A sulfide solid electrolyte and its preparation method and application

By doping antimony and oxygen elements into the sulfide electrolyte, a sulfide solid electrolyte with high stability and high conductivity is prepared, which solves the problems of poor stability and low conductivity in the prior art, and realizes the organic solvent and Excellent performance in the air broadens its range of applications in lithium-ion batteries.

CN114597483BActive Publication Date: 2024-11-12SVOLT ENERGY TECH (WUXI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210266277.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-17
Publication Date
2024-11-12
Estimated Expiration
2042-03-17

AI Technical Summary

Technical Problem

The existing sulfide solid electrolytes have problems of poor stability and low conductivity, which limits their application in organic solvents and air.

Method used

By doping antimony and oxygen elements in the sulfide electrolyte, a sulfide solid electrolyte with excellent stability and high conductivity is prepared. The chemical formula is LiaSibSbcS5-xOx. The sulfur-silver germanium ore phase electrolyte is obtained by annealing and sintering treatment, which improves its Stability in organic solvents and air.

Benefits of technology

The high stability and high conductivity of sulfide solid electrolyte in organic solvents and air were achieved, the room temperature ion conductivity decreased by ≤15%, the dry room dew point decreased by ≤20%, and the lithium was expanded Application potential in ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114597483B_ABST
    Figure CN114597483B_ABST
Patent Text Reader

Abstract

The present invention provides a sulfide solid electrolyte and a preparation method and application thereof. The chemical formula of the sulfide solid electrolyte is Li a Si b Sb c S 5‑x O x I, where 6≤a≤7, 0.5≤b≤0.7, 0.3≤c≤0.5, 0
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium ion batteries and relates to a sulfide solid electrolyte and a preparation method and application thereof. Background Art

[0002] All-solid-state batteries use non-flammable inorganic solid electrolytes to replace traditional flammable, explosive and leaky organic electrolytes. They have inherent high safety characteristics. At the same time, metal negative electrode materials can be introduced to further improve the energy density of the battery. They are an important development direction for the next generation of high-energy-density batteries.

[0003] As a key part of all-solid-state batteries, sulfide solid electrolytes have high room temperature ionic conductivity and good interface contact with electrode materials, making them the most promising inorganic solid electrolytes. However, sulfide solid electrolytes are unstable to organic solvents, which is not conducive to the development of electrolyte wet coating processes. They are also easily decomposed in the air and have high environmental requirements for preparation, storage and transportation, which limits their further application.

[0004] CN113451638A discloses a sulfide solid electrolyte membrane and a solid lithium ion battery. The sulfide solid electrolyte membrane comprises a polymer membrane with a three-dimensional skeleton structure and a sulfide solid electrolyte material forming a continuous phase.

[0005] CN113745651A discloses a coated sulfide solid electrolyte and its preparation method and application. The coated sulfide solid electrolyte is a coated sulfide solid electrolyte in which an oxide solid electrolyte layer is coated on the surface of sulfide solid electrolyte particles. A specific oxide solid electrolyte is coated on the surface of a sulfide solid electrolyte to obtain a coated sulfide solid electrolyte.

[0006] The sulfide solid electrolyte provided by the above scheme has the problems of poor stability or low conductivity. Therefore, it is very necessary to develop a sulfide solid electrolyte with good stability and high conductivity. Summary of the invention

[0007] The object of the present invention is to provide a sulfide solid electrolyte and a preparation method and application thereof. The sulfide solid electrolyte of the present invention can improve its stability in organic solvents and air by doping antimony and oxygen elements in the electrolyte, and at the same time improve its conductivity.

[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a sulfide solid electrolyte, wherein the chemical formula of the sulfide solid electrolyte is Li a Si b Sb c S5-x O x I, where 6 ≤ a ≤ 7, for example: 6, 6.2, 6.6, 6.8 or 7, etc., 0.5 ≤ b ≤ 0.7, for example: 0.5, 0.55, 0.6, 0.65 or 0.7, etc., 0.3 ≤ c ≤ 0.5, for example: 0.3, 0.35, 0.4, 0.45 or 0.5, etc., 0 < x < 1, for example: 0.02, 0.1, 0.5, 0.8 or 0.9, etc., and the phase of the sulfide solid electrolyte is the argyrodite phase.

[0010] The sulfide solid electrolyte of the present invention has excellent stability against organic solvents (the organic solvents include any one or a combination of at least two of ethylene carbonate, fluoroethylene carbonate, ethyl methyl carbonate, dimethyl carbonate, N-methyl-2-pyrrolidone, tetrahydrofuran, ethylene glycol dimethyl ether, anisole, 1,3-dioxolane) and air. When soaked in the organic solvent at room temperature and 80 °C for 2 h, the ionic conductivity decreases by ≤ 15%. When exposed in a dry room with a dew point of -40 °C for 4 h, the ionic conductivity decreases by ≤ 20%.

