Environmentally friendly infrared light transmitting glass composition and optical glass manufacturing method using the same
By mixing Ge, Ga and Se in a specific ratio and treating it at high temperature, infrared light-transmitting glass without heavy metals is prepared, which solves the environmental protection and optical property problems caused by heavy metal components in the existing technology and achieves excellent optical and physical properties.
Patent Information
- Application Number
- CN202180006116.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-10
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-09-10
AI Technical Summary
Existing infrared optical glass contains harmful heavy metal components such as arsenic (As) and antimony (Sb), which pose environmental protection and optical property problems during the manufacturing and use processes.
Infrared light-transmitting glass without heavy metals is prepared by mixing materials such as Ge, Ga and Se in specific proportions, melting them at high temperatures and cooling them slowly, ensuring the optical properties of the optical glass.
An environmentally friendly infrared light-transmitting glass that does not contain heavy metals has been realized, has excellent optical properties and physical properties, and is suitable for infrared cameras and other electronic equipment.
Smart Images

Figure CN114599618B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a composition for infrared light transmitting glass which does not contain harmful raw materials such as As or Sb in chalcogen elements and a method for manufacturing optical glass using the same. Background Art
[0002] The content described in this section merely provides background information for one embodiment of the present invention and does not constitute prior art.
[0003] Infrared cameras have been mainly used for special purposes such as night vision goggles in the military field, but they are also gradually being used in civilian fields such as night vision for vehicles, biometrics, and fire monitoring. In particular, the recent commercialization of modular infrared cameras that can be installed on smartphones has raised the possibility that infrared cameras will be applicable to various electronic devices and daily life.
[0004] Infrared cameras are divided into mid-infrared band (3μm to 5μm) cameras and far-infrared band (8μm to 12μm) cameras. Infrared cameras are devices that visualize the wavelengths emitted by objects as they change temperature as thermal images based on the principle of blackbody radiation. Mid-infrared cameras visualize wavelengths emitted from high-temperature objects such as fires, while far-infrared cameras visualize the peak wavelength (~10μm) of the blackbody radiation spectrum emitted from the body temperature of warm-blooded animals.
[0005] The infrared camera includes a lens made of an optical glass material that transmits infrared light. The lens focuses the infrared light so that the sensor in the infrared camera can sense the infrared light.
[0006] The raw materials of existing optical glass that transmits infrared light contain arsenic (As) and antimony (Sb) as heavy metal components. In the past, sufficient optical properties (for example, refractive index, dispersion, or the amount of change in refractive index with temperature, etc.) could be ensured only if these components were included in the raw materials of existing optical glass. However, since the heavy metal components are included in the raw materials, problems may occur due to the heavy metal components in various processes such as the manufacturing process, the process of using optical parts containing the raw materials, or the process of post-processing optical parts whose service life has expired. Summary of the invention
[0007] (Problems to be solved by the invention)
[0008] An object of one embodiment of the present invention is to provide an environmentally friendly infrared light transmitting glass composition that does not contain harmful raw materials such as As (arsenic) or Sb (antimony) and a method for manufacturing optical glass using the same.
[0009] Another object of one embodiment of the present invention is to provide an environmentally friendly infrared light-transmitting glass composition having sufficient optical properties even without containing heavy metal components, and a method for producing optical glass using the same.
[0010] (Measures taken to solve the problem)
[0011] According to one aspect of the present invention, there is provided a method for manufacturing an optical glass, which manufactures an optical glass that transmits light in the infrared band above a set reference value, and the optical glass manufacturing method is characterized in that it includes: a loading process of mixing Ge, Ga and Se in set contents respectively into a set container; a melting process of melting the set container under a first set environment; and a slow cooling process of slowly cooling the container that has undergone the melting process under a second set environment.
[0012] According to one aspect of the present invention, the optical glass manufacturing method is characterized in that, during the above-mentioned loading process, 50 to 70 mol% of Se and 30 to 50 mol% of Ge and Ga are loaded into the above-mentioned set container, and Ge and Ga are loaded in the range of 3 to 15:1 respectively.
[0013] According to one aspect of the present invention, the optical glass manufacturing method is characterized in that, in the melting process, the predetermined container is melted at a temperature of 900 to 1000° C. for a predetermined time while being shaken.
[0014] According to one aspect of the present invention, the optical glass manufacturing method is characterized in that the set time is 12 hours.
[0015] According to one aspect of the present invention, the optical glass manufacturing method is characterized in that, in the slow cooling process, the container that has undergone the melting process is slowly cooled at a glass transition temperature for a set time.
[0016] According to one aspect of the present invention, the optical glass manufacturing method is characterized in that the set time is 3 hours.
[0017] According to one aspect of the present invention, there is provided a glass composition, which is a glass composition that transmits light in the infrared band to a set reference value or above, and the glass composition is characterized in that it includes Ge, Ga and Se, wherein the content of Ge is 22.5 to 46.875 mol%, the content of Ga is 1.875 to 12.5 mol%, and the content of Se is 50 to 70 mol%.
[0018] According to one aspect of the present invention, there is provided a method for manufacturing an optical glass, which manufactures an optical glass that transmits light in the infrared band above a set reference value, and the optical glass manufacturing method is characterized in that it includes: a loading process of mixing Ge, Ga, Se and Te in set contents respectively and loading them into a set container; a melting process of melting the set container under a first set environment; and a slow cooling process of slowly cooling the container that has undergone the melting process under a second set environment.
[0019] According to one aspect of the present invention, the optical glass manufacturing method is characterized in that, during the above-mentioned loading process, x mol% Te and (50-x) to (70-x) mol% Se are loaded into the above-mentioned set container and 30 to 50 mol% Ge and Ga are loaded, and Ge and Ga are loaded in the range of 3 to 15:1 respectively.
[0020] According to one aspect of the present invention, the optical glass manufacturing method is characterized in that the amount of Te charged into the predetermined container is 1 to 7 mol%.
[0021] According to one aspect of the present invention, the optical glass manufacturing method is characterized in that, in the melting process, the predetermined container is melted at a temperature of 900 to 1000° C. for a predetermined time.
[0022] According to one aspect of the present invention, there is provided a glass composition, which is a glass composition that transmits light in the infrared band to a set reference value or above, and the glass composition is characterized in that it includes Ge, Ga, Se and Te, wherein the content of Ge is 22.5 to 46.875 mol%, the content of Ga is 1.875 to 12.5 mol%, the content of Se is 43 to 69 mol%, and the content of Te is 1 to 7 mol%.
