Negative electrode active material containing silicon composite formed by conductive fiber network, preparation method thereof, and lithium secondary battery containing the same

By using silicon composites assembled with conductive fiber networks in lithium secondary batteries, the problem of volume changes caused by the insertion and deintercalation of lithium ions is solved, the life and output characteristics of the battery are improved, and the safety and high capacity of the battery are ensured.

CN114600277BActive Publication Date: 2024-10-01GRAPSIL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980101489.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-10-22
Filing Date
2019-10-29
Publication Date
2024-10-01
Estimated Expiration
2039-10-29

AI Technical Summary

Technical Problem

The carbon-based material negative active material used in existing lithium secondary batteries causes volume expansion and contraction during the intercalation and deintercalation of lithium ions, resulting in the loss of conductive paths, reducing battery life and output characteristics, and it is difficult to achieve uniform physical and chemical Bonding to obtain stable quality negative electrode materials.

Method used

A high-capacity negative active material with excellent conductivity is formed by dispersing silicon nanoparticles on a first amorphous carbon matrix to form a primary silicon composite, and assembling a network of conductive fibers to form a secondary silicon composite, utilizing the conductive fiber network Conductive paths are formed to support the silicon composite, reducing volume changes and electrode damage.

Benefits of technology

It improves the life characteristics and output characteristics of lithium secondary batteries, ensures the safety and high capacity of the battery, significantly improves the initial efficiency and capacity retention rate, and reduces electrode damage and contact between silicon nanoparticles and electrolyte.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114600277B_ABST
    Figure CN114600277B_ABST
Patent Text Reader

Abstract

The present invention provides a high-capacity negative electrode active material and a lithium secondary battery containing the same. The negative electrode active material includes a primary silicon composite formed by dispersing silicon nanoparticles on a first amorphous carbon matrix, and a secondary silicon composite formed by assembling the primary silicon composite on a second amorphous carbon matrix through a network of conductive fibers, thereby blocking the contact between the silicon nanoparticles and the electrolyte, so that the negative electrode active material has excellent conductivity, and the lithium secondary battery has excellent life characteristics, output characteristics and safety.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a high-capacity negative electrode active material and a preparation method thereof, and a lithium secondary battery comprising the negative electrode active material. The negative electrode active material comprises a silicon composite formed by a network of conductive fibers and has excellent conductivity. The lithium secondary battery has excellent life characteristics, output characteristics and safety. Background Art

[0002] Lithium secondary batteries are widely used as power sources for mobile electronic devices including mobile phones, and as demand for large devices such as electric vehicles increases, the application fields of lithium secondary batteries are expanding.

[0003] At the same time, most of the currently commercialized lithium secondary batteries use carbon-based materials as negative electrode active materials. In particular, graphite exhibits highly reversible charge / discharge behavior due to the uniaxial orientation of the graphite layer (single-layer graphite layer, graphene layer), thereby showing excellent life characteristics. In addition, since graphite exhibits an almost similar potential to lithium metal, when a battery is formed with a lithium oxide-based positive electrode, it has the advantage of being able to obtain high energy. However, despite these advantages, at the current stage where high-capacity batteries are required, the low theoretical capacity of graphite (372mAh / g) plays a limiting role.

[0004] Therefore, attempts have been made to use metal materials showing relatively high capacity, such as Si, Sn, and Al, as alternative carbon-based negative electrode active materials. However, these metal materials undergo large volume expansion and contraction during the insertion and extraction of lithium ions, which may lead to micronization and loss of conductive paths, thereby reducing overall battery performance, such as reducing life characteristics.

[0005] In order to solve the above problems, many efforts have been made, such as simply mixing various carbon materials with Si, or chemically fixing micropowdered Si on the carbon surface using silane coupling agents, or fixing amorphous carbon on the Si surface by chemical vapor deposition (CVD).

[0006] However, in the case of a material in which a carbon material is simply mixed with Si, Si undergoes large volume expansion and contraction as charge and discharge proceed, and carbon is separated from silicon, thereby reducing conductivity and significantly reducing life characteristics.

[0007] On the other hand, in the case of materials in which micropowdered silicon or the like is chemically fixed to the carbon surface by using a silane coupling agent, CVD, etc., the bonding duration by the silane coupling agent or CVD is not long, so the life characteristics may be reduced as the charge and discharge cycles proceed. Furthermore, there is a problem that it is difficult to obtain a negative electrode material of stable quality by uniform physical and chemical bonding.

[0008] Despite these various attempts, there remains the problem of electrode damage due to expansion of Si during discharge.

[0009] Therefore, there is a great demand for a high-capacity negative electrode active material having excellent conductivity and a lithium secondary battery including the negative electrode active material and having excellent life characteristics and output characteristics and high safety. Summary of the invention

[0010] Technical issues

[0011] The present invention aims to solve the above-mentioned problems of the prior art and unresolved technical problems.

[0012] Specifically, an object of the present invention is to provide a high-capacity negative electrode active material having excellent conductivity by including a silicon composite formed by a network of conductive fibers.

[0013] The object of the present invention is to provide a method for preparing the negative electrode active material.