[0011] Preferably, the conductivity of the sulfide solid electrolyte is 10 -3 ~1.2×10 -2 Scm -1 For example: 10 -3 Scm -1 、1.1×10 -3 Scm -1 、1.5×10 -3 Scm -1 、10 -2 Scm -1 or 1.2×10 -2 Scm -1 .

[0012] Preferably, the D50 of the sulfide solid electrolyte is 1 - 10 μm, for example: 1 μm, 2 μm, 5 μm, 8 μm or 10 μm, etc.

[0013] Preferably, the stable electrochemical window of the sulfide solid electrolyte is ≥ 5 V, for example: 5 V, 5.1 V, 5.2 V, 5.3 V or 5.4 V, etc.

[0014] In a second aspect, the present invention provides a method for preparing a sulfide solid electrolyte as described in the first aspect, and the preparation method includes the following steps:

[0015] Mix Li2S, LiI, a silicon source, an antimony source and an oxygen source, and obtain the sulfide solid electrolyte through annealing and sintering treatment.

[0016] The method of the present invention has simple process, widely available raw materials, controllable preparation process and high repeatability; the sulfide solid electrolyte prepared by the method has excellent stability to organic solvents and high room temperature lithium ion conductivity.

[0017] Preferably, the silicon source includes elemental silicon and / or silicon disulfide.

[0018] Preferably, the antimony source includes any one of Sb, Sb2S3 or Sb2S5, or a combination of at least two of them.

[0019] Preferably, the oxygen source includes any one of SiO2, Sb2O3 or Sb2O5, or a combination of at least two of them.

[0020] Preferably, the mixing method includes any one of manual grinding, mechanical stirring, mechanical shaking, ball milling or roller milling, or a combination of at least two of them, preferably ball milling and / or roller milling.

[0021] Preferably, the ball-to-material ratio of the ball mill is (1-60):1, for example: 1:1, 5:1, 10:1, 20:1, 40:1 or 60:1, etc.

[0022] Preferably, the rotation speed of the ball mill is 200-600 rpm, for example, 200 rpm, 300 rpm, 400 rpm, 500 rpm or 600 rpm.

[0023] Preferably, the ball milling time is 4 to 24 hours, for example: 4 hours, 8 hours, 12 hours, 16 hours, 20 hours or 24 hours.

[0024] Preferably, the atmosphere of the annealing and sintering treatment is any one of vacuum, argon or nitrogen, or a combination of at least two of them.

[0025] Preferably, the temperature of the annealing and sintering treatment is 400-600°C, for example, 400°C, 450°C, 500°C, 550°C or 600°C.

[0026] Preferably, the annealing and sintering treatment time is 1 to 48 hours, for example: 1 hour, 12 hours, 18 hours, 24 hours or 48 hours.

[0027] In a third aspect, the present invention provides a lithium-ion battery, wherein the lithium-ion battery comprises the sulfide solid electrolyte as described in the first aspect.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] (1) The sulfide solid electrolyte of the present invention has excellent stability to organic solvents and air. When immersed in an organic solvent at room temperature and 80°C for 2 hours, the ion conductivity decreases by ≤15%. When exposed to a dry room at a dew point of -40°C for 4 hours, the ion conductivity decreases by ≤20%.

[0030] (2) The sulfide solid electrolyte of the present invention has excellent lithium ion conductivity, and the conductivity at room temperature is 10 -3 ~1.2×10 -2 S cm -1 , particles are 2-5μm. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is the X-ray diffraction spectrum of the sulfide solid electrolyte described in Example 1.

[0032] Figure 2 This is a SEM image of the sulfide solid electrolyte described in Example 1.

[0033] Figure 3 This is a magnified SEM image of the sulfide solid electrolyte described in Example 1.

[0034] Figure 4 This is the room temperature AC impedance diagram of the sulfide solid electrolyte described in Example 1.

[0035] Figure 5 This is the room temperature AC impedance diagram of the sulfide solid electrolyte described in Comparative Example 2. DETAILED DESCRIPTION

[0036] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only used to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0037] Example 1

[0038] This embodiment provides a sulfide solid electrolyte, which is prepared by the following method:

[0039] Li2S, SiS2, SiO2, Sb2S5, and LiI were added to a roller mill in a molar ratio of 56:7:5:4:20, and zirconium oxide balls were added at a mass ratio of 10:1 to the raw materials. The mixture was mixed at 300 rpm for 24 hours to obtain a precursor powder. After mixing, the product was sintered at 550°C for 12 hours under an argon atmosphere to obtain the final product Li 6.6 Si 0.6 Sb 0.4 S 4.5 O 0.5I electrolyte, the electrochemical window of the electrolyte can reach 6 V. The physical phase of the sulfide solid electrolyte is argyrodite phase.

