All-solid-state battery
By using an anode active material with a silicon clathrate type II crystal phase and appropriate constraint pressure, the problem of reduced capacity retention rate caused by volume changes of the Si anode during charge and discharge is solved, and full performance under low or no constraint pressure is achieved. The solid battery capacity maintenance rate is good and the battery structure is simplified.
Patent Information
- Application Number
- CN202111458455.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-02
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-12-02
AI Technical Summary
Si, as the negative active material, has a large volume change during charge and discharge, which leads to a decrease in the capacity maintenance rate of all-solid-state batteries, and requires high confinement pressure to maintain ion and electron conduction paths, resulting in the need for the use of large constraint fixtures.
Use a negative active material with silicon clathrate type II crystal phase, and apply a constraint pressure of 0MPa to 5MPa in the stacking direction to adjust the capacity ratio of the negative electrode capacity to the positive electrode capacity so that it can be maintained under no or low constraint pressure. Good capacity maintenance.
It achieves good capacity maintenance of all-solid-state batteries without or with low constraint pressure, avoids the need for large constraint fixtures, and simplifies the battery structure.
Smart Images

Figure CN114628781B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to all-solid-state batteries. Background Art
[0002] A fully solid-state battery is a battery having a solid electrolyte layer between a positive electrode layer and a negative electrode layer, and has the advantage of being easy to simplify safety devices compared to a liquid-based battery having an electrolyte containing a flammable organic solvent. In addition, Si-based active materials are known as active materials for fully solid-state batteries. For example, Patent Document 1 discloses a fully solid-state battery using a Si-containing active material as a negative electrode active material.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2017-112029 Summary of the invention
[0006] Problems to be solved by the invention
[0007] The theoretical capacity of Si is large, which is effective for the high energy density of the battery. On the other hand, the volume change of Si during charging and discharging is large, and the volume change of the electrode layer and the battery during charging and discharging using Si is large. If the volume change during charging and discharging is large, the ion conduction path and the electronic conduction path are easily cut off, and the capacity retention rate of the all-solid-state battery is easily reduced. In order to ensure the ion conduction path and the electronic conduction path, it is envisaged to give a high constraint pressure, but in order to give the constraint pressure, a constraint fixture is required, and in order to give a high constraint pressure, a large constraint fixture is required.
[0008] The present disclosure has been made in view of the above-mentioned actual situation, and a main object of the present disclosure is to provide an all-solid-state battery having a good capacity maintenance rate even when no confinement pressure is applied or a low confinement pressure is applied.
[0009] Means for solving problems
[0010] In the present disclosure, the following all-solid-state battery is provided, which is an all-solid-state battery having a positive electrode layer, a solid electrolyte layer and a negative electrode layer stacked in sequence, wherein the above-mentioned negative electrode layer contains a negative electrode active material having a silicon inclusion compound type II crystal phase, and the above-mentioned all-solid-state battery is given a constraint pressure of greater than 0 MPa and less than 5 MPa in the stacking direction, and when the capacity ratio of the negative electrode capacity to the positive electrode capacity is set to A, the above-mentioned capacity ratio A is greater than 2.5 and less than 4.8.
[0011] According to the present disclosure, by using a negative electrode active material having a silicon inclusion compound II-type crystal phase and setting the capacity ratio A to a predetermined range, an all-solid-state battery having a good capacity retention rate even when no confinement pressure or a low confinement pressure is applied is produced.
[0012] In the above disclosure, the above constraint pressure may be 2.5 MPa or less.
[0013] In the above disclosure, the capacity ratio A may be 4.1 or less.
[0014] In the above disclosure, the capacity ratio A may be 3.0 or more.
[0015] In the above disclosure, the all-solid-state battery may not have a restraining jig for imparting the restraining pressure.
[0016] In the above disclosure, when the negative electrode active material is subjected to X-ray diffraction measurement using CuKα rays, peaks are observed at positions of 2θ=20.09°±0.50° and 31.72°±0.50°.
[0017] Effects of the Invention
[0018] The present disclosure achieves the effect of being able to provide an all-solid-state battery having a good capacity retention rate even when no confinement pressure is applied or when a low confinement pressure is applied. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a schematic perspective view for explaining the crystal phase of Si.
[0020] Figure 2 This is a schematic cross-sectional view showing an example of an all-solid-state battery in the present disclosure.
[0021] Description of Reference Numerals
[0022] 1. Positive electrode layer
[0023] 2···Solid electrolyte layer
[0024] 3. Negative electrode layer
[0025] 4. Positive electrode collector
[0026] 5···Negative electrode collector
[0027] 6···Battery housing
[0028] 10···All-solid-state batteries DETAILED DESCRIPTION
[0029] Hereinafter, the all-solid-state battery in the present disclosure will be described in detail.