[0014] Another object of the present invention is to provide a lithium secondary battery including the negative electrode active material and having excellent life characteristics and output characteristics and having remarkable safety.

[0015] Technical Solution

[0016] The present invention provides a negative electrode active material, which includes: a primary silicon composite formed by dispersing silicon nanoparticles on a first amorphous carbon matrix; and a secondary silicon composite formed by assembling the primary silicon composite on a second amorphous carbon matrix through a network of conductive fibers.

[0017] The silicon nanoparticles may be at least any one of amorphous silicon nanoparticles having an average particle diameter of 10 to 200 nm and crystalline silicon nanoparticles having a crystal size of greater than 0 nm and less than 30 nm.

[0018] The primary silicon composite may have an average particle size of 0.2-1.3 μm.

[0019] The secondary silicon composite may have an average particle size of 1-80 μm.

[0020] The network of conductive fibers may be at least partially in contact with the primary silicon composite to form a conductive path.

[0021] The network of conductive fibers may be at least partially exposed on a surface of the secondary silicon composite.

[0022] The conductive fiber may be at least one selected from graphene, carbon fiber, carbon nanotube, conductive polymer fiber and metal wire.

[0023] The electrical conductivity of the second amorphous carbon may be higher than the electrical conductivity of the first amorphous carbon.

[0024] The present invention also provides a method for preparing a negative electrode active material, the method comprising the following steps:

[0025] preparing a primary silicon composite by mixing a first amorphous carbon precursor and silicon nanoparticles and performing a heat treatment; and

[0026] Preparation of secondary silicon composite: After mixing the primary silicon composite, the second amorphous carbon precursor and the conductive fiber, a secondary heat treatment is performed, so that the secondary silicon composite is assembled through the network of the conductive fiber to form the secondary silicon composite.

[0027] Based on 100 parts by weight of the silicon nanoparticles, the first amorphous carbon precursor may be 50-200 parts by weight.

[0028] Based on 100 parts by weight of the silicon nanoparticles, the second amorphous carbon precursor may be 50-200 parts by weight.

[0029] Based on 100 parts by weight of the silicon nanoparticles, the conductive fibers may be present in an amount of 20-80 parts by weight.

[0030] The primary heat treatment and the secondary heat treatment may be performed at 800° C. to 1200° C. for 1 to 3 hours, respectively.

[0031] The present invention provides a lithium secondary battery comprising the negative electrode active material.

[0032] Beneficial Effects

[0033] The negative electrode active material according to the present invention includes silicon nanoparticles showing high capacity, and thus the life characteristics of the lithium secondary battery can be improved.

[0034] Furthermore, according to the present invention, the negative electrode active material includes the secondary silicon composite assembled with the primary silicon composite, and thus the output characteristics of the lithium secondary battery can be improved as the lithium ion movement path increases.

[0035] In addition, according to the present invention, although the silicon nanoparticles repeatedly expand and shrink due to the embedding and de-embedding of lithium ions, the damage to the electrode can be minimized due to the buffering effect of the silicon nanoparticles that are nanosized and highly dispersible and the first amorphous carbon matrix and the second amorphous carbon matrix containing the silicon nanoparticles, and the contact between the silicon nanoparticles and the electrolyte can be suppressed, thereby ensuring the safety of the lithium secondary battery.

[0036] In addition, according to the present invention, since the primary silicon composite forms a conductive path through a network assembly of conductive fibers, the lithium secondary battery thus produced has a high capacity and a remarkable initial efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 It is a schematic diagram showing a cross section of a negative electrode active material according to one embodiment of the present invention.

[0038] Figure 2 This is a SEM photograph of the primary silicon composite of Experimental Example 1.

[0039] Figure 3 This is a SEM photograph of the secondary silicon composite of Experimental Example 1.

[0040] Figure 4 This is a SEM photograph of the negative electrode active material of Comparative Example 1 in Experimental Example 1.

[0041] Figure 5 This is the particle size data of the secondary silicon composite in Experimental Example 2.

[0042] Figure 6 Graph showing the capacity retention rate according to the number of cycles in Experimental Example 4. DETAILED DESCRIPTION

[0043] Negative active material

[0044] Figure 1 Schematic diagram of a cross section of a negative electrode active material according to one embodiment of the present invention, but the present invention is not limited to the above-described form.

[0045] refer to Figure 1 The negative electrode active material includes: a primary silicon composite 112 formed by dispersing silicon nanoparticles 110 on a first amorphous carbon matrix 111; and a secondary silicon composite 100 formed by assembling the primary silicon composite 112 on a second amorphous carbon matrix 121 through a network of conductive fibers 130.

[0046] In the present invention, the term "first amorphous carbon matrix 111" means that the first amorphous carbon exists to form a continuous phase.

[0047] In the present invention, the term “primary silicon composite 112” refers to one or more silicon nanoparticles 110 continuously or discontinuously distributed on the first amorphous carbon matrix 111 to form a particle that looks like a particle, and is a structure in which the surface of the silicon nanoparticle 110 is surrounded by the first amorphous carbon.

[0048] In the present invention, the “second amorphous carbon matrix 121 ” means that the second amorphous carbon exists in the form of a continuous phase.

