 1, characterized in that: The method specifically comprises the following steps: Step 1, adding 3,4-dihalothiophene and a lithium reagent into a solvent, and reacting to obtain a reaction solution I; Step 2, adding phenyl dihalophosphine to the reaction solution I to react to obtain an intermediate product I; Step 3, adding the intermediate product I to the solvent again, adding a lithium reagent to react, and then adding a phenyl dihalophosphine to react to obtain an intermediate product II; Step 4: adding the intermediate product II into a solvent, adding a sulfurizing agent, and performing post-treatment to obtain a phenylphosphinothiophene-based thermally excited delayed fluorescence host material.

3. The method according to claim 2, characterized in that In step 1, the lithium reagent is selected from alkyl lithium.

4. The method according to claim 2, characterized in that: In step 2, the molar ratio of the phenyl dihalophosphine to 3,4-dihalothiophene is 1:(0.45-0.65).

5. The method according to claim 2, characterized in that: In step 3, the lithium reagent is selected from alkyl lithium.

6. Use of the phenylphosphinothiophene thermally excited delayed fluorescent host material according to claim 1 for preparing an electrophosphorescent device.