Lithium replenishing material and preparation method thereof, lithium ion battery and lithium replenishing method thereof

Through weak polar organic solvent coating and step-by-step multi-platform charging technology, the stability and processing problems of lithium supplement materials are solved, the electrochemical performance of lithium batteries is improved, and the efficient removal of lithium ions and the improvement of battery performance is achieved.

CN114566645BActive Publication Date: 2024-11-29XTC NEW ENERGY MATERIALS(XIAMEN) LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202210102351.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-27
Publication Date
2024-11-29
Estimated Expiration
2042-01-27

AI Technical Summary

Technical Problem

The structure of lithium supplementary materials in existing lithium batteries is unstable, easy to absorb water and dehiscend, and has no electrochemical activity on the surface, resulting in poor processing performance. The existing coating and doping methods are not effective, which cannot meet the needs of different lithium supplementary materials systems. Moreover, the electrical conductivity is poor and the electrical performance cannot be effectively exerted.

Method used

Weak polar organic solvent is used to coat the lithium supplement raw materials, form a protective layer through ball milling, and combine it with the step multi-platform charging method to maximize the removal of lithium ions in the lithium supplement material, improving the lithium supplement capacity and battery performance.

Benefits of technology

It significantly improves the air stability and processing performance of lithium supplement materials, enhances the overall performance of the battery, avoids cumbersome doping and coating tests, and is suitable for various lithium supplement material systems, improves the first charging capacity of the battery and Cyclic performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114566645B_ABST
    Figure CN114566645B_ABST
Patent Text Reader

Abstract

The present invention provides a lithium supplement material and a preparation method thereof, a lithium ion battery and a lithium supplement method thereof, and relates to the technical field of lithium batteries. The lithium supplement material is obtained by coating a weakly polar organic solvent on the surface of a lithium supplement raw material, thereby improving the poor air stability of the lithium supplement material and effectively avoiding the side effects caused by the introduction of the lithium supplement material. The present invention also relates to a lithium supplement method for a battery containing the lithium supplement material, comprising: generating a plurality of lithium desorption charging platforms according to the first cycle charging curve of the lithium supplement material, and performing step-by-step multi-platform charging on the battery according to the lithium desorption charging platform, so as to maximize the efficient desorption of lithium ions in the lithium supplement material, greatly improve the lithium supplement capacity of the material, and enhance the overall performance of the battery system. The method is simple to implement, highly versatile, and can be applied to a variety of lithium supplement materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium batteries, and in particular to lithium supplementing materials and preparation methods thereof, lithium ion batteries and lithium supplementing methods thereof. Background Art

[0002] In order to improve the energy density of lithium-ion batteries, high-capacity silicon negative electrode materials are gradually becoming the choice of battery companies and material suppliers, becoming one of the most promising negative electrode materials for the next generation of lithium-ion batteries. However, the large volume expansion of silicon negative electrodes and the low initial coulombic efficiency limit their practical application. Since the coulombic efficiency of the positive electrode material is much higher than that of the negative electrode, a solid electrolyte film, namely the SEI film, will be formed on the surface of the negative electrode material during the first charging process, which will consume lithium ions. In the battery, lithium ions are almost entirely provided by the positive electrode material, which will inevitably lead to the inability to fully utilize the capacity of the positive electrode material, resulting in waste of positive electrode materials and reduced battery capacity. Based on this, people have proposed the concept of "lithium replenishment", which is to replenish the lithium ions consumed by the formation of the SEI film during the first charging process of the battery by "replenishing lithium" on the negative electrode, positive electrode or separator.