[0023] According to one aspect of the present invention, there is provided a method for manufacturing an optical glass, which manufactures an optical glass that transmits light in the infrared band above a set reference value, and the optical glass manufacturing method is characterized in that it includes: a loading process of mixing Ge, Ga, Se and S in set contents respectively and loading them into a set container; a melting process of melting the set container under a first set environment; and a slow cooling process of slowly cooling the container that has undergone the melting process under a second set environment.
[0024] According to one aspect of the present invention, the optical glass manufacturing method is characterized in that, during the above-mentioned loading process, x mol% Te and (50-x) to (70-x) mol% Se are loaded into the above-mentioned set container and 30 to 50 mol% Ge and Ga are loaded, and Ge and Ga are loaded in the range of 3 to 15:1 respectively.
[0025] According to one aspect of the present invention, the optical glass manufacturing method is characterized in that the amount of S charged into the predetermined container is 10 to 50 mol%.
[0026] According to one aspect of the present invention, there is provided a glass composition, which is a glass composition that transmits light in the infrared band to a set reference value or above, and the glass composition is characterized in that it includes Ge, Ga, Se and S, wherein the content of Ge is 22.5 to 46.875 mol%, the content of Ga is 1.875 to 12.5 mol%, the content of Se is 10 to 57.5 mol%, and the content of S is 2.5 to 50 mol%.
[0027] According to one aspect of the present invention, there is provided a glass composition that transmits light in the infrared band at a set reference value or more, wherein the glass composition contains Ge, Ga, and Se at a set content, or contains Te or S at a set content in Ge, Ga, and Se, and does not contain heavy metal components such as As (arsenic), Sb (antimony), Pb (lead), Br (bromine), or La (lanthanum).
[0028] (Effects of the Invention)
[0029] As described above, according to one aspect of the present invention, since the heavy metal component is not contained, it has the advantage of being environmentally friendly.
[0030] According to one aspect of the present invention, there is an advantage that the optical component does not contain any heavy metal components and can have sufficient optical properties for use as an optical component. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 is a flow chart illustrating a method of manufacturing a far-infrared light transmitting optical glass according to one embodiment of the present invention.
[0032] Figure 2 : is a ternary diagram illustrating the contents of components constituting the composition for far-infrared light transmitting glass according to the first embodiment of the present invention.
[0033] FIG. 3 is a diagram illustrating an optical glass prepared using the composition according to the first embodiment of the present invention.
[0034] Figure 4 This is a graph showing the measurement of internal defects of an optical glass prepared using the composition according to the first example of the present invention.
[0035] Figure 5 : is a graph illustrating characteristics for confirming the vitrification of the composition according to the first example of the present invention.
[0036] Figure 6 is a graph illustrating the transmittance of the composition according to the first embodiment of the present invention in the far infrared light band.
[0037] Figure 7 is a graph illustrating the coefficient of thermal expansion of the composition according to the first embodiment of the present invention.
[0038] Figure 8 and Fig. 9 is a graph illustrating thermal characteristics and glass transition temperature of the composition according to the first embodiment of the present invention with temperature.
[0039] Fig.10 is a graph illustrating the hardness of the composition according to the first embodiment of the present invention.
[0040] Fig.11 is a graph illustrating the refractive index of the composition according to the first embodiment of the present invention.
[0041] Fig.12 and Fig.13 is a graph illustrating changes in the refractive index of the composition according to the first embodiment of the present invention with temperature and wavelength.
[0042] Fig.14 : is a graph showing the contents of components constituting the composition for far-infrared light transmitting glass according to the second embodiment of the present invention.
[0043] FIG. 15 is a diagram illustrating an optical glass prepared using a composition according to a second embodiment of the present invention.
[0044] Fig.16 This is a diagram showing the measurement of internal defects of an optical glass prepared using the composition according to the second example of the present invention.
[0045] Fig.17 : is a graph illustrating characteristics for confirming the vitrification of the composition according to the second example of the present invention.
[0046] Fig.18 is a graph illustrating the transmittance of the composition according to the second embodiment of the present invention in the far infrared light band.
[0047] Fig.19 is a graph illustrating the coefficient of thermal expansion of a composition according to a second embodiment of the present invention.
[0048] Fig. 20 and Fig.21 is a graph illustrating thermal characteristics and glass transition temperature of a composition according to a second embodiment of the present invention according to temperature.
[0049] Fig. 22 is a graph illustrating the hardness of a composition according to a second embodiment of the present invention.
[0050] Fig.23 is a graph illustrating the refractive index of a composition according to a second embodiment of the present invention.
[0051] Fig.24 is a graph illustrating dispersion values of a composition according to a second embodiment of the present invention.
[0052] Fig.25 : is a graph showing the contents of components constituting the composition for far-infrared light transmitting glass according to the third embodiment of the present invention.
[0053] FIG. 26 is a diagram illustrating an optical glass prepared using the composition according to the third embodiment of the present invention.
[0054] Fig. 27 This is a graph showing the measurement of internal defects of an optical glass prepared using the composition according to the third example of the present invention.
[0055] Fig.28 : is a graph illustrating characteristics for confirming the vitrification of the composition according to the third example of the present invention.
[0056] Fig.29 and Fig.30 is a graph illustrating the transmittance of the composition according to the third embodiment of the present invention in the far infrared light band.
[0057] Fig.31 is a graph illustrating the coefficient of thermal expansion of a composition according to a third embodiment of the present invention.
[0058] Fig.32 and Fig.33 is a graph illustrating thermal characteristics and glass transition temperature of a composition according to a third embodiment of the present invention according to temperature.
[0059] Fig.34 is a graph illustrating the hardness of a composition according to a third embodiment of the present invention.
[0060] Fig.35 is a graph illustrating the refractive index of a composition according to a third embodiment of the present invention.
[0061] Fig.36is a graph illustrating dispersion values of a composition according to a third embodiment of the present invention. DETAILED DESCRIPTION
[0062] The present invention is capable of various modifications and various embodiments, and therefore specific embodiments are illustrated in the drawings and described in detail. However, this is not intended to limit the present invention to specific embodiments, but should be understood to include all modifications, equivalents or substitutes that fall within the concept and technical scope of the present invention. In describing the drawings, similar reference numerals are used for similar components.