[0049] In the present invention, the "secondary silicon composite 100" refers to a structure in which the primary silicon composite 112 is aggregated on the second amorphous carbon matrix 121 and the particles are continuously or discontinuously distributed to form particles that look like a single particle, that is, the surface of the primary silicon composite 112 is surrounded by the second amorphous carbon.

[0050] In the present invention, “the secondary silicon composite 100 formed by assembling the primary silicon composites 112 through the network of the conductive fibers 130 ” means that the conductive fibers 130 act as a support to fix the plurality of primary silicon composites 112 to form the secondary silicon composite 100 .

[0051] The theoretical capacity of silicon is about 3600 mA / g, which shows a relatively high capacity compared with traditional carbon-based negative electrode materials. However, the problem is that it causes large volume expansion and contraction during the insertion and deintercalation of lithium ions, resulting in micronization, loss of conductive paths, etc., which leads to reduced life characteristics.

[0052] According to the present invention, even during the charging and discharging process of the battery, due to the embedding and de-embedding of lithium ions, the silicon nanoparticles 110 repeatedly shrink and expand, and the nano-sized particles showing high dispersibility and the first amorphous carbon matrix 111 and the second amorphous carbon matrix 121 surrounding it play a buffering role to minimize the volume change. In addition, due to the excellent mechanical strength of the negative electrode active material of the present invention, it also has excellent durability during, for example, rolling, etc. in the manufacturing process of the battery, so that the damage of the electrode can be minimized. Therefore, even during the repeated charging and discharging process of the battery, the contact between the silicon nanoparticles 110 and the electrolyte can be suppressed, so that the safety of the secondary battery can be ensured and excellent life characteristics can be shown.

[0053] On the other hand, when the conductive components in the negative electrode active material layer are unevenly distributed and aggregated, dead spaces where electrons cannot move between the negative electrode active material layers may occur, which is the cause of reduced conductivity or relatively increased resistance, thereby causing a problem of reduced output characteristics.

[0054] According to the present invention, micropores formed during the assembly process of the secondary silicon composite 100 assembled with the primary silicon composite 112 serve as movement channels for lithium ions. Therefore, the output characteristics of the lithium secondary battery can be improved.

[0055] Furthermore, since the shape of the primary silicon composite 112 is maintained by the network of the conductive fibers 130 and the secondary silicon composite 100 is formed during the assembly process, the lithium secondary battery using the negative active material of the present invention has high capacity and outstanding initial efficiency.

[0056] According to the present invention, the silicon nanoparticles 110 are dispersed on the first amorphous carbon matrix 111 in the form of existing independently from each other, and even if aggregation occurs, only a few particles may be aggregated.

[0057] The silicon nanoparticles 110 may be at least one of amorphous silicon nanoparticles and crystalline silicon nanoparticles.

[0058] The amorphous silicon nanoparticles may have an average particle size of 10-200 nm. When the average particle size is not within the above range and is too small, the process efficiency is reduced. On the other hand, when the average particle size is too large, micronization, contact with the electrolyte, etc. may occur during charging and discharging, so it is not preferred.

[0059] The crystalline silicon nanoparticles are heat treated at high temperature during the preparation process to adjust the crystal size so that they do not grow to a crystal size of 30 nm or more, so that the crystal size can be more than 0 nm and less than 30 nm. When the crystal size is within this range, high capacity can be achieved, and thus the initial efficiency of the lithium secondary battery can be improved.

[0060] The first amorphous carbon may be 50-200 parts by weight based on 100 parts by weight of the silicon nanoparticles 110. When the amount of the first amorphous carbon is not within this range and is excessive, the resistance may increase, so the output characteristics may deteriorate. When the amount of the silicon nanoparticles 110 is excessive, the micronization phenomenon may be aggravated during the charging and discharging process, so it is not preferred. Specifically, the first amorphous carbon may be 80-100 parts by weight based on 100 parts by weight of the silicon nanoparticles 110.

[0061] The primary silicon composite 112 is a particle that looks like a particle shape in which one or more silicon nanoparticles 110 are continuously or discontinuously distributed and arranged on the first amorphous carbon matrix 111, and the average particle size thereof may be 0.2-1.3 μm. When the average particle size is too small, the process efficiency may be reduced. On the other hand, when the average particle size is too large, the resistance increases due to the increase in the lithium ion path, and the charge and discharge efficiency decreases, so it is not preferred. Specifically, the average particle size may be 0.3-1 μm.

[0062] The conductive fibers 130 of the secondary silicon composite 100 can act as a support and can aggregate a plurality of primary silicon composites 112 to form a structure, and the average particle size thereof can be 1-80 μm. When the average particle size is too small, the process efficiency may be reduced, and when the average particle size is too large, the resistance may increase due to the increase in the lithium ion path, resulting in a reduction in the charging and discharging efficiency, which is not preferred. Specifically, the average particle size can be 5-15 μm.

[0063] Since at least a portion of the network of the conductive fibers 130 contacts the surface of the primary silicon composite 112 to form a conductive path, the conductivity can be increased and the resistance can be reduced, so the output characteristics can be further improved. In addition, the conductive fibers 130 can have the effect of suppressing the volume change of the primary silicon composite 112 during charge and discharge.