[0003] At present, lithium supplement additives have become a research hotspot in the field of lithium batteries in recent years. The existing positive electrode lithium supplement process mainly adds a small amount of high-capacity positive electrode material during the positive electrode homogenization process. During the first charge, the excess lithium element is removed from the high-capacity positive electrode material and embedded in the negative electrode to supplement the irreversible capacity of the first charge and discharge. However, this type of lithium supplement material itself has an unstable structure, poor air storage, easy water absorption and deliquescence, and the material has no electrochemical activity on the surface, high residual lithium content, high alkalinity, and difficulty in exerting electrochemical performance. The problems restrict its processing performance, such as high alkalinity causing the positive electrode adhesive to fail, which greatly limits its application in the field of lithium batteries. In the prior art, in order to improve the stability of lithium supplement materials, some researchers form a coating layer of carbon or polymer on the outside of the lithium supplement material by vapor phase chemical deposition, polymerization or composite, so as to block the contact reaction between moisture and carbon dioxide in the air and the core lithium supplement material. In addition, some researchers introduce lithium supplement materials by spraying the mixture to solve the problem of difficulty in processing lithium supplement materials. However, the above methods have problems such as poor coating effect and uniformity, high cost, or difficulty in scalability. They cannot meet the needs of different lithium supplement material systems, and no effective solutions have been found for problems such as poor conductivity of the material itself and the inability to effectively exert electrical properties. Summary of the invention

[0004] In order to solve the above technical problems, the present disclosure provides a lithium supplement material and a preparation method thereof, a lithium ion battery and a lithium supplement method thereof.

[0005] A first aspect of the present disclosure provides a positive electrode lithium supplement material, comprising a lithium supplement raw material and a protective layer coated on the surface of the lithium supplement raw material, wherein the protective layer is formed by immersing in a weak polar organic solvent.

[0006] The second aspect of the present disclosure provides a method for preparing a positive electrode lithium supplement material, comprising: immersing a lithium supplement raw material in a weakly polar organic solvent, adding a ball milling medium, and after ball milling, performing solid-liquid separation to obtain a positive electrode lithium supplement material.

[0007] In one embodiment of the present disclosure, the weakly polar organic solvent includes one or more of isopentane, n-pentane, petroleum ether, hexane, cyclohexane, cyclopentane, heptane, carbon tetrachloride and trichlorotrifluoroethane.

[0008] In one embodiment of the present disclosure, the ball-to-material ratio of the ball milling medium to the lithium supplement raw material is 1 to 10:1, and the rotation speed of the ball mill is 50 to 500 rad / min.

[0009] In one embodiment of the present disclosure, the lithium supplement raw material is selected from lithium metal and / or lithium-containing composites, wherein the lithium-containing composites include lithium and other metal composite alloys, organic lithium acids, and binary or multi-component substances generated by the combination of lithium elements in inorganic lithium acids with other anions or metal / non-metal compounds.

[0010] In one embodiment of the present disclosure, the lithium supplement raw material is selected from one or more of lithium metal, Li2NiO2, Li2CuO2, Li5FeO4, Li6CoO4 and Li6MnO4.

[0011] A third aspect of the present disclosure provides a lithium-ion battery lithium replenishment method, comprising:

[0012] S1, preparing a positive electrode lithium supplement material according to any of the preparation methods described above;

[0013] S2, obtaining a first-cycle charging curve of the positive electrode lithium supplementing material, and generating a plurality of lithium de-charging platforms according to the first-cycle charging curve;

[0014] S3, mixing the positive electrode active material with the positive electrode lithium supplement material to obtain a battery positive electrode material, making the battery positive electrode material into a positive electrode sheet, and making a battery with the positive electrode sheet and the negative electrode sheet;

[0015] S4, performing step-by-step multi-platform charging on the battery based on the lithium removal charging platform obtained in step S2 to remove lithium ions from the positive electrode lithium supplement material.

[0016] In one embodiment of the present disclosure, in step S2, generating a plurality of lithium-removal charging platforms according to the first cycle charging curve includes:

[0017] In the voltage interval of the first cycle charging curve, a preset voltage span is used as a voltage platform, and the voltage interval is divided into a plurality of voltage platforms;

[0018] It is determined whether the specific capacity of the voltage platform is greater than a preset specific capacity threshold, and the voltage platform that meets the condition is calibrated as a lithium-depletion voltage platform.

[0019] In one embodiment of the present disclosure, the voltage span is 0.1 to 0.5 V; and the specific capacity threshold is 20 to 2000 mAh / g.

[0020] In one embodiment of the present disclosure, in step S3, the positive electrode active material is selected from one or more of lithium iron phosphate, lithium manganese oxide, lithium cobalt oxide, and nickel cobalt manganese.