[0040] The X-ray diffraction spectrum of the sulfide solid electrolyte is as follows: Figure 1 shown.

[0041] The SEM image of the sulfide solid electrolyte is as follows: Figure 2-3 shown.

[0042] Example 2

[0043] This embodiment provides a sulfide solid electrolyte, which is prepared by the following method:

[0044] Li2S, SiS2, SiO2, Sb2S5, and LiI were added to a high-energy ball mill at a molar ratio of 56:9:3:4:20, and zirconium oxide balls were added at a ball-to-raw material mass ratio of 20:1. The mixture was mixed at 550 rpm for 12 hours to obtain a precursor powder. The product was sintered at 450 °C for 6 hours under vacuum to obtain the final product Li 6.6 Si 0.6 Sb 0.4 S 4.7 O 0.3 I electrolyte, the electrochemical window of the electrolyte can reach 5 V. The physical phase of the sulfide solid electrolyte is argyrodite phase.

[0045] Example 3

[0046] This embodiment provides a sulfide solid electrolyte, which is prepared by the following method:

[0047] Li2S, SiS2, SiO2, Sb2S5, and LiI were added into a mortar at a molar ratio of 56:5:7:4:20 and hand-grinded for 4 hours to obtain a precursor powder. The product was sintered at 500°C for 12 hours under a nitrogen atmosphere to obtain the final product Li 6.6 Si 0.6 Sb 0.4 S 4.3 O 0.7 I electrolyte. The physical phase of the sulfide solid electrolyte is argyrodite phase.

[0048] Example 4

[0049] The only difference between this embodiment and embodiment 1 is that the sintering temperature is 350° C., and the other conditions and parameters are exactly the same as those in embodiment 1.

[0050] Example 5

[0051] The only difference between this embodiment and embodiment 1 is that the sintering temperature is 650° C., and the other conditions and parameters are exactly the same as those in embodiment 1.

[0052] Comparative Example 1

[0053] The only difference between this comparative example and Example 1 is that no antimony source is added, and other conditions and parameters are exactly the same as those in Example 1.

[0054] Comparative Example 2

[0055] This comparative example provides a sulfide solid electrolyte, which is prepared by the following method:

[0056] Li2S, SiS2, Sb2S5, and LiI were added to a roller mill in a molar ratio of 14:3:1:5, and zirconium oxide balls were added at a mass ratio of 10:1 to the raw materials. The mixture was mixed at 300 rpm for 24 hours to obtain a precursor powder. The product was sintered at 550 °C for 12 hours under an argon atmosphere to obtain the final product Li 6.6 Si 0.6 Sb 0.4 S5I.

[0057] Performance Testing:

[0058] (1) The sulfide solid electrolytes obtained in Examples 1-5 and Comparative Examples 1-2 were tested for their electrical conductivity. After the test, they were immersed in a mixed solvent of tetrahydrofuran and anisole, respectively, and dried after being immersed for 2 h at room temperature and 80° C. After being immersed, their electrical conductivity was tested. After the obtained sulfide solid electrolytes were exposed to a dry room with a dew point of -40° C. for 4 h, their electrical conductivity was tested. The test results are shown in Table 1:

[0059] Table 1

[0060]

[0061]

[0062] As can be seen from Table 1, from Examples 1-5, the initial conductivity of the sulfide solid electrolyte of the present invention can reach 7.4 mS cm -2 As mentioned above, with the doping of a certain proportion of oxygen elements, the conductivity of electrolyte lithium ions is improved. At the same time, the sintering temperature has a greater impact on the conductivity.

[0063] By comparing Example 1 with Examples 4-5, it can be seen that in the preparation process of the sulfide solid electrolyte of the present invention, the temperature of the annealing and sintering treatment will affect the performance of the obtained sulfide solid electrolyte. The temperature of the annealing and sintering treatment is controlled at 400-600°C, and the performance of the obtained sulfide solid electrolyte is better. If the temperature of the annealing and sintering treatment is too low, the component phases cannot be fully melted for solid phase reaction. If the temperature of the annealing and sintering treatment is too high, the ceramic phase is obvious, the grain boundary impedance becomes significantly larger, and it is not conducive to lithium ion conduction.

[0064] From the comparison between Example 1 and Comparative Example 1, it can be seen that the doping of antimony element in the sulfide solid electrolyte in the present invention is beneficial to broadening the lithium ion transmission channel and greatly improving the lithium ion transmission capacity.