[0064] The network of the conductive fibers 130 may be at least partially exposed on the surface of the secondary silicon composite 100 , thereby imparting conductivity to the negative active material.

[0065] For example, at least 5-20 volume % of the entire conductive fibers 130 may be exposed on the surface of the secondary silicon composite 100. This is the optimal range for ensuring the support effect and conductivity of the primary silicon composite 112. If it is out of this range, the expected effect of the present invention cannot be exerted, which is not preferred.

[0066] The conductive fiber 130 exhibits conductivity, and its material is not limited as long as it can be electrically connected to the primary silicon composite 112. For example, the conductive fiber 130 can be one or more selected from graphene, carbon fiber, carbon nanotube, conductive polymer fiber or metal wire. The metal can be stainless steel, aluminum, nickel, copper, titanium, platinum, gold, silver, ruthenium, tantalum, niobium, hafnium, zirconium, vanadium, indium, cobalt, tungsten, tin, beryllium, molybdenum or alloys or laminates thereof, but is not limited thereto.

[0067] The cross-sectional diameter and length of the conductive fiber 130 can be determined according to the particle size of the primary silicon composite 112 and the secondary silicon composite 100. For example, the cross-sectional diameter of the conductive fiber 130 can be 10-500 nm, and the length can be 0.1-100 μm. The diameter of the conductive fiber 130 can actually be uniform or variable, and at least a portion of the long axis of the conductive fiber 130 can be straight, curved, bent, or branched.

[0068] The second amorphous carbon may be 50-200 parts by weight based on 100 parts by weight of the silicon nanoparticles 110. When the amount of the second amorphous carbon is not within the above range but is excessive, resistance may increase, and thus output characteristics may be reduced, and when the amount of the primary silicon composite 112 is excessive, micronization may be aggravated during charging and discharging, and thus it is not preferred.

[0069] The conductive fiber 130 may be 20-80 parts by weight based on 100 parts by weight of the silicon nanoparticles 110. When the amount of the conductive fiber is too small, it is difficult to maintain the shape according to the assembly of the primary silicon composite 112, and when the amount of the conductive fiber is too large, the resistance increases and the output characteristics may be reduced, which is not preferred.

[0070] The first amorphous carbon and the second amorphous carbon are not limited as long as they are known in the art. For example, one or a combination of two or more selected from soft carbon, hard carbon, pitch carbide, mesophase pitch carbide and calcined coke can be used respectively.

[0071] The conductivity of the first amorphous carbon and the second amorphous carbon may vary according to the materials used, the synthesis method, the treatment method, etc. In the present invention, the conductivity of the second amorphous carbon may be relatively higher than the conductivity of the first amorphous carbon. As described above, since the mesh structure of the conductive fiber 130 forms a conductive path, at least a portion of which is exposed on the surface of the secondary silicon composite 100, when the conductivity of the second amorphous carbon is relatively large, the output characteristics of the lithium secondary battery can be improved.

[0072] Method for preparing negative electrode active material

[0073] In another aspect, the present invention provides a method for preparing a negative electrode active material, the method comprising the following steps:

[0074] preparing a primary silicon composite 112 by mixing a first amorphous carbon precursor and silicon nanoparticles 110 and then performing a heat treatment; and

[0075] Preparation of the secondary silicon composite 100 : The primary silicon composite 112 , the second amorphous carbon precursor and the conductive fibers 130 are mixed and then subjected to a secondary heat treatment, so that the primary silicon composite 112 is assembled through the network of the conductive fibers 130 to form the secondary silicon composite 100 .

[0076] When the primary heat treatment is performed, the first amorphous carbon precursor is softened and carbonized to cover the silicon nanoparticles 110 and form a first amorphous carbon matrix 111 formed of the first amorphous carbon precursor, thereby forming a primary silicon composite 112 .

[0077] Various characteristics such as the particle sizes of the silicon nanoparticles 110 , the primary silicon composite 112 , the conductive fibers 130 , and the secondary silicon composite 100 have been described above, and thus repeated description thereof will be omitted below.

[0078] However, when the average particle size of the primary silicon composite 112 is too small, the process efficiency may be reduced. On the other hand, when the average particle size of the primary silicon composite 112 is too large, the resistance may be increased due to the increase of the lithium ion path, thereby reducing the charging and discharging efficiency, which is not preferred. Therefore, in the present invention, a process of adjusting the average particle size by pulverizing the primary silicon composite 112 may be performed. Specifically, before mixing the primary silicon composite 112, the second amorphous carbon precursor, and the conductive fiber 130, a process of pulverizing the primary silicon composite 112 to adjust the particle size to 0.2-1.3 μm, more specifically 0.3-1 μm, may be performed.

[0079] The first amorphous carbon precursor is one or more carbon precursors selected from coal-based pitch, mesophase pitch, petroleum-based pitch, coal-based oil, petroleum-based heavy oil, organic synthetic pitch, or polymer resins such as phenolic resin, furan resin, or polyimide resin.