[0021] In one embodiment of the present disclosure, in step S4, performing step-by-step multi-platform charging on the battery based on the lithium-removal charging platform obtained in step S3 includes:

[0022] After entering the first de-lithium charging platform with the first constant current charging, the voltage value is maintained unchanged and constant voltage charging is performed until the current is reduced to the second current;

[0023] Then, after entering the next de-lithium charging platform with the first constant current charging, the voltage value is maintained unchanged and constant voltage charging is performed until the current is reduced to the second current;

[0024] Repeat the above charging process until the last lithium-removing charging platform is charged;

[0025] If the last de-lithium charging platform is not the target cut-off voltage, the constant current charging continues to the target cut-off voltage.

[0026] In one embodiment of the present disclosure, during the step multi-platform charging process, constant current charging is performed under a first temperature condition, then the temperature is raised to a second temperature for constant voltage charging, and then the temperature is lowered to the first temperature for constant current charging, and the above temperature change process is repeated until charging reaches the last delithiation charging platform, wherein the second temperature is greater than the first temperature.

[0027] In one embodiment of the present disclosure, the first temperature is 20-40°C, and the second temperature is 45-80°C.

[0028] In one embodiment of the present disclosure, the current density of the first current is 10-50 mA / g; the current density of the second current is 1-5 mA / g.

[0029] In one embodiment of the present disclosure, in step S3, the weight percentage of the positive electrode lithium supplement material in the battery positive electrode material does not exceed 5%.

[0030] A fourth aspect of the present disclosure provides a lithium-ion battery obtained according to any one of the above-mentioned lithium-ion battery lithium replenishment methods.

[0031] The beneficial effects of the lithium supplement material and preparation method thereof, lithium ion battery and lithium supplement method thereof according to the embodiments of the present invention are:

[0032] The poor air stability of lithium-supplementing materials and the difficulty in processing battery slurry are improved by coating with weak polar organic solvents. By soaking the lithium-supplementing raw materials in weak polar organic solvents and performing a simple wet ball milling and firing-free treatment, a layer of weak polar organic protective film is formed on the surface of the material, which can block water and CO2 in the air, and at the same time prevent the residues of the lithium-supplementing materials after delithiation from dissolving into NMP and the electrolyte to cause side reactions. According to the first-cycle charging curve of the lithium-supplementing material, multiple delithiation charging platforms are generated, and the battery is charged on a step-by-step basis according to the delithiation charging platform, so that the lithium ions in the lithium-supplementing material can be efficiently removed to the maximum extent, which greatly improves the lithium-supplementing capacity of the material and enhances the overall performance of the battery system. Moreover, the lithium-supplementing method disclosed in the present invention avoids cumbersome doping and coating trial-and-error tests, has strong versatility, and can be applied to various lithium-supplementing material systems. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0034] Figure 1 A flow chart of a lithium replenishment method for a lithium-ion battery according to an embodiment of the present invention;

[0035] Figure 2 Schematic diagram of the step-by-step multi-platform charging process of step S4 in the lithium replenishment method for a lithium-ion battery according to an embodiment of the present invention. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0037] The lithium replenishing material and preparation method thereof, the lithium ion battery and the lithium replenishing method thereof according to the embodiments of the present invention are described in detail below.

[0038] A positive electrode lithium supplement material provided by an embodiment of the present invention comprises a lithium supplement raw material and a protective layer coated on the surface of the lithium supplement raw material, wherein the protective layer is formed by soaking in a weak polar organic solvent.

[0039] The preparation method of the positive electrode lithium supplement material comprises: soaking the lithium supplement raw material in a weak polar organic solvent, adding a ball milling medium, and after ball milling, performing solid-liquid separation to obtain the positive electrode lithium supplement material.

[0040] In one embodiment of the present disclosure, the weakly polar organic solvent includes one or more of isopentane, n-pentane, petroleum ether, hexane, cyclohexane, cyclopentane, heptane, carbon tetrachloride and trichlorotrifluoroethane. The above-mentioned weakly polar organic solvent has a small polarity, which is conducive to forming a coating layer on the surface of the lithium supplement raw material. Through a simple wet ball milling method, no additional sintering step is required, the process is simple and easy to implement.