[0063] The terms first, second, A, B, etc. can be used to describe a variety of components, but the above components shall not be limited to the above terms. The above terms are only used to distinguish one component from other components. For example, without departing from the scope of the present invention, the first component can be named as the second component, and similarly, the second component can also be named as the first component. The term "and / or" includes a combination of multiple related and recorded items or one of multiple related and recorded items.
[0064] When it is mentioned that a certain component is "connected" or "joined" to another component, it is possible that the component is directly connected or joined to the other component, but it should be understood that there may be other components between the two. On the contrary, when it is mentioned that a certain component is "directly connected" or "directly joined" to another component, it should be understood that there are no other components between the two.
[0065] The terms used in this application are only used to illustrate specific embodiments and are not intended to limit the present invention. Singular expressions include plural expressions unless there is a clear difference in meaning in the context. In this application, the terms "including" or "having" should be understood as not excluding in advance the existence or additional possibility of features, numbers, steps, actions, constituent elements, parts or their combinations recorded in the specification.
[0066] Unless otherwise defined, all terms used herein including technical or scientific terms have the same meanings as commonly understood by one of ordinary skill in the art.
[0067] Terms as defined in commonly used dictionaries should be interpreted as having meanings consistent with the meanings given by the context of the relevant art, and shall not be ideally or excessively interpreted into formal meanings unless explicitly defined in this application.
[0068] In addition, each configuration, process, step, method, etc. included in each embodiment of the present invention can be shared within the scope of no technical contradiction.
[0069] Figure 1 is a flow chart illustrating a method of manufacturing a far-infrared light transmitting optical glass according to one embodiment of the present invention.
[0070] The glass composition is manufactured into a far-infrared light transmitting optical glass through the following preparation process. The far-infrared light transmitting glass has a transmittance of more than a set reference value for the light in the far-infrared band of the incident light. The far-infrared light transmitting glass can be used not only in the military field, but also in the civilian field in various ways such as being built into infrared cameras, smart devices or home appliances. At this time, the far-infrared light transmitting glass can be used as glass itself so that it can be used in various fields, but in more cases, it is used by molding optical parts such as lenses from glass. Therefore, the raw materials forming the far-infrared light transmitting glass composition according to one embodiment of the present invention are mixed in a set ratio and go through the following preparation process, so that even if it does not contain heavy metals or harmful elements such as As (arsenic), Sb (antimony), Pb (lead), Br (bromine) or La (lanthanum), it can be made into a far-infrared light transmitting optical glass that ensures excellent optical properties and physical properties.
[0071] The set raw materials are mixed at set contents and loaded into the set containers (S110).
[0072] The raw materials constituting the glass composition include a main component and a dopant. The main component is a component that must be included in order to make the raw material into a far-infrared light transmitting glass composition or a far-infrared light transmitting glass. As the main components, Ge (germanium), Ga (gallium) and Se (selenium) are included. The content of Se is 50 to 70 mol%, and the remaining content contains Ge and Ga in a set ratio of mol%. Here, the set ratio of Ge and Ga can be 3 to 15:1. For example, when the content of Se is 60 mol%, the content of Ge can be 30 to 37.5 mol%, and the content of Ga can be 2.5 to 10 mol%. The selected components are included as the main components of the raw materials in the above-mentioned contents, so that the glass forming area can be ensured. In addition, when the content of each selected component is appropriately adjusted, the far-infrared light lens that does not contain any heavy metals can ensure excellent optical properties such as far-infrared light transmittance or refractive index.
[0073] As the raw material constituting the glass composition, a dopant may be further included together with the main component. The dopant is a component included together with the raw material to improve specific optical properties such as refractive index or dispersion while maintaining other optical properties of the optical glass to be manufactured. Te (tellurium) or S (sulfur) may be included as a dopant. Depending on the amount of the dopant included, the content of Se is reduced accordingly. For example, as in the example described above, when the content of Se is 60 mol%, the content of Se is 55 mol% when the content of Te is 5 mol%. In this way, by further including a dopant, it is possible to have better optical properties in terms of refractive index or dispersion.
[0074] The raw materials including the main component or the main component and the dopant are mixed and placed in a predetermined container. The predetermined container may be a quartz tube, and the raw materials are mixed and placed in a container such as a quartz tube. Once the raw materials are placed, the predetermined container is sealed in a vacuum state. If it is not in a vacuum state, the raw materials may be combined with oxygen in the atmosphere, and the properties of the raw materials may change. Therefore, the raw materials are placed in a predetermined container and sealed in a vacuum state.
[0075] The container filled with the raw material is exposed to a first set environment (S120).
[0076] The quartz tube is exposed to a first set environment. Here, the first set environment may be an environment exposed to a temperature of 900 to 1000° C. for about 12 hours. The quartz tube is placed in a device such as a lock electric furnace and exposed to a temperature of 900 to 1000° C., so that various raw materials in the quartz tube are melted.
[0077] The container in which the raw material has been melted is slowly cooled under the second set environment ( S130 ).
[0078] The quartz tube is slowly cooled under the second set environment. Here, the second set environment can be an environment exposed to the glass transition temperature for about 3 hours. The glass transition temperature varies with the characteristics of the raw materials, and the quartz tube is slowly cooled under the glass transition temperature determined by the raw materials loaded into the quartz tube. The raw materials in the quartz tube are slowly cooled under the glass transition temperature for about 3 hours, thereby producing a far-infrared light transmitting optical glass.
[0079] Figure 2 : is a ternary diagram illustrating the contents of components constituting the composition for far-infrared light transmitting glass according to the first embodiment of the present invention.
[0080] The composition for far-infrared light-transmitting glass according to the first embodiment of the present invention (hereinafter, simply referred to as “first composition”) refers to a composition containing the following raw materials.
[0081] 1) Ge: 37.5 mol%, Ga: 2.5 mol%, Se: 60 mol% (210)
[0082] 2) Ge: 35 mol%, Ga: 5 mol%, Se: 60 mol% (220)
[0083] 3) Ge: 32.5 mol%, Ga: 7.5 mol%, Se: 60 mol% (230)
[0084] 4) Ge: 30 mol%, Ga: 10 mol%, Se: 60 mol% (240)
[0085] The content of Se is 60 mol% in a range of 50 to 70 mol%, and Ge and Ga are contained in a ratio of 3:1 (240) to 15:1 (210) in a range of 40 mol%.
[0086] FIG. 3 schematically shows an optical glass prepared using a first composition containing each raw material only in the aforementioned content.