[0080] The first amorphous carbon precursor may be 50-200 parts by weight based on 100 parts by weight of the silicon nanoparticles 110. When the amount of the first amorphous carbon precursor is not within this range and is excessive, the resistance may increase, so the output characteristics may deteriorate. When the amount of the silicon nanoparticles 110 is excessive, the micronization phenomenon may be aggravated during the charging and discharging process, so it is not preferred. Specifically, based on 100 parts by weight of the silicon nanoparticles 110, the first amorphous carbon precursor may be 80-100 parts by weight.

[0081] Mixing can be performed by dry mixing or wet mixing, and the present invention is not particularly limited thereto, but dry mixing is preferred.

[0082] As a dry mixing method, a method generally used for preparing mixed powders can be used, and mechanical grinding (milling) can be performed for uniform particle mixing. Mechanical grinding is a method of crushing a sample while applying mechanical energy to the sample, for example, a roller mill, a ball mill, a mechanical fusion machine or a jet mill can be used, and specifically, a ball mill that effectively utilizes high impact energy can be used.

[0083] The mechanical grinding treatment conditions can be appropriately adjusted according to the equipment used. The faster the rotation speed, the faster the product is generated, and the longer the rotation time, the higher the conversion rate from raw materials to products. For example, when using a common ball mill, it is preferably carried out under the conditions of 1000-3000 rpm and 0.5-5 minutes per minute, more specifically, under the conditions of 1500-2500 rpm and 1-3 minutes per minute.

[0084] The primary heat treatment may be performed at 800° C. to 1200° C. for 1-3 hours. When the primary heat treatment condition is out of the above range, the amorphous carbon is not sufficiently softened, and thus, it is difficult to place the amorphous carbon on the surface of the silicon nanoparticles 110, and the manufacturing process may be deteriorated, so it is not preferred.

[0085] When the secondary heat treatment is performed, the second amorphous carbon precursor is softened and carbonized to cover the primary silicon composite 112 and form a second amorphous carbon matrix 121 formed of second amorphous carbon, so that the secondary silicon composite 100 may be formed.

[0086] The second amorphous carbon precursor is one or more carbon precursors selected from coal-based pitch, mesophase pitch, petroleum-based pitch, coal-based oil, petroleum-based heavy oil, organic synthetic pitch, or polymer resins such as phenolic resin, furan resin or polyimide resin.

[0087] The second amorphous carbon precursor may be 50-200 parts by weight based on 100 parts by weight of the silicon nanoparticles 110. When the amount of the second amorphous carbon precursor is not within the above range but is excessive, resistance may increase, and thus output characteristics may be reduced, and when the amount of the primary silicon composite 112 is excessive, micronization may be aggravated during charging and discharging, and thus it is not preferred.

[0088] Mixing can be performed by dry mixing or wet mixing, and the present invention is not particularly limited thereto, but dry mixing is preferred.

[0089] As a dry mixing method, a method generally used for preparing mixed powders can be used, and mechanical grinding can be performed for uniform particle mixing. Mechanical grinding is a method of crushing a sample while applying mechanical energy to the sample, for example, a roller mill, a ball mill, a mechanical fusion machine or a jet mill can be used, and specifically, a ball mill that effectively utilizes high impact energy can be used.

[0090] The mechanical grinding treatment conditions can be appropriately adjusted according to the equipment used. The faster the rotation speed, the faster the product is generated, and the longer the rotation time, the higher the conversion rate from raw materials to products. For example, when using a common ball mill, preferably, the rotation number per minute is 1000-3000rpm and 0.5-5 minutes. Under the conditions, more specifically, the rotation number per minute is 1500-2500rpm and 1-3 minutes.

[0091] The secondary heat treatment may be performed at 800° C. to 1200° C. for 1-3 hours. When it is not within the above range, amorphous carbon is not sufficiently softened, and therefore, it is difficult to place amorphous carbon on the surface of the primary silicon composite 112, and the manufacturing process may be deteriorated, so it is not preferred.

[0092] On the other hand, based on 100 parts by weight of the silicon nanoparticles 110, the conductive fibers 130 may be 20 - 80 parts by weight. When the amount of the conductive fibers is too small, it is difficult to maintain the shape according to the assembly of the primary silicon composite 112, and when the amount of the conductive fibers is too large, the resistance increases and the output characteristics may deteriorate, so it is not preferred.

[0093] The conductivity of the first amorphous carbon and the second amorphous carbon may vary depending on the materials used, the synthesis method, the treatment method, etc. In the present invention, the conductivity of the second amorphous carbon may be relatively higher than that of the first amorphous carbon. As described above, since the network structure of the conductive fibers 130 forms a conduction path and at least a part of it is exposed on the surface of the secondary silicon composite 100, when the conductivity of the second amorphous carbon is large, the output characteristics of the lithium secondary battery can be improved.

[0094] Lithium secondary battery

[0095] The present invention provides a lithium secondary battery including a negative electrode active material.

[0096] The lithium secondary battery may include a positive electrode containing a positive electrode active material, a negative electrode containing a negative electrode active material, and an electrolyte.

[0097] The positive electrode is formed by coating a positive electrode mixture containing a positive electrode active material on a current collector, and, if necessary, the positive electrode mixture may further contain a binder and a conductive material.