[0041] In one embodiment of the present disclosure, the ball-to-material ratio of the ball milling medium to the lithium supplement raw material is 1 to 10:1, and the ball milling speed is 50 to 500 rad / min. More preferably, the ball-to-material ratio is 2 to 5:1, for example, the ball-to-material ratio is 2:1, 3:1, 4:1, 5:1, etc. The speed is preferably 100 to 300 rad / min, for example, 150 rad / min, 200 rad / min, 250 rad / min, etc. By adjusting the appropriate ball-to-material ratio and speed, the lithium supplement raw material is ground and crushed, the coating area of ​​the weak organic solvent on the lithium supplement raw material is increased, and the uniformity of the coating is improved.

[0042] In one embodiment of the present disclosure, the ball milling medium is zirconium balls, such as commercially available high-purity zirconium oxide ceramic balls, which have high strength and good toughness.

[0043] In one embodiment of the present disclosure, the lithium supplement raw material is selected from lithium metal and / or lithium-containing composites, wherein the lithium-containing composites include lithium and other metal composite alloys, organic acid lithium, and inorganic acid lithium in which lithium elements are combined with other anions or metal / non-metal compounds to form binary or multi-element substances. Further preferably, the lithium supplement raw material is selected from one or more of lithium metal, Li2NiO2, Li2CuO2, Li5FeO4, Li6CoO4 and Li6MnO4.

[0044] This embodiment also provides a lithium-ion battery lithium replenishment method, comprising:

[0045] Step S1, preparing a positive electrode lithium supplement material; the preparation method of the positive electrode lithium supplement material is as shown above, that is, the lithium supplement raw material is immersed in a weak polar organic solvent, a ball milling medium is added, and after ball milling, solid-liquid separation is performed to obtain the positive electrode lithium supplement material.

[0046] Step S2, obtaining the first cycle charging curve of the positive electrode lithium supplement material obtained in step S1, and generating a plurality of lithium desorption charging platforms according to the first cycle charging curve.

[0047] Specifically, obtaining the first cycle charging curve of the positive electrode lithium supplement material obtained in step S1 specifically includes:

[0048] Step S21, the positive electrode lithium replenishing material prepared in step S1, the positive electrode lithium replenishing material and the conductive agent and the binder are mixed in a mass ratio of 8:1:1, and a dispersant and a solvent are added to make a button battery. The button battery is tested with a small current in the voltage range of 2V to 5V to obtain the first cycle charging curve of the positive electrode lithium replenishing material. Further preferably, the current density of the small current test is 5 to 10mA / g. For example, the button battery is charged and tested with a current of 10mA / g in the voltage range of 2V to 5V to obtain the first cycle charging curve.

[0049] Among them, the conductive agent is, for example, graphite, and the adhesive is, for example, PVDF. The dispersant can be, for example, lithium tetrafluoroborate, lithium hexafluoroborate, lithium hexafluoroarsenate, lithium diformate borate, etc. The solvent can be, for example, ethylene carbonate (EC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), vinylene carbonate (VC), fluoroethylene carbonate (FEC), sulfite (PS), etc. For example, in one embodiment, the positive electrode lithium supplement material is mixed with graphite and PVDF in a mass ratio of 8:1:1, and the electrolyte is added and mixed, and the electrolyte includes 1.2M LiPF6, EC, EMC, DMC in a volume ratio of 1:1:1, and 1wt.% VC and 1wt.% FEC.

[0050] Specifically, generating a plurality of lithium-removal charging platforms according to the first-cycle charging curve specifically includes:

[0051] Step S22, within the voltage interval of the first cycle charging curve, the voltage interval is divided into a plurality of voltage platforms with a preset voltage span as a voltage platform. Specifically, the voltage interval may be, for example, 2V to 5V.

[0052] Further preferably, the preset voltage span is 0.1V to 0.5V, such as 0.1V, 0.2V, 0.3V, etc. In one embodiment, the voltage interval is divided with a voltage span of 0.1V as a voltage platform.