[0030] The all-solid-state battery disclosed in the present invention is an all-solid-state battery in which a positive electrode layer, a solid electrolyte layer and a negative electrode layer are stacked in sequence, wherein the negative electrode layer contains a negative electrode active material having a silicon clathrate (silicon clathrate) type II crystal phase, and the all-solid-state battery is given a constraint pressure of greater than 0 MPa and less than 5 MPa in the stacking direction. When the capacity ratio of the negative electrode capacity to the positive electrode capacity is set to A, the above capacity ratio A is greater than 2.5 and less than 4.8.
[0031] According to the present disclosure, by using a negative electrode active material having a silicon inclusion compound II-type crystal phase and setting the capacity ratio A to a predetermined range, an all-solid-state battery having a good capacity retention rate even when no confinement pressure or a low confinement pressure is applied is produced.
[0032] As mentioned above, Si is known as a negative electrode active material with a large theoretical capacity. Ordinary Si has a diamond-type crystal phase. Figure 1 As shown in (a), in the diamond-type Si crystal phase, a plurality of Si elements form tetrahedrons. The tetrahedrons have no space inside that can accommodate metal ions such as Li ions, and thus are prone to volume changes due to charge and discharge.
[0033] On the other hand, in the present disclosure, a negative electrode active material having a silicon inclusion compound II type crystal phase is used. Figure 1 As shown in (b), in the silicon inclusion compound II type crystal phase, a polyhedron (cage) including pentagons or hexagons is formed by multiple Si elements. The polyhedron has a space inside that can accommodate metal ions such as Li ions. By inserting metal ions into this space, the volume change caused by charging and discharging can be suppressed.
[0034] Furthermore, in the present disclosure, by using a negative electrode active material having a silicon inclusion compound II type crystal phase and making the capacity ratio A within a specified range, a good capacity retention rate can be obtained even when no constraint pressure is applied or a low constraint pressure is applied. In particular, in the embodiments described later, even if no constraint pressure is applied, a capacity retention rate equivalent to that when a constraint pressure of 5 MPa is applied can be achieved. As a constraint pressure of a conventional all-solid-state battery, a constraint pressure of 5 MPa is equivalent to a relatively low pressure, but it is also equivalent to 500 t / m 2 The case where such a constraint pressure is applied and the case where no constraint pressure is applied can achieve the same capacity maintenance rate, which can be said to be a significant effect. Furthermore, the all-solid-state battery disclosed in the present invention has the advantage of not requiring the installation of a large constraint fixture and being able to simplify the structure of the all-solid-state battery.
[0035] 1. Constraint pressure and capacity ratio
[0036] The all-solid battery in the present disclosure is given a constraint pressure of more than 0MPa and less than 5MPa in the stacking direction. The constraint pressure can be given using a constraint fixture described later. Here, "0MPa constraint pressure" means that no constraint pressure is given. As an example of a situation where the constraint pressure is 0MPa, there can be cited a situation where the all-solid battery does not have a constraint fixture, a situation where the all-solid battery has a constraint fixture but no constraint pressure is given, a situation where the interior of the laminated cell is vacuumed so as to utilize atmospheric pressure constraints, etc.
[0037] The restraining pressure may be 0 MPa or may be greater than 0 MPa. In the latter case, the restraining pressure is, for example, 0.1 MPa or more, or 0.5 MPa or more. On the other hand, the restraining pressure is usually less than 5 MPa, and may be 4.5 MPa or less, 3 MPa or less, 2.5 MPa or less, or 1.0 MPa or less.
[0038] In addition, in the present disclosure, the capacity ratio of the negative electrode capacity to the positive electrode capacity is set to A. The capacity ratio A is generally greater than 2.5 and may be greater than 3.0. When the capacity ratio A is too small, a good capacity retention rate may not be obtained. On the other hand, the capacity ratio A is generally less than 4.8 and may be less than 4.1. When the capacity ratio A is too large, a good volume energy density may not be obtained. The negative electrode capacity can be obtained by multiplying the amount of the negative electrode active material by the theoretical capacity of the negative electrode active material. On the other hand, the positive electrode capacity can be obtained by multiplying the amount of the positive electrode active material by the charging capacity of the positive electrode active material. With respect to the charging capacity of the positive electrode active material, a monopolar powder battery cell using metal Li as the counter electrode is prepared, and CCCV charging (1 / 100C cutoff or 20 hours cutoff) is performed at 0.1C, and the obtained initial charging capacity is set as the charging capacity of the positive electrode active material. The capacity ratio A can be adjusted by changing the ratio of the positive electrode active material to the negative electrode active material. Specifically, it can be adjusted by changing the thickness of at least one layer of the positive electrode layer and the negative electrode layer.