[0098] The positive electrode active material may be, for example, LiNi 0.8-x Co 0.2 Al x O2, LiCo x Mn y O2, LiNi x Co y O2, LiNi x Mn y O2, LiNi x Co y Mn z O2, LiCoO2, LiNiO2, LiMnO2, LiFePO4, LiCoPO4, LiMnPO4 or Li4Ti5O 12 etc. lithium metal oxides (0 < x < 1, 0 < y < 1); chalcogenides such as Cu2Mo6S8, FeS, CoS or MiS; oxides, sulfides and halides of scandium, ruthenium, titanium, vanadium, molybdenum, chromium, manganese, iron, cobalt, nickel, copper, zinc, etc. More specifically, LiNi 0.8 Co 0.1 Mn 0.1O2, TiS2, ZrS2, RuO2, Co3O4, Mo6S8 and V2O5, etc., but not limited to these.

[0099] The shape of the positive electrode active material is not particularly limited, and may be in the form of particles, for example, may be spherical, elliptical or cuboid. The average particle size of the positive electrode active material may be in the range of 1-50 μm, but is not limited thereto. The average particle size of the positive electrode active material may be obtained, for example, by measuring the particle size of the active material observed with a scanning electron microscope (SEM) and calculating its average value.

[0100] The binder is not particularly limited, and a fluorine-containing binder such as polyvinylidene fluoride (PVDF) and polytetrafluoroethylene (PTFE) may be used, but is not limited thereto.

[0101] The content of the binder is not particularly limited as long as the positive electrode active material can be fixed, and the content of the binder may be in the range of 0 wt % to 10 wt % relative to the total weight of the positive electrode.

[0102] There is no particular limitation on the conductive material as long as the conductivity of the positive electrode can be improved. For example, nickel powder, cobalt oxide, titanium oxide, carbon, etc. can be used. Specifically, the carbon can be any one or more selected from Ketjen black, acetylene black, furnace black, graphite, carbon fiber and fullerene.

[0103] The content of the conductive material may be selected in consideration of other battery conditions such as the type of the conductive material, for example, the content of the conductive material may be in the range of 1 wt % to 10 wt % relative to the total weight of the positive electrode.

[0104] The thickness of the positive electrode mixture layer prepared by coating a positive electrode mixture including a positive electrode active material, a binder and a conductive material on a current collector may be, for example, 0.1 to 1000 μm.

[0105] According to circumstances, in the present invention, the positive electrode mixture may include 0.1 wt % to 60 wt %, specifically 10 wt % to 50 wt % of the solid electrolyte relative to the total weight of the positive electrode mixture.

[0106] The thickness of the positive electrode mixture layer may be, for example, 0.1 to 1000 μm.

[0107] The material of the positive electrode current collector is not particularly limited, as long as it is a material of the positive electrode current collector that does not cause chemical changes in the battery and has high conductivity. For example, stainless steel, aluminum, nickel, titanium, calcined carbon, or a material in which the surface of aluminum or stainless steel is surface-treated with carbon, nickel, titanium, silver, etc., can be used. In addition, the positive electrode current collector can be in various forms such as a film, sheet, foil, net, porous body, foam, non-woven fabric, etc., with fine concavoconvexity formed on the surface.

[0108] The negative electrode can use a negative electrode in which a negative electrode mixture containing a negative electrode active material is coated on a negative electrode current collector. The negative electrode active material can be a negative electrode active material according to the present invention, however, depending on the situation, metal oxides, metals, lithium composite oxides, crystalline carbon, amorphous carbon, etc. can be used together. As needed, the negative electrode mixture can further include a binder and a conductive material as described above.

[0109] There is no particular restriction on the negative electrode current collector at this time, as long as it does not cause chemical changes to the lithium secondary battery and has conductivity. For example, copper, stainless steel, aluminum, nickel, titanium or calcined carbon, or aluminum-cadmium alloys that have surface-treated copper or stainless steel with carbon, nickel, titanium, silver, etc., can be used. In addition, similar to the positive electrode current collector, the negative electrode current collector can be in various forms such as a film, sheet, foil, net, porous body, foam, and non-woven fabric with fine concavoconvex surfaces.

[0110] The electrolyte consists of an organic solvent and an electrolyte.

[0111] The organic solvent is not particularly limited as long as it is commonly used. For example, one or more selected from propylene carbonate, ethylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, methylpropyl carbonate, dipropyl carbonate, dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, vinylene carbonate, cyclopentane sulfone, gamma-butyrolactone, propylene sulfite and tetrahydrofuran can be used.

[0112] There is no limitation on the lithium salt, as long as it is a commonly used lithium salt that can be included as an electrolyte. For example, as the anion of the lithium salt, a lithium salt selected from F - , Cl - ,I - 、NO 3- 、N(CN) 2- , BF 4- , ClO 4- PF 6- 、(CF3)2PF 4- 、(CF3)3PF 3- 、(CF3)4PF 2- 、(CF3)5PF - 、(CF3)6P - CF3SO 3- CF3CF2SO 3- 、(CF3SO2)2N - 、(FSO2)2N - CF3CF2(CF3)2CO - 、(CF3SO2)2CH - 、(SF5)3C - 、(CF3SO2)3C- 、CF3(CF2)7SO 3- CF3CO 2- 、CH3CO 2- 、SCN - and (CF3CF2SO2)2N - One of them.