[0053] Step S23, determining whether the specific capacity of the voltage platform is greater than a preset specific capacity threshold, and calibrating the voltage platform that meets the condition as a de-lithiation voltage platform.

[0054] Further preferably, the preset specific capacity threshold is 20 to 2000mAh / g, and the voltage platform range is 20 to 2000mAh / (g*preset voltage span). More preferably, the preset specific capacity threshold is 50 to 1000mAh / g, and the voltage platform range is 50 to 1000mAh / (g*preset voltage span). For example, in one embodiment, the preset voltage span is 0.1V, the preset specific capacity threshold is 50mAh / g, and in the voltage range of 2V to 5V, the specific capacity of the voltage platforms of 3.1V, 3.2V, and 4.1V is greater than 50mAh / g, then 3.1V, 3.2V, and 4.1V are calibrated as delithiation voltage platforms Vp1 (3.1V), Vp2 (3.2V), and Vp3 (4.1V) respectively.

[0055] S3, mixing the positive electrode active material with the positive electrode lithium supplement material obtained in step S1 to obtain a positive electrode material for a battery, making the positive electrode material for the battery into a positive electrode sheet, and making the positive electrode sheet and the negative electrode sheet into a battery. Further preferably, the weight percentage of the positive electrode lithium supplement material in the positive electrode material for the battery does not exceed 5%.

[0056] Further preferably, the positive electrode active material is selected from one or more of lithium iron phosphate, lithium manganese oxide, lithium cobalt oxide, and nickel cobalt manganese.

[0057] In one embodiment, the positive electrode material of the battery is made into a positive electrode sheet, and the positive electrode sheet and the negative electrode sheet are made into a battery, specifically including: adding a conductive agent, a binder, a dispersant, and a solvent to the positive electrode material of the battery to make a positive electrode slurry, coating the positive electrode slurry on the current collector, and completing the production of the positive electrode sheet by rolling. Graphite and / or silicon-carbon material are used as negative electrode materials, mixed with a conductive agent, a binder, etc. to make a negative electrode slurry, coating the negative electrode slurry on the current collector, and completing the production of the negative electrode sheet by rolling. The positive electrode sheet, the separator, and the negative electrode sheet are wound to form a battery.

[0058] S4, based on the lithium removal charging platform obtained in step S2, the battery is charged in a stepped multi-platform manner to remove lithium ions in the positive electrode lithium supplement material. By means of multi-platform charging, lithium ions can be fully removed, and the positive electrode material of the battery will provide more lithium ions to offset the lithium ions consumed in the formation process of the SEI film, so that the initial charging capacity of the battery is greatly improved.

[0059] See also Figure 2 As shown, in this step, the step of performing step-by-step multi-platform charging on the battery using the lithium-removing charging platform obtained in step S3 specifically includes:

[0060] Step S31, after charging with the first constant current A1 to enter the first lithium de-charging platform Vp1, the voltage value Vp1 is maintained unchanged and constant voltage charging is performed until the current decreases to the second current A2;

[0061] Step S32, after entering the next lithium removal charging platform (Vp2, etc.) with the first current A1 constant current charging, the voltage value (Vp2, etc.) is maintained unchanged, and constant voltage charging is performed until the current is reduced to the second current A2;

[0062] Step S33, repeating the charging process of step S32 until charging reaches the last lithium-removal charging platform Vpn, where n represents a total of n lithium-removal charging platforms;

[0063] Step S34, if the last de-lithiation charging platform Vpn is not the target cut-off voltage, then continue constant current charging to the target cut-off voltage. Preferably, in this step, constant current charging can be performed with the first current A1 to the target cut-off voltage.

[0064] Through the above-mentioned multi-step platform charging process, the lithium ions of the lithium supplement material are concentrated on the corresponding lithium de-ion charging platform and are efficiently de-ionized.

[0065] Further preferably, the current density of the first current A1 is 10-50 mA / g; and the current density of the second current A2 is 1-5 mA / g.