[0087] Fig. 3 is a diagram illustrating an optical glass prepared with a composition according to a first embodiment of the present invention. Here, the manufactured optical glass can be grown to have a diameter having a set reference value, for example, grown to have a diameter of more than 35 mm and have an ingot form. The optical glass prepared with the composition according to the first embodiment of the present invention grows and can also have a diameter of up to 60 mm.
[0088] Figure 3a to Figure 3d The glass embodied with each first composition (210 to 240) is shown. Figure 3a to Figure 3d It can be confirmed that each of the first compositions did not undergo crystallization during the process of being specifically realized as glass.
[0089] Figure 4 This is a diagram showing the measurement of internal defects of an optical glass prepared using the composition according to the first example of the present invention.
[0090] Figure 4 a to Figure 4 d is a photograph showing the internal defects of optical glasses 210 to 240. In order to measure the internal defects, far-infrared light is irradiated to the manufactured optical glass. When there are no internal defects, the transmittance of far-infrared light is excellent, so the central black part is photographed lightly. On the contrary, when there are internal defects, the transmittance of far-infrared light is reduced, so the central black part is photographed relatively darkly. Figure 4 a to Figure 4c, it can be confirmed that the optical glasses 210 to 230 have no defects inside, and thus have excellent far-infrared light transmittance. Figure 4 d, it can be confirmed that although the optical glass 240 is relatively inferior, it is excellent in far-infrared light transmittance.
[0091] Figure 5 : is a graph illustrating characteristics for confirming the vitrification of the composition according to the first example of the present invention.
[0092] Figure 5 The graph of is a graph illustrating the characteristics when each first composition is embodied as a 35 mm optical glass. It can be confirmed that the optical glasses 210 to 240 are all vitrified and no crystallization peak (Peak) is found at all angles. That is, each optical glass embodied from the first composition does not crystallize inside, so it can be confirmed that it can have excellent far-infrared light transmittance.
[0093] Figure 6 is a graph illustrating the transmittance of the composition according to the first embodiment of the present invention in the far infrared light band.
[0094] Figure 6 The graph of is a graph illustrating the characteristics when each first composition is specifically implemented as a 4 mm optical glass. It can be confirmed that each optical glass 210 to 240 has an average transmittance of 60% or more in the 8 to 12 μm band, which is a far-infrared light band. More specifically, optical glass 210 shows an average transmittance of 61.87%, optical glass 220 shows an average transmittance of 64.54%, optical glass 230 shows an average transmittance of 64.40%, and optical glass 240 shows an average transmittance of 63.98%.
[0095] The decrease in the transmittance of far-infrared light in the 12μm band is caused by the combination of Ge and O. It can be confirmed that Ge decreases relatively with the increase of Ga, resulting in a decrease in transmittance.
[0096] Figure 7 is a graph illustrating the coefficient of thermal expansion of the composition according to the first embodiment of the present invention.
[0097] Each of the optical glasses 210 to 240 also shows a relatively low change in the coefficient of thermal expansion at a temperature change of approximately 350°C. If the coefficient of thermal expansion changes sharply with temperature, the shape of the optical glass changes with temperature. If it is just glass, the effect on the shape change will be relatively small, but if the glass is made into an optical structure, the optical properties of the optical structure may change. Each of the optical glasses 210 to 240 has a relatively low coefficient of thermal expansion of 12.9531×10 -6 K, 12.8806×10-6 K, 12.3196×10 -6 K, 12.5219×10 -6 K, but no tendency related to the change in the content of the components is shown. This is more obvious when compared with the thermal expansion coefficient of the existing far-infrared light transmitting glass (containing heavy metals) sold on the market. Among the existing far-infrared light transmitting glasses (containing heavy metals), the product with excellent thermal expansion coefficient is 12.5×10 -6 K (Schott (Germany Schott) IRG 22), in addition, the product with excellent thermal expansion coefficient also has 14.0×10 -6 K (Schott (Germany) IRG 25), 20.0×10 -6 K (Schott (Germany) IRG24) or 21.4×10 -6 K (IRG26 of Schott (Germany) Co., Ltd.), etc. Referring to this, it can be confirmed that each of the optical glasses 210 to 240 has an excellent thermal expansion coefficient.
[0098] Figure 8 and Fig. 9 is a graph illustrating thermal characteristics and glass transition temperature of the composition according to the first embodiment of the present invention with temperature.
[0099] Figure 8 This is a graph obtained by performing TG-DTA thermal analysis on each of the optical glasses 210 to 240. Figure 8 and Fig. 9 The optical glasses 210 to 240 have glass transition temperatures of 325.1° C., 317.3° C., 317.9° C., and 316.9° C., respectively. As the Ga content in the raw materials forming the optical glass increases, the glass transition temperature shows a tendency to decrease. This is due to the connection loss of the network and the decrease in the bond strength between Ga and Se.
[0100] Fig.10 is a graph illustrating the hardness of the composition according to the first embodiment of the present invention.
[0101] Hardness is a property that shows the physical characteristics of optical glass, and it can determine how tough it is to be scratched by external forces. Existing (heavy metal-containing) far-infrared light-transmitting optical glasses sold on the market have an average hardness of 150 to 155 HK. In contrast, optical glasses 210 to 240 all have an excellent hardness of more than 170 HK, and it can be confirmed that the higher the Ga content, the higher the hardness, based on the Ga content of 5 mol%.
[0102] Fig.11 is a graph illustrating the refractive index of the composition according to the first embodiment of the present invention.
[0103] Fig.11 The graph is a graph showing the refractive index of the optical glass 220 and the optical glass 240 measured at every 1 μm interval within the wavelength range of 3 to 12 μm.
[0104] The two optical glasses 220 and 240 have a refractive index in the range of 2.50 to 2.52 in the far infrared light band (8 to 12 μm), and both have a refractive index of more than 2.4. The two optical glasses 220 and 240 have refractive indices of 2.50706 and 2.51320 in the 10 μm band, respectively, and dispersion values of 92.63 and 87.07 in the 8 to 12 μm band, respectively, and can be confirmed to have low dispersion characteristics.
[0105] Fig.12 and Fig.13 is a graph illustrating changes in the refractive index of the composition according to the first embodiment of the present invention with temperature and wavelength.
[0106] Fig.12 is a graph illustrating how the refractive index of the optical glass 220 changes with temperature for light in the wavelength bands of 4 μm and 10 μm. Fig.13 2 is a graph illustrating the change of the refractive index of the optical glass 240 with respect to light in the wavelength bands of 4 μm and 10 μm, depending on the temperature.