[0113] The secondary battery is completed by placing a separator between the positive electrode and the negative electrode to form a battery structure, winding or folding the battery structure, and then placing it in a cylindrical battery case or a rectangular battery case and injecting an electrolyte. Alternatively, the battery structure is stacked into a double battery structure, impregnated with an electrolyte, and the resultant is placed in a soft pack and sealed.

[0114] Description will be made with reference to the following examples, but the following examples are for the purpose of illustrating the present invention, and the scope of the present invention is not limited thereto.

[0115] [Example 1]

[0116] As a raw material for the first amorphous carbon, pitch with a carbonization rate of 40% and silicon nanoparticles with an average particle size of 100nm were mixed in a weight ratio of 4:6, and then purified and subjected to high-temperature treatment at 1000°C for 1 hour in an electric reactor in a nitrogen atmosphere. During the heat treatment, the pitch softened and carbonized to form a first carbon matrix covering the silicon nanoparticles, which was then pulverized to form a primary silicon composite with an average particle size of 0.2-1.3μm.

[0117] The primary silicon composite, pitch with a carbonization rate of 60% as a raw material of the second amorphous carbon, and carbon fibers were mixed in a weight ratio of 6:3:1, and then a purification process was performed. Next, a high-temperature heat treatment was performed at 975°C for 2 hours in an electric reactor in a nitrogen atmosphere. During the heat treatment, the pitch was softened and carbonized to form a second carbon matrix covering the primary silicon composite, and the primary silicon composite was assembled through a network of carbon fibers to form a secondary silicon composite. A negative electrode active material made of a secondary silicon composite was prepared.

[0118] <Comparative Example 1>

[0119] As a negative electrode active material, a silicon-carbon composite (Si / C) having a D50 of 12.2 μm was prepared.

[0120] <Experimental Example 1>

[0121] The SEM image of the primary silicon composite before pulverization prepared in Example 1 is shown below. Figure 2 In addition, the SEM images of the secondary silicon composite prepared in Example 1 and the negative electrode active material of Comparative Example 1 are shown in Figure 3 and Figure 4 middle.

[0122] Refer to the following Figure 2 The average particle size of the primary silicon composite before pulverization prepared in Example 1 is about 8 μm. When the average particle size of the primary silicon composite is too large, the resistance increases due to the increase in lithium ion paths, resulting in a decrease in charging and discharging efficiency. Therefore, it is preferred to pulverize before use.

[0123] refer to Figure 3 The secondary silicon composite particles according to Example 1 were uniform in shape and the aggregation between particles was minimized. However, the silicon composite particles according to Comparative Example 1 were not uniformly distributed and the particles aggregated.

[0124] <Experimental Example 2>

[0125] The particle size data of the secondary silicon composite prepared in Example 1 are shown below: Figure 5 middle.

[0126] refer to Figure 5 , D of the secondary silicon composite prepared in Example 1 50 It is 8.256μm.

[0127] <Experimental Example 3>

[0128] The negative electrode plates prepared using the negative electrode active materials according to Example 1 and Comparative Example 1 were cut into pieces with an area of ​​1.4875 cm 2 The lithium (Li) metal film was cut into a circle with an area of ​​1.4875 cm 2 Here, in the design of the negative electrode plate, the rolling density is 1.55 grams per cubic centimeter (g / cc) and the current density is 2.95 mA / cm 2 , the plate capacity is 510 mAh / g. A porous polyethylene separator is inserted between the positive electrode and the negative electrode, and 0.5 wt% of vinylene carbonate is dissolved in a mixed solution of ethyl methyl carbonate (EMC) and ethylene carbonate (EC) in a volume ratio of 7:3. Next, a lithium coin half-cell is prepared by injecting an electrolyte in which LiPF6 is dissolved at a concentration of 1 M.

[0129] The thickness change rate, discharge capacity, initial efficiency, capacity retention rate of Example 1 and the discharge capacity and initial efficiency of Comparative Example 1 were measured using lithium coin-type half cells and are shown in Table 1 below.

[0130] In the 1st cycle (formation cycle) and the 2nd cycle, charging and discharging were performed at 0.1C (standard cycle). In the 3rd to 49th cycles, charging and discharging were performed at 0.5C charging / 1.0C discharging. In the case of the 50th cycle, the cycle was completed in the charged state (i.e., the state in which lithium exists in the negative electrode). In this state, the battery was disassembled and the thickness was measured, and the rate of change of the electrode thickness after 50 cycles relative to the average of the charged thickness at the initial charge (the average of 5 samples) was calculated.

[0131] The basic charging and discharging conditions are as follows.

[0132] -Charging conditions: constant current (CC) / constant voltage (CV) (0.01V / 0.01C, current cut-off)

[0133] -Discharge condition: Constant current (CC) condition 1.5V cut-off

[0134] The discharge capacity (mAh / g) and initial efficiency (%) were derived from the results of the first charge and discharge. Specifically, the initial efficiency (%) was derived from the following formula.