[0039] 2. The composition of all-solid-state batteries
[0040] Figure 2 This is a schematic cross-sectional view showing an example of an all-solid-state battery in the present disclosure. Figure 2 In the all-solid battery 10 shown, a positive electrode layer 1, a solid electrolyte layer 2, and a negative electrode layer 3 are sequentially stacked. In addition, the all-solid battery 10 has a positive electrode collector 4 for collecting current from the positive electrode layer 1, a negative electrode collector 5 for collecting current from the negative electrode layer 3, and a battery case 6 for housing these components.
[0041] (1) Negative electrode layer
[0042] The negative electrode layer in the present disclosure contains a negative electrode active material having a silicon inclusion compound II type crystal phase. In addition, the negative electrode layer may contain at least one of a conductive material, a binder, and a solid electrolyte as required.
[0043] The negative electrode active material has a silicon inclusion compound type II crystal phase. The silicon inclusion compound type II crystal phase generally belongs to the space group (Fd-3m). The silicon inclusion compound type II crystal phase has typical peaks at 2θ=20.09°, 21.00°, 26.51°, 31.72°, 36.26°, and 53.01° in the X-ray diffraction measurement using CuKα rays. Each of these peak positions can be offset in the range of ±0.50°, in the range of ±0.30°, or in the range of ±0.10°.
[0044] The negative electrode active material preferably has a silicon clathrate type II crystal phase as a main phase. “Having a silicon clathrate type II crystal phase as a main phase” means that a peak belonging to the silicon clathrate type II crystal phase has the highest diffraction intensity among the peaks observed by X-ray diffraction measurement.
[0045] In the silicon inclusion compound II type crystal phase, the peak at 2θ=20.09°±0.50° is designated as peak A, and the peak at 2θ=31.72°±0.50° is designated as peak B. In addition, the intensity of peak A is designated as I A , set the intensity of peak B to I B On the other hand, the maximum intensity at 2θ = 22° to 23° is defined as I M 2θ=22° to 23° is a range in which the peak of a crystal phase generally associated with Si does not appear, and thus can be used as a reference.
[0046] I A / I M The value of is preferably greater than 1. A / I M When the value of is less than 1, it can be judged that the silicon inclusion compound II type crystal phase is not substantially formed. A / I M The value of is, for example, 2 or more, 5 or more, or 7 or more. A / I M There is no particular upper limit on the value of A / I M becomes greater than 1000).
[0047] I B / I M The value of is preferably greater than 1. B / I M When the value of is 1 or less, it can be judged that the silicon inclusion compound II type crystal phase is not substantially formed. B / I M The value of is, for example, greater than 2, and may be greater than 5. B / I M There is no particular upper limit on the value of B / I M becomes greater than 1000).
[0048] In addition, the negative electrode active material may or may not have a silicon inclusion compound type I crystal phase. "Not having a crystal phase" can be confirmed by not confirming the peak of the crystal phase in the X-ray diffraction measurement. The silicon inclusion compound type I crystal phase usually belongs to the space group (Pm-3n). The silicon inclusion compound type I crystal phase has typical peaks at 2θ=19.44°, 21.32°, 30.33°, 31.60°, 32.82°, 36.29°, 52.39°, and 55.49° in the X-ray diffraction measurement using CuKα rays. Each of these peak positions can be offset in the range of ±0.50°, can be offset in the range of ±0.30°, and can be offset in the range of ±0.10°.
[0049] In addition, the negative electrode active material may have a diamond-type Si crystal phase or may not have it, preferably the latter. The diamond-type Si crystal phase has typical peaks at 2θ=28.44°, 47.31°, 56.10°, 69.17°, and 76.37° in the X-ray diffraction measurement using CuKα rays. Each of these peak positions can be offset in the range of ±0.50°, in the range of ±0.30°, or in the range of ±0.10°.
[0050] As the shape of the negative electrode active material, for example, a particle shape can be cited. The active material can be a primary particle or a secondary particle formed by aggregation of primary particles. The average particle size of the primary particles is, for example, greater than 50 nm, greater than 100 nm, or greater than 150 nm. On the other hand, the average particle size of the primary particles can be, for example, less than 3000 nm, less than 1500 nm, or less than 1000 nm. In addition, the average particle size of the secondary particles can be, for example, greater than 1 μm, greater than 2 μm, or greater than 5 μm. On the other hand, the average particle size of the secondary particles can be, for example, less than 60 μm, or less than 40 μm. It should be noted that the average particle size can be obtained, for example, by observation using an SEM. The number of samples is preferably large, for example, greater than 20, greater than 50, or greater than 100.