[0107] Even though the external temperature of the optical glass changes within the range of -40 to 120° C., the refractive index of the two optical glasses 220 and 240 remains at a change of about 0.28 to 0.4%. That is, it can be confirmed that the refractive index of the two optical glasses 220 and 240 is strong against temperature change.
[0108] In addition, it was confirmed that the optical glass 220 had a dn / dT value of 63.6×10 -6 K, optical glass 240 has a dn / dT value of 63.6×10 -6 K. If we refer to the existing (heavy metal-containing) far-infrared light transmitting glass sold on the market, the dn / dT value is 61.1×10 -6 K (Schott (Germany) IRG 25) to 67.1×10 -6 K (Schott IRG 22), it can be confirmed that there is almost no difference from the commercialized product.
[0109] With reference to the various data described above, it can be confirmed that the optical glasses 210 to 240 prepared using the first composition ensure excellent physical properties (hardness), excellent refractive index and dispersion values, and normal glass transition temperature and transmittance despite not containing heavy metals.
[0110] Fig.14 : is a graph showing the contents of components constituting the composition for far-infrared light transmitting glass according to the second example of the present invention.
[0111] The composition for far-infrared light-transmitting glass according to the second embodiment of the present invention (hereinafter, simply referred to as “second composition”) refers to a composition containing the following raw materials.
[0112] 1) Ge: 35 mol%, Ga: 5 mol%, Se: 60 mol% (220)
[0113] 2) Ge: 35 mol%, Ga: 5 mol%, Se: 59 mol%, Te: 1 mol% (GGSe-1Te)
[0114] 3) Ge: 35 mol%, Ga: 5 mol%, Se: 57 mol%, Te: 3 mol% (GGSe-3Te)
[0115] 4) Ge: 35 mol%, Ga: 5 mol%, Se: 55 mol%, Te: 5 mol% (GGSe-5Te)
[0116] 5) Ge: 35 mol%, Ga: 5 mol%, Se: 53 mol%, Te: 7 mol% (GGSe-7Te)
[0117] The content of Te is x mol%, the content of Se is (60-x) mol%, and Ge and Ga are contained in a ratio of 7:1 within 40 mol%. At this time, with respect to the content (x) of Te, 1 to 7 mol% may be contained. In the case where Te is contained as a dopant, the refractive index of the optical glass prepared with the second composition is increased. In the case where the refractive index is increased, the focusing power of the incident light is increased, thereby being able to reduce chromatic aberration. In addition, in the case where the optical glass is processed into an optical composition, the number of optical compositions included in a particular device is reduced due to the high refractive index.
[0118] However, the raw material content of the second composition described above is only an example for illustrating the characteristics of the optical glass prepared by the second composition to be described below, and is not necessarily limited to the content described above. As described in the first composition, Te and Se can have a content of 50 to 70 mol%, and Ga and Ga can be contained in the remaining content except the Se content at a ratio of 3 to 15:1. For convenience, the second composition (220, GGSe-1Te, GGSe-3Te, GGSe-5Te, GGSe-7Te) with the ratio described above is used as a reference for the following description, but it is not necessarily limited to this.
[0119] FIG. 15 schematically shows an optical glass prepared using the second composition containing the respective raw materials in the aforementioned contents.
[0120] Fig. 15 is a diagram illustrating an optical glass prepared with a composition according to a second embodiment of the present invention. Here, the optical glass produced can be grown to a diameter having a set reference value, for example, grown to have a diameter of more than 35 mm and have an ingot form. The optical glass prepared with the composition according to the second embodiment of the present invention grows and can also have a diameter of up to 60 mm.
[0121] Figures 15a to 15d The figure shows the glasses embodied by the second compositions (GGSe-1Te, GGSe-3Te, GGSe-5Te, GGSe-7Te). Figures 15a to 15d It can be confirmed that each second composition did not undergo crystallization during the process of being specifically realized as glass.
[0122] Fig.16 This is a diagram showing the measurement of internal defects of an optical glass prepared using the composition according to the second example of the present invention.
[0123] Reference Fig.16 a to Fig.16 d. It can be confirmed that the optical glasses (GGSe-1Te, GGSe-3Te, GGSe-5Te, and GGSe-7Te) have no internal defects and thus have excellent far-infrared light transmittance.
[0124] Fig.17 : is a graph illustrating characteristics for confirming the vitrification of the composition according to the second example of the present invention.
[0125] Fig.17 The graph of is a graph illustrating the characteristics of each second composition when it is embodied as a 35 mm optical glass. It can be confirmed that the optical glasses (GGSe-1Te, GGSe-3Te, GGSe-5Te, GGSe-7Te) are all vitrified and no crystallization peak is found at all angles. That is, each optical glass embodied with the second composition does not crystallize inside, so it can be confirmed that it can have excellent far-infrared light transmittance.
[0126] Fig.18 is a graph illustrating the transmittance of the composition according to the second embodiment of the present invention in the far infrared light band.
[0127] Fig.18The graph is a graph illustrating the characteristics of each second composition when it is specifically implemented as a 4mm optical glass. It can be confirmed that each optical glass (GGSe-1Te, GGSe-3Te, GGSe-5Te, GGSe-7Te) has an average transmittance of more than 60% in the 8 to 12μm band, which is a far-infrared light band. More specifically, the optical glass (GGSe-1Te) shows an average transmittance of 65.80%, the optical glass (GGSe-3Te) shows an average transmittance of 64.14%, the optical glass (GGSe-5Te) shows an average transmittance of 63.87%, and the optical glass (GGSe-7Te) shows an average transmittance of 64.23%.
[0128] Fig.19 is a graph illustrating the coefficient of thermal expansion of a composition according to a second embodiment of the present invention.
[0129] Each optical glass (GGSe-1Te, GGSe-3Te, GGSe-5Te, GGSe-7Te) also shows a relatively low change in thermal expansion coefficient at a temperature change of approximately 350°C. Each optical glass (GGSe-1Te, GGSe-3Te, GGSe-5Te, GGSe-7Te) has a relatively low thermal expansion coefficient of 12.7955×10 -6 K, 12.7527×10 -6 K, 12.8338×10 -6 K, 13.2806×10 -6 K shows a tendency to increase with the increase of Te content. It can be confirmed that this is not much different from the thermal expansion coefficient of the existing far-infrared light transmitting glass (containing heavy metals) sold on the market. Among the existing far-infrared light transmitting glasses (containing heavy metals), the product with excellent thermal expansion coefficient is 12.5×10 -6 K (Schott (Germany Schott) IRG 22), in addition, the product with excellent thermal expansion coefficient also has 14.0×10 -6 K (Schott (Germany) IRG 25), 20.0×10 -6 K (Schott (Germany) IRG 24) or 21.4×10 -6 K (IRG 26 of Schott (Germany) Company), etc. With reference to this, it can be confirmed that each optical glass (GGSe-1Te, GGSe-3Te, GGSe-5Te, GGSe-7Te) has a thermal expansion coefficient similar to or better than that of commercial products.