[0135] - Initial efficiency (%) = (discharge capacity after the first discharge / first charge capacity) × 100

[0136] The capacity retention rate and electrode thickness change rate were derived by the following calculations.

[0137] -Capacity retention rate (%) = (49th discharge capacity / 1st discharge capacity) × 100

[0138] -Electrode thickness change rate (%) = (electrode thickness change after the 50th cycle / electrode thickness after the second cycle charge) × 100

[0139] [Table 1]

[0140]

[0141] According to Table 1, the negative electrode active material according to Example 1 exhibited excellent discharge capacity and initial efficiency compared to the negative electrode active material according to Comparative Example 1 using the silicon-carbon composite not including the composition of the present invention.

[0142] <Experimental Example 4>

[0143] Batteries using the negative electrode active material including the secondary silicon composite according to Example 1 and the negative electrode active material according to Comparative Example 1 were prepared. Specifically, negative electrodes including the above negative electrode active materials were prepared, and positive electrodes using NCM111 as positive electrode active materials were prepared. Here, the negative electrode had a rolling density of 1.565 g / cm3, a current of 2.95 mA / cm 2The positive electrode has a current density of 2.65 mA / cm 2 A current density of 1.56 g / cm3, a rolling density of 1.56 g / cm3 and an N / P of 1.10. A binder containing 1.5 wt% SBR and 1.5 wt% CMC was used. A porous polyethylene separator was inserted between the positive and negative electrodes. 0.5 wt% vinylene carbonate was dissolved in a mixed solution of ethyl methyl carbonate (EMC) and ethylene carbonate (EC) in a volume ratio of 7:3. A lithium coin-type half-cell was prepared by injecting an electrolyte in which LiPF6 was dissolved at a concentration of 1 M.

[0144] The charging condition of the lithium secondary battery is CC / CV, 0.5C charging, 4.2V / 0.05C cut-off, and the discharging condition is CC, 1.0C discharging and 2.85V cut-off. The capacity retention rate is measured (measured twice) and is shown in Figure 5 middle.

[0145] refer to Figure 5 , the difference in initial efficiency value becomes larger as the number of cycles increases. The higher the initial efficiency, the greater the amount of positive electrode material used when manufacturing a secondary battery of the same capacity, which has a great impact on the increase in cost, and therefore, a high-efficiency negative electrode material must be used. As described above, it is confirmed that the negative electrode active material composed of the secondary silicon composite according to the present invention has high efficiency and excellent life characteristics.

Claims

1. A negative electrode active material comprising: A primary silicon composite formed by dispersing silicon nanoparticles on a first amorphous carbon matrix, the primary silicon composite having an average particle size of 0.2-1.3 μm; and a secondary silicon composite formed by assembling the primary silicon composite on a second amorphous carbon matrix through a network of conductive fibers, wherein the network of conductive fibers is at least partially in contact with the primary silicon composite to form a conductive path, and the network of conductive fibers is at least partially exposed on the surface of the secondary silicon composite, The conductive fiber is at least one selected from graphene, carbon fiber, and metal wire. 2 . The negative electrode active material according to claim 1 , wherein the silicon nanoparticles are at least any one of amorphous silicon nanoparticles having an average particle size of 10 to 200 nm and crystalline silicon nanoparticles having a crystal size of greater than 0 nm and less than 30 nm. 3 . The negative electrode active material according to claim 1 , wherein the secondary silicon composite has an average particle size of 1 to 80 μm. 4 . The negative active material according to claim 1 , wherein the electrical conductivity of the second amorphous carbon is higher than that of the first amorphous carbon.

5. A method for preparing a negative electrode active material, the method comprising the following steps: preparing a primary silicon composite by mixing a first amorphous carbon precursor and silicon nanoparticles, and then performing a heat treatment at 1000-1200° C.; The primary silicon composite is crushed so that the average particle size of the primary silicon composite is 0.2-1.3 μm; and Preparation of secondary silicon composite: mixing the pulverized primary silicon composite, the second amorphous carbon precursor and the conductive fiber, and then performing a secondary heat treatment at 975-1200° C., The secondary silicon composite is formed by assembling the primary silicon composite through the network of conductive fibers, the network of conductive fibers is at least partially in contact with the primary silicon composite to form a conductive path, and the network of conductive fibers is at least partially exposed on the surface of the secondary silicon composite. The conductive fiber is at least one selected from graphene, carbon fiber, and metal wire.

6. The method for preparing a negative electrode active material according to claim 5, wherein: Based on 100 parts by weight of the silicon nanoparticles, the first amorphous carbon precursor is in an amount of 50-200 parts by weight.

7. The method for preparing a negative electrode active material according to claim 5, wherein: Based on 100 parts by weight of the silicon nanoparticles, the second amorphous carbon precursor is 50-200 parts by weight.

8. The method for preparing a negative electrode active material according to claim 5, wherein: Based on 100 parts by weight of the silicon nanoparticles, the conductive fibers are in an amount of 20-80 parts by weight.

9. The method for preparing a negative electrode active material according to claim 5, wherein: The primary heat treatment and the secondary heat treatment are respectively performed for 1-3 hours. 10 . A lithium secondary battery comprising the negative electrode active material according to claim 1 .