[0065] From the comparison between Example 1 and Comparative Example 2, it can be seen that the present invention dopes oxygen into the sulfide solid electrolyte, and mixes oxygen and sulfur, which is beneficial to lithium ion conduction.

[0066] (2) The thickness and impedance of the sulfide solid electrolyte obtained in Example 1 after exposure to an organic solvent or air were measured. The test results are shown in Table 2:

[0067] Table 2

[0068] Processing Thickness(cm) Impedance(Ω) initial 0.1 11.6 Soak in organic solvent at room temperature 0.099 13.0 80℃ organic solvent immersion 0.141 13.4 Exposure in dry room with dew point -40℃ 0.1 13.6

[0069] It can be seen from Table 2 that the sulfide solid electrolyte of the present invention has relatively good solvent stability and environmental stability in the air. After being immersed in an organic solvent for 2 hours, the impedance is ≤13.4Ω. In the test of exposure to a dry room dew point of -40°C for 4 hours, the impedance of the solid electrolyte material is ≤13.6Ω.

[0070] The room temperature AC impedance diagram of the sulfide solid electrolyte described in Example 1 is as follows Figure 4 As shown, the room temperature AC impedance diagram of the sulfide solid electrolyte described in Comparative Example 2 is as follows Figure 5 As shown by Figure 4 and Figure 5 It can be seen that after the material is doped and modified, both the initial conductivity and the solvent stability and air stability are greatly improved and enhanced.

[0071] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A sulfide solid electrolyte, characterized in that: The chemical formula of the sulfide solid electrolyte is Li a Si b Sb c S 5-x O x I, wherein 6≤a≤7, 0.5≤b≤0.7, 0.3≤c≤0.5, 0.5≤x≤0.7, and the physical phase of the sulfide solid electrolyte is argyrodite phase; The oxygen in the chemical formula is provided by the following oxygen source, which includes any one or a combination of at least two of SiO2, Sb2O3 or Sb2O5; The initial conductivity of the sulfide solid electrolyte is ≥7.4 mS cm -1 ; The sulfide solid electrolyte is immersed in an organic solvent at room temperature and 80° C. for 2 hours, and the ionic conductivity decreases by ≤15%; the organic solvent comprises any one of ethylene carbonate, fluoroethylene carbonate, ethyl methyl carbonate, dimethyl carbonate, N-methyl-2-pyrrolidone, tetrahydrofuran, ethylene glycol dimethyl ether, anisole, and 1,3-oxycyclopentane, or a combination of at least two thereof; The sulfide solid electrolyte is exposed to a dry room dew point of -40°C for 4 hours, and the ion conductivity decreases by ≤20%.

2. The sulfide solid electrolyte according to claim 1, characterized in that The D50 of the sulfide solid electrolyte is 1 to 10 μm.

3. The sulfide solid electrolyte according to claim 1, characterized in that The stable electrochemical window of the sulfide solid electrolyte is ≥5V.

4. A method for preparing the sulfide solid electrolyte according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: Li2S, LiI, a silicon source, an antimony source and an oxygen source are mixed, and the sulfide solid electrolyte is obtained by annealing and sintering.

5. The preparation method according to claim 4, characterized in that: The silicon source includes elemental silicon and / or silicon disulfide.

6. The preparation method according to claim 4, characterized in that: The antimony source includes any one of Sb, Sb2S3 or Sb2S5 or a combination of at least two of them.

7. The preparation method according to claim 4, characterized in that: The mixing method includes any one of manual grinding, mechanical stirring, mechanical shaking, ball milling or roller milling, or a combination of at least two of them.

8. The preparation method according to claim 7, characterized in that: The mixing method includes ball milling and / or roller milling.

9. The preparation method according to claim 8, characterized in that: The ball-to-material ratio of the ball mill is (1-60):

1.

10. The preparation method according to claim 8, characterized in that: The rotation speed of the ball mill is 200-600 rpm.

11. The preparation method according to claim 8, characterized in that: The ball milling time is 4 to 24 hours.

12. The preparation method according to claim 4, characterized in that: The atmosphere of the annealing and sintering treatment is any one of vacuum, argon or nitrogen, or a combination of at least two of them.

13. The preparation method according to claim 4, characterized in that: The temperature of the annealing and sintering treatment is 400-600°C.

14. The preparation method according to claim 4, characterized in that: The annealing and sintering treatment time is 1 to 48 hours.

15. A lithium ion battery, characterized in that: The lithium-ion battery comprises the sulfide solid electrolyte according to any one of claims 1 to 3.