[0130] Fig. 20 and Fig.21is a graph illustrating thermal characteristics and glass transition temperature of a composition according to a second embodiment of the present invention with respect to temperature.
[0131] Fig. 20 This is a graph of TG-DTA thermal analysis of various optical glasses (GGSe-1Te, GGSe-3Te, GGSe-5Te, GGSe-7Te). Fig. 20 and Fig.21 , the glass transition temperatures of the optical glasses (GGSe-1Te, GGSe-3Te, GGSe-5Te, GGSe-7Te) are 326.9°C, 324.4°C, 313.3°C, and 310.3°C, respectively. As the Te content in the raw materials forming the optical glass increases, the glass transition temperature shows a tendency to decrease. Te >Z se (Z is the atomic number) and the atomic radius of Te is larger than the atomic radius of Se. As the amount of Te increases, the glass transition temperature decreases.
[0132] Fig. 22 is a graph illustrating the hardness of the composition according to the second embodiment of the present invention.
[0133] It can be confirmed that the optical glasses (GGSe-1Te, GGSe-3Te, GGSe-5Te, GGSe-7Te) all have an excellent hardness of more than 170HK, and the harder the glass is, the lower the hardness is.
[0134] Fig.23 is a graph illustrating the refractive index of a composition according to a second embodiment of the present invention.
[0135] Each optical glass (GGSe-1Te, GGSe-3Te, GGSe-5Te, GGSe-7Te) has a refractive index ranging from 2.51 to 2.61 in the far-infrared light band (8 to 12 μm), and all have an excellent refractive index of more than 2.5. The more the content of Te as a dopant increases, the more the refractive index of the optical glass increases. In particular, each optical glass (GGSe-1Te, GGSe-3Te, GGSe-5Te, GGSe-7Te) has a refractive index of 2.5204, 2.5394, 2.5623 and 2.5852 in the 10 μm band, respectively, and it can be confirmed that the refractive index has been significantly improved compared to the case without a dopant.
[0136] Fig.24 is a graph illustrating dispersion values of a composition according to a second embodiment of the present invention.
[0137] Pictured at Fig.24The table shows the refractive index of each optical glass (GGSe-1Te, GGSe-3Te, GGSe-5Te, GGSe-7Te) for each wavelength band. With reference to the table, the dispersion value of each optical glass (GGSe-1Te, GGSe-3Te, GGSe-5Te, GGSe-7Te) in the 8 to 12 μm band can be calculated as follows.
[0138]
[0139] Here, ν refers to the dispersion value in the 8 to 12 μm band, and n refers to the refractive index at each wavelength. Observing the dispersion value, each optical glass (GGSe-1Te, GGSe-3Te, GGSe-5Te, GGSe-7Te) has a dispersion value of 94.67, 97.43, 100.99, and 103.88, respectively, and it can be confirmed that the dispersion value increases as the content of Te as a dopant increases.
[0140] That is, it was confirmed that in the case of an optical glass containing Te as a dopant, a very good refractive index was ensured and excellent low dispersion characteristics were provided.
[0141] Fig.25 : is a graph showing the contents of components constituting the composition for far-infrared light transmitting glass according to the third embodiment of the present invention.
[0142] The composition for far-infrared light-transmitting glass according to the third embodiment of the present invention (hereinafter, simply referred to as “third composition”) refers to a composition containing the following raw materials.
[0143] 1) Ge: 35 mol%, Ga: 5 mol%, Se: 60 mol% (220)
[0144] 2) Ge: 35 mol%, Ga: 5 mol%, Se: 57.5 mol%, S: 2.5 mol% (GGSe-2.5S)
[0145] 3) Ge: 35 mol%, Ga: 5 mol%, Se: 55 mol%, S: 5 mol% (GGSe-5S)
[0146] 4) Ge: 35 mol%, Ga: 5 mol%, Se: 52.5 mol%, S: 7.5 mol% (GGSe-7.5S)
[0147] 5) Ge: 35 mol%, Ga: 5 mol%, Se: 50 mol%, S: 10 mol% (GGSe-10S)
[0148] 6) Ge: 35 mol%, Ga: 5 mol%, Se: 40 mol%, S: 20 mol% (GGSe-20S)
[0149] 7) Ge: 35 mol%, Ga: 5 mol%, Se: 30 mol%, S: 30 mol% (GGSe-30S)
[0150] 8) Ge: 35 mol%, Ga: 5 mol%, Se: 20 mol%, S: 40 mol% (GGSe-40S)
[0151] 9) Ge: 35 mol%, Ga: 5 mol%, Se: 10 mol%, S: 50 mol% (GGSe-50S)
[0152] 10) Ge: 35 mol%, Ga: 5 mol%, Se: 0 mol%, S: 60 mol% (GGSe-60S)
[0153] The content of S is x mol%, the content of Se is (60-x) mol%, and Ge and Ga are contained in a ratio of 7:1 within 40 mol%. At this time, the content of S (x) can be 2.5 to 60 mol%. In the case of including S as a dopant, the dispersion value of the optical glass prepared using the third composition increases, and therefore, it can be processed into an optical composition with a high dispersion value.
[0154] Similarly, the raw material content of the third composition described above is only an example for illustrating the characteristics of the optical glass prepared by the third composition to be described below, and is not necessarily limited to the content described above. As described in the first composition, Se and S can have a content of 50 to 70 mol%, and Ga and Ga can be included in the remaining content except the Se content at a ratio of 3 to 15:1. For convenience, the third composition (GGSe-2.5S to GGSe-60S) of the ratio described above is used as a reference for the following description, but it is not necessarily limited to this.
[0155] FIG. 26 schematically shows an optical glass prepared using a third composition containing the respective raw materials in the aforementioned contents.
[0156] Fig. 26 is a diagram illustrating an optical glass prepared with a composition according to the third embodiment of the present invention. Here, the optical glass produced can grow to a diameter having a set reference value, for example, to have a diameter of more than 35 mm and have an ingot form. The optical glass prepared with the composition according to the third embodiment of the present invention grows and can also have a diameter of up to 60 mm.