[0066] Further preferably, during the step multi-platform charging process, constant current charging is performed under the first temperature T1, then the temperature is raised to the second temperature T2 for constant voltage charging, and then the temperature is lowered to the first temperature T1 for constant current charging, and the above temperature change process is repeated until the last de-lithium charging platform Vpn is charged, wherein the second temperature T2 is greater than the first temperature T1. More preferably, in a preferred embodiment, the first temperature T1 is 20-40°C, and the second temperature T2 is 45-80°C. Among them, the first temperature T1 and the second temperature T2 are the temperatures of the voltage platform.

[0067] By setting a variable temperature process during the multi-step platform charging process, the temperature of the lithium-removing charging platform is increased, the release of lithium ions is accelerated, and the number of lithium ions released is increased, shortening the overall activation time of the battery. Cooling treatment is performed during charging on the non-lithium-removing charging platform to reduce the adverse effects of long-term high temperature on the battery.

[0068] This embodiment also provides a lithium-ion battery obtained according to the above-mentioned lithium-ion battery lithium replenishment method.

[0069] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0070] Example

[0071] This embodiment provides a lithium-ion battery lithium replenishment method, comprising:

[0072] (1) The positive electrode lithium replenishing raw material is immersed in a weak polar organic solvent, zirconium balls are added according to a ball-to-material weight ratio of 3:1, ball milling is performed at 300 rad / min for mixing / crushing, and a funnel is used for suction filtration and liquid-solid separation to obtain a positive electrode lithium replenishing material with a weak polar organic solvent coated on the surface.

[0073] (2) The positive electrode lithium replenishing material obtained in (1) is mixed with a conductive agent and a binder in a ratio of 8:1:1, and a dispersant and a solvent are added to complete the production of a button battery. A small current test of 10 mA / g is performed in the voltage range of 2 V to 5 V to obtain the first cycle charging curve of the positive electrode lithium replenishing material.

[0074] (3) Based on the first cycle charging curve obtained in (2), the voltage range of 2V to 5V is divided into charging platforms with 0.1V as a voltage platform, and the voltage platforms with a specific capacity greater than 50mAh / g are calibrated as delithiation voltage platforms Vp1, Vp2, ..., Vpn in sequence.

[0075] (4) The positive electrode lithium supplement material obtained in (1) is mixed with the positive electrode active material in a certain proportion, and a conductive agent, a binder, a dispersant and a solvent are added to complete the production of the positive electrode plate. At the same time, the negative electrode material is selected from graphite or silicon carbon or a mixture of the two materials, and matched with the negative electrode plate to complete the battery production.

[0076] (5) According to the de-lithiation voltage platforms Vp1, Vp2, ..., Vpn obtained in (3), the battery is charged in a step-by-step manner. The specific process is as follows: the charging voltage range is V0 to V 截止 , from the initial voltage V0, constant current charging with current A1 at temperature T1 until entering voltage platform Vp1, heating to T2, maintaining voltage Vp1 at temperature T2 for constant voltage charging, the current continues to decrease and decreases to current A2. Cooling down to temperature T1, changing to constant current charging with current A1 until entering voltage platform Vp2, heating up to T2, constant voltage charging at temperature T2, repeating the above charging process, to the last lithium de-ion charging platform Vpn, maintaining voltage Vpn at temperature T2 for constant voltage charging until the current drops to A2, then cooling down to temperature T1, constant current charging with current A1 until entering cut-off voltage V 截止 , ending the charging process.

[0077] Test Example 1

[0078] According to step (1) of the above embodiment, the performance of the positive electrode lithium supplement material obtained by coating with different weakly polar organic solvents was tested, and the test results are shown in Table 1. Table 1 shows the performance test results of the positive electrode lithium supplement material Li2NiO2 coated with different weakly polar organic solvents.

[0079] Table 1

[0080]

[0081] a : The capacity of the positive electrode lithium replenishing material is the first charging capacity of a button battery made of the positive electrode lithium replenishing material as the positive electrode active material (for the specific preparation method, see step (2) of the above embodiment).