[0157] Figures 26a to 26dThe glass embodied with each third composition (GGSe-10S to GGSe-40S) is shown. Figures 26a to 26d It can be confirmed that each of the third compositions did not undergo crystallization during the process of being specifically realized as glass.
[0158] Fig. 27 This is a diagram showing the measurement of internal defects of an optical glass prepared using the composition according to the third example of the present invention.
[0159] Reference Fig. 27 a to Fig. 27 d. It can be confirmed that the optical glass (GGSe-10S to GGSe-40S) has no internal defects and thus has excellent far-infrared light transmittance.
[0160] Fig.28 : is a graph illustrating characteristics for confirming vitrification of the composition according to the third example of the present invention.
[0161] Fig.28 The graph of is a graph illustrating the characteristics when each third composition is embodied as a 35 mm optical glass. It can be confirmed that the optical glasses (GGSe-10S to GGSe-40S) are all vitrified and no crystallization peak is found at all angles. That is, each optical glass embodied with the third composition does not crystallize inside, so it can be confirmed that it can have excellent far-infrared light transmittance.
[0162] Fig.29 and Fig.30 is a graph illustrating the transmittance of the composition according to the third embodiment of the present invention in the far infrared light band.
[0163] Pictured at Fig.29 and Fig.30The graph is a graph illustrating the characteristics of each third composition when it is specifically implemented as a 4mm optical glass. It can be confirmed that each optical glass (GGSe-2.5S to GGSe-40S) has an average transmittance of more than 50% in the 8 to 12μm band as the far-infrared light band. More specifically, the optical glass (GGSe-2.5S) shows an average transmittance of 63.2%, the optical glass (GGSe-5S) shows an average transmittance of 64.2%, the optical glass (GGSe-7.5S) shows an average transmittance of 62.4%, the optical glass (GGSe-10S) shows an average transmittance of 62%, the optical glass (GGSe-20S) shows an average transmittance of 59.5%, the optical glass (GGSe-30S) shows an average transmittance of 56.8%, and the optical glass (GGSe-40S) shows an average transmittance of 53.7%. It shows that the more the content of S decreases, the more the transmittance increases. When optical glass is subjected to a non-reflective coating or the like, it can have a higher transmittance.
[0164] Fig.31 is a graph illustrating the coefficient of thermal expansion of a composition according to a third embodiment of the present invention.
[0165] Each optical glass (GGSe-10S to GGSe-40S) also shows a relatively low change in thermal expansion coefficient at a temperature change of approximately 350°C. Each optical glass (GGSe-10S to GGSe-40S) has a relatively low thermal expansion coefficient, and the thermal expansion coefficient is 12.2702×10 -6 K, 12.5033×10 -6 K, 11.9670×10 -6 K, 12.1307×10 -6 K, but no tendency is shown. This is more obvious when compared with the thermal expansion coefficient of existing far-infrared light transmitting glass (containing heavy metals) sold on the market. Among the existing far-infrared light transmitting glass (containing heavy metals), the product with excellent thermal expansion coefficient is 12.5×10 -6 K (Schott (Germany Schott) IRG 22), in addition, the product with excellent thermal expansion coefficient also has 14.0×10 -6 K (Schott (Germany) IRG 25), 20.0×10 -6 K (Schott (Germany) IRG 24) or 21.4×10 -6 K (IRG26 of Schott (Germany) Co., Ltd.), etc. Referring to this, it can be confirmed that each optical glass (GGSe-10S to GGSe-40S) has a thermal expansion coefficient similar to or better than that of commercial products.
[0166] Fig.32 and Fig.33 is a graph illustrating thermal characteristics and glass transition temperature of a composition according to a third embodiment of the present invention according to temperature.
[0167] Fig.32 This is a graph of TG-DTA thermal analysis of various optical glasses (GGSe-10S to GGSe-40S). Fig.32 and Fig.33 , the glass transition temperatures of the optical glasses (GGSe-10S to GGSe-40S) are 321.2°C, 324.7°C, 313.3°C, and 331.5°C, respectively. As the S content in the raw materials forming the optical glass increases, the glass transition temperature shows an increasing trend. This is because as the S content increases, the coordination number (Coordination number) of GeS4 increases. 4 GeSe with a coordination number of 2 2 This is because more units are formed, thereby improving the connectivity of the network. In addition, this is because the strength of the Ge-S bond (279 kJ / mol) is stronger than the strength of the Ge-Se bond (230 kJ / mol).
[0168] Fig.34 is a graph illustrating the hardness of a composition according to a third embodiment of the present invention.
[0169] It can be confirmed that the optical glasses (GGSe-10S to GGSe-40S) all have an excellent hardness of 175HK or more, and the harder the glass is, the higher the S content is.
[0170] Fig.35 is a graph illustrating the refractive index of a composition according to a third embodiment of the present invention.
[0171] Each optical glass (GGSe-2.5S, GGSe-5S, GGSe-7.5S) has a refractive index in the range of 2.46 to 2.5 in the far infrared light band (8 to 12 μm), and all have an excellent refractive index of more than 2.45. The more the content of S as a dopant decreases, the more the refractive index of the optical glass increases.
[0172] Fig.36 is a graph illustrating dispersion values of a composition according to a third embodiment of the present invention.
[0173] Pictured at Fig.36The table shows the refractive index of each optical glass (GGSe-2.5S, GGSe-5S, GGSe-7.5S) for each wavelength. Referring to the table, the dispersion values of each optical glass (GGSe-2.5S, GGSe-5S, GGSe-7.5S) in the 8 to 12 μm band are as follows. Each optical glass (GGSe-2.5S, GGSe-5S, GGSe-7.5S) has a relatively low dispersion characteristic, and its dispersion values are 87.2, 85.8 and 82.3, respectively. It can be confirmed that the less the content of S as a dopant, the more the dispersion value increases.
[0174] That is, it was confirmed that in the case of an optical glass containing S as a dopant, as the S content decreases, a better refractive index is ensured and excellent low dispersion characteristics are obtained.
[0175] Although in Figure 1 It is recorded that each process is performed sequentially, but this is only an illustrative description of the technical concept of one embodiment of the present invention. In other words, a person skilled in the art can perform various modifications and variations by changing the order recorded in each drawing or performing more than one process in parallel within the scope of the essential characteristics of one embodiment of the present invention. Therefore, Figure 1 Not limited to a chronological order.