[0082] As shown in Table 1, the use of weakly polar organic solvents to coat the lithium replenishing raw materials increases the capacity of the positive electrode lithium replenishing material in the initial state (0h, not shelved), and the capacity retention rate is still good in the subsequent long-term shelving tests (10h, 20h, 30h). Among them, in implementations 1 to 4, the coating effect of cyclohexane is the best. For Comparative Example 1, which is not coated with a weak organic solvent, although the capacity in the initial state is relatively high, its capacity is significantly attenuated after being shelved for a period of time. In other comparative examples 2 to 4 that use organic solvents with higher polarity for coating, several conventional solvents greatly limit the capacity of the materials.

[0083] Test Example 2

[0084] According to step (1) and step (2) of the above embodiment, charging tests were performed on the obtained different positive electrode lithium supplement materials (the coated weak organic solvents were all cyclohexane). The first cycle charging test results of different positive electrode lithium supplement materials at different voltage platforms are shown in Table 2 below.

[0085] Table 2

[0086]

[0087]

[0088] *: √ indicates that the specific capacity of the charging platform is greater than 50 mAh / g; × indicates that the specific capacity of the platform is not greater than 50 mAh / g.

[0089] It can be seen from Table 2 that the delithiation charging platforms of the positive electrode lithium replenishing material Li2CuO2 are: 3.1V, 3.2V, 4.1V; the delithiation charging platforms of the positive electrode lithium replenishing material Li2NiO2 are: 3.5V, 3.6V, 3.7V; 3.8V, 4.1V; the delithiation charging platforms of the positive electrode lithium replenishing material Li5FeO4 are: 3.3V, 3.9V, 4.0V; the delithiation charging platforms of the positive electrode lithium replenishing material Li6CoO4 are: 3.2V, 3.3V, 3.6V, 3.7V.

[0090] Test Example 3

[0091] According to the lithium replenishment method of the above embodiment, the performance of the positive electrode lithium replenishment material under different charging systems was tested, and the test results are shown in Table 3.

[0092] Among them, in Examples 5 to 9, the charging voltage range is 2.5 to 4.4V, and the specific charging process is: from the initial voltage of 2.5V, constant current charging with current A1 at temperature T1 until the voltage platform reaches 3.5V (Vp1), heating to T2, maintaining the voltage at 3.5V for constant voltage charging at temperature T2, and the current continues to decrease to current A2. Cool down to temperature T1, change to constant current charging with current A1 until the voltage platform reaches 3.6V (Vp2), heat up to T2, maintain the voltage at 3.6V for constant voltage charging at temperature T2 until the current drops to A2. Cool down to T1, constant current charging with current A1 until the voltage platform reaches 3.8V (Vp3), heat up to T2, maintain the voltage at 3.8V for constant voltage charging at temperature T2 until the current drops to A2. Cool down to T1, charge with constant current A1 until the voltage reaches 4.1V (Vp4), heat up to T2, keep the voltage at 4.1V at T2 for constant voltage charging until the current drops to A2. Cool down to T1, charge with constant current A1 until the cut-off voltage reaches 4.4V, and end the charging process.

[0093] Among them, in comparative examples 4-5, the specific charging process is: from the initial voltage of 2.5V, constant current charging is performed at a current A1 under a temperature T1 to a cut-off voltage of 4.4V.

[0094] Table 3

[0095]

[0096] b : The positive electrode active material is nickel, cobalt and manganese, and the content ratio is 80%:10%:10%.

[0097] As can be seen from Table 3, based on the first cycle charging conditions of the positive electrode lithium replenishment material, multiple lithium desorption voltage platforms are set, and the battery is charged in a step-by-step manner. The overall activation time of the battery (total charging time) is significantly reduced, which effectively improves the lithium desorption efficiency of the positive electrode lithium replenishment material. At the same time, the capacity of the positive electrode lithium replenishment material is further utilized, and the cycle performance is also improved.

[0098] Test Example 4

[0099] According to the lithium replenishment method of the above embodiment, the performance of different positive electrode lithium replenishment materials under different charging systems was tested, and the test results are shown in Table 4. Among them, the lithium desorption charging platform of Examples 10 to 15 is set according to the test results of Table 2. The charging voltage range is 2.5 to 4.4V. The test results are shown in Table 4 below.

[0100] Table 4

[0101]

[0102] It can be seen from Table 4 that the lithium replenishment method provided in this embodiment can be applied to a variety of positive electrode lithium replenishment materials, has good versatility, and is convenient for large-scale application.

[0103] The embodiments described above are part of the embodiments of the present invention, rather than all of the embodiments. The detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

Claims

1. A lithium-ion battery lithium replenishment method, characterized in that: include: S1, soaking the lithium supplement raw material in a weak polar organic solvent, adding a ball milling medium, and after ball milling, performing solid-liquid separation to obtain a positive electrode lithium supplement material; S2, obtaining a first-cycle charging curve of the positive electrode lithium supplementing material, and generating a plurality of lithium de-charging platforms according to the first-cycle charging curve; S3, mixing the positive electrode active material with the positive electrode lithium supplement material to obtain a battery positive electrode material, making the battery positive electrode material into a positive electrode sheet, and making a battery with the positive electrode sheet and the negative electrode sheet; S4, performing step-by-step multi-platform charging on the battery based on the lithium removal charging platform obtained in step S2 to remove lithium ions from the positive electrode lithium supplement material; Among them, step S4 includes: after entering the first de-lithium charging platform with a first current constant current charging under the first temperature condition, maintaining the voltage value unchanged, heating to the second temperature for constant voltage charging, until the current drops to the second current; cooling to the first temperature and entering the next de-lithium charging platform with the first current constant current charging, maintaining the voltage value unchanged, heating to the second temperature for constant voltage charging, until the current drops to the second current; repeating the above variable temperature charging process until charging to the last de-lithium charging platform; if the last de-lithium charging platform is not the target cut-off voltage, continuing to cool to the first temperature and charging with a constant current to the target cut-off voltage, wherein the second temperature is greater than the first temperature; the first temperature is 20 to 40°C, and the second temperature is 45 to 80°C.

2. The lithium replenishing method for lithium ion batteries according to claim 1, characterized in that: The weakly polar organic solvent includes one or more of isopentane, n-pentane, petroleum ether, hexane, cyclohexane, cyclopentane, heptane, carbon tetrachloride and trichlorotrifluoroethane.

3. The lithium replenishing method for a lithium ion battery according to claim 1, characterized in that: The ball-to-material ratio of the ball milling medium to the lithium supplementing raw material is 1 to 10:1, and the rotation speed of the ball mill is 50 to 500 rad / min.

4. The lithium replenishing method for lithium ion batteries according to claim 1, characterized in that: The lithium supplement raw material is selected from one or more of lithium metal, Li2NiO2, Li2CuO2, Li5FeO4, Li6CoO4 and Li6MnO4.

5. The lithium replenishing method for lithium ion batteries according to claim 1, characterized in that: In step S2, generating a plurality of lithium-removal charging platforms according to the first cycle charging curve includes: In the voltage interval of the first cycle charging curve, a preset voltage span is used as a voltage platform, and the voltage interval is divided into a plurality of voltage platforms; It is determined whether the specific capacity of the voltage platform is greater than a preset specific capacity threshold, and the voltage platform that meets the condition is calibrated as a lithium-depletion voltage platform.

6. The lithium replenishing method for lithium ion batteries according to claim 5, characterized in that: The voltage span is 0.1 to 0.5 V; the specific capacity threshold is 20 to 2000 mAh / g.

7. The lithium replenishment method for lithium-ion batteries according to claim 1, characterized in that: In step S3, the positive electrode active material is selected from one or more of lithium iron phosphate, lithium manganese oxide, lithium cobalt oxide, and nickel cobalt manganese.

8. The lithium replenishing method for lithium ion batteries according to claim 1, characterized in that: The current density of the first current is 10-50 mA / g; the current density of the second current is 1-5 mA / g.

9. The lithium replenishment method for lithium-ion batteries according to claim 1, characterized in that: In step S3, the weight percentage of the positive electrode lithium supplement material in the battery positive electrode material does not exceed 5%.

10. A lithium ion battery, characterized in that: Obtained according to the lithium replenishment method for lithium-ion batteries according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of lithium supplementing conductive slurry, lithium supplementing conductive paste, lithium ion battery and electronic equipment

    CN112447963A

  • Lithium supplement method for lithium ion battery

    CN113540591A

  • KR20190110345A