[0176] On the other hand, the diagram in Figure 1 Each process in the present invention can be specifically implemented in a computer-readable recording medium with a computer-readable code. The computer-readable recording medium includes all types of recording devices that store data that can be read by a computer system. That is, the computer-readable recording medium includes storage media such as magnetic storage media (e.g., ROM, floppy disk, hard disk, etc.) and optical reading media (e.g., CD-ROM, DVD, etc.). In addition, the computer-readable recording medium can be distributed in a computer system connected to a network to store and execute the computer-readable code in a distributed manner.
[0177] The above description is only an illustrative description of the technical idea of this embodiment. A person skilled in the art can make various modifications and variations without departing from the essential characteristics of this embodiment. Therefore, this embodiment is intended to illustrate the technical idea of this embodiment, not to limit the technical idea of this embodiment, and the scope of the technical idea of this embodiment is not limited by these embodiments. The protection scope of this embodiment shall be interpreted by the attached claims, and all technical ideas within the scope equivalent thereto shall be interpreted as being included in the scope of rights of this embodiment.
[0178] This patent is the result of research carried out with the support of the Korean government (Ministry of Trade, Industry and Energy) and the Korea Institute of Industrial Technology Evaluation and Management in 2020 (Project unique number: 1415168029, specific project number: 20002803, project name: Development of core technology of far-infrared optical glass and lens without As and Sb for mobile devices);
[0179] This is the result of research carried out with funding from the South Korean government (Ministry of Trade, Industry and Energy) in 2021 and support from the Korea Industrial Technology Agency (specific project number: P0017725, project name: Support for the industrialization of optical raw materials for camera lenses).
[0180] (CROSS-REFERENCE TO RELATED APPLICATIONS)
[0181] If this patent application claims priority under Section 119(a) of the United States Patent Act (35 U.S.C. §119(a)) to Patent Application No. 10-2020-0119159 filed in Korea on September 16, 2020, all of the contents are incorporated as references into this patent application. Furthermore, if this patent application also claims priority to countries other than the United States based on the same reasons as above, all of the contents are incorporated as references into this patent application.
Claims
1. A glass composition which transmits 60% or more of light in the far-infrared wavelength range of 8 to 12 μm and has a hardness of 170 HK or more and a refractive index of 2.4 or more, wherein: Includes Ge, Ga and Se, and excludes As and Sb, Among them, the content of Se is 60 mol%, the content of Ge and Ga is 40 mol% in total, and the ratio of Ge to Ga is 3:1 to 15:
1.
2. A method for manufacturing optical glass, wherein the optical glass transmits 60% or more of light in the 8 to 12 μm band, which is a far infrared band, and has a hardness of 170 HK or more and a refractive index of 2.4 or more, characterized in that: include: A process of mixing Ge, Ga and Se except As and Sb in predetermined contents and charging them into a predetermined container, wherein the content of Se is 60 mol%, the content of Ge and Ga is 40 mol% in total, and the ratio of Ge to Ga is 3:1 to 15:1; A melting process of melting the above-mentioned set container under a first set environment; as well as A slow cooling process of slowly cooling the container that has undergone the above-mentioned melting process under the second set environment.
3. The method for manufacturing optical glass according to claim 2, characterized in that: In the above melting process, the above-defined container is melted at a temperature of 900 to 1000° C. for a defined period of time.
4. The method for producing optical glass according to claim 3, characterized in that: The time set above is 12 hours.
5. The method for manufacturing optical glass according to claim 2, characterized in that: In the above-mentioned slow cooling process, the container that has undergone the above-mentioned melting process is slowly cooled at the glass transition temperature for a set time.
6. The method for manufacturing optical glass according to claim 5, characterized in that: The time set above is 3 hours.
7. A glass composition which transmits 60% or more of light in the far-infrared wavelength range of 8 to 12 μm and has a hardness of 170 HK or more and a refractive index of 2.5 or more, characterized in that: Includes Ge, Ga, Se and Te, and excludes As and Sb, Among them, the content x of Te is 1 to 7 mol%, the content of Se is (60-x) mol%, the content of Ge and Ga is 40 mol% in total, and the ratio of Ge to Ga is 7:
1.
8. A method for manufacturing optical glass, wherein the optical glass transmits 60% or more of light in the far-infrared wavelength range of 8 to 12 μm and has a hardness of 170 HK or more and a refractive index of 2.5 or more, characterized in that: include: A process of mixing Ge, Ga, Se and Te except As and Sb in predetermined contents and charging them into a predetermined container, wherein the content x of Te is 1 to 7 mol%, the content of Se is (60-x) mol%, the total content of Ge and Ga is 40 mol%, and the ratio of Ge to Ga is 7:1; A melting process of melting the above-mentioned set container under a first set environment; as well as A slow cooling process of slowly cooling the container that has undergone the above-mentioned melting process under the second set environment.
9. The method for manufacturing optical glass according to claim 8, characterized in that: In the above melting process, the above-defined container is melted at a temperature of 900 to 1000° C. for a defined period of time.
10. A glass composition which transmits 50% or more of light in the far-infrared wavelength range of 8 to 12 μm and has a hardness of 175 HK or more and a refractive index of 2.45 or more, characterized in that: Includes Ge, Ga, Se and S, and excludes As and Sb, Among them, the content x of S is 2.5 to 60 mol%, the content of Se is (60-x) mol%, the content of Ge and Ga is 40 mol% in total, and the ratio of Ge to Ga is 7:
1.
11. A method for manufacturing optical glass, wherein the optical glass transmits 50% or more of light in the far-infrared wavelength range of 8 to 12 μm and has a hardness of 175 HK or more and a refractive index of 2.45 or more, characterized in that: include: A process of mixing Ge, Ga, Se and S except As and Sb in predetermined contents and charging them into a predetermined container, wherein the content x of S is 2.5 to 60 mol%, the content of Se is (60-x) mol%, the total content of Ge and Ga is 40 mol%, and the ratio of Ge to Ga is 7:1; A melting process of melting the above-mentioned set container under a first set environment; as well as A slow cooling process of slowly cooling the container that has undergone the above-mentioned melting process under the second set environment.
Citation Information
Patent Citations
A quality expectation information providing apparatus for providing dynamic changing connections to wireless networks based on learning models of quality expectations
KR1020200119159A
Sulfur optical glass
CN104402220A
Glass composition and infrared transmitting lens including the same
KR101756747B1