[0051] The negative electrode active material may have voids inside the primary particle. As described above, the silicon inclusion compound II type crystal phase has a cage that can contain metal ions such as Li ions, so that the volume change caused by charging and discharging can be suppressed. If the primary particle having this crystal phase has voids inside, the voids also help to suppress the volume change, so the volume change caused by charging and discharging can be further suppressed. As a result, the constraint pressure of the all-solid-state battery can be further reduced. The negative electrode active material preferably contains a large number of tiny voids with a pore diameter of less than 100nm. This is because the collapse of the voids caused by pressing can be suppressed. The void amount of the void with a pore diameter of less than 100nm is, for example, more than 0.05cc / g, can be more than 0.07cc / g, or can be more than 0.10cc / g. On the other hand, the above-mentioned void amount is, for example, less than 0.15cc / g. The void amount can be obtained, for example, by mercury porosimetry, BET measurement, gas adsorption method, 3D-SEM, and 3D-TEM. In addition, the negative electrode active material does not need to have voids inside the primary particles.
[0052] When the negative electrode active material has voids inside the primary particles, the void ratio is, for example, 4% or more, or 10% or more. Alternatively, the void ratio is, for example, 40% or less, or 20% or less.
[0053] The composition of the negative electrode active material is not particularly limited, but is preferably composed of Na x Si 136 (0≤x≤24). x may be 0 or greater than 0. On the other hand, x may be 10 or less or 5 or less. It should be noted that the negative electrode active material may contain unavoidable components (such as Li, C and O). The composition of the active material can be obtained, for example, by EDX, XRD, XRF, ICP, or atomic absorption spectrometry.
[0054] The method for producing the negative electrode active material in the present disclosure is not particularly limited, and an example includes a method comprising: a synthesis step of synthesizing a Zintl compound containing Na and Si and having a Zintl phase; and a removal step of removing the Na from the Zintl compound.
[0055] In the synthesis process, for example, a Zintl compound can be obtained by heat treating a raw material mixture containing Na (single substance) and Si (single substance). In terms of the ratio of Na (single substance) to Si (single substance), Na (single substance) is, for example, 0.8 mol parts or more and 1.5 mol parts or less relative to 1 mol part of Si (single substance). The heat treatment temperature is, for example, 500° C. or more and 1000° C. or less. The heat treatment time is, for example, 1 hour or more and 50 hours or less.
[0056] In the removal step, Na is removed from the Zintl compound by, for example, heat treatment. The heat treatment temperature is, for example, 280° C. to 500° C. The heat treatment time is, for example, 1 hour to 50 hours. The heat treatment may be performed under normal pressure or under reduced pressure.
[0057] The negative electrode active material having voids inside the primary particle can be obtained, for example, by reacting a precursor active material having a silicon inclusion compound II type crystal phase with Li to form an alloy compound, and then removing Li from the alloy compound. Examples of Li extraction materials for removing Li include alcohols such as ethanol and acids such as acetic acid.
[0058] In addition, the proportion of the negative electrode active material in the negative electrode layer is, for example, 20% by weight or more, 30% by weight or more, 40% by weight or more, or 60% by weight or more. When the proportion of the negative electrode active material is too small, sufficient energy density may not be obtained. On the other hand, the proportion of the negative electrode active material is, for example, 80% by weight or less, or 70% by weight or less. When the proportion of the negative electrode active material is too much, the ionic conductivity and electronic conductivity in the negative electrode layer may decrease relatively.
[0059] When the negative electrode layer contains a solid electrolyte, the weight ratio of the negative electrode active material to the solid electrolyte (negative electrode active material:solid electrolyte) is, for example, 85:15 to 30:70, or 80:20 to 40:60.
[0060] As a solid electrolyte, for example, the solid electrolyte described in "(3) Solid electrolyte layer" described later can be cited. As a conductive material, for example, a carbon material, a metal particle, and a conductive polymer can be cited. As a carbon material, for example, a particulate carbon material such as acetylene black (AB) and Ketjen black (KB), a fibrous carbon material such as a carbon fiber, a carbon nanotube (CNT), and a carbon nanofiber (CNF) can be cited. In addition, as an adhesive, for example, a rubber-based adhesive and a fluoride-based adhesive can be cited.
[0061] The thickness of the negative electrode layer is, for example, 0.1 μm or more and 1000 μm or less, 1 μm or more and 100 μm or less, or 30 μm or more and 100 μm or less.
[0062] (2) Positive electrode layer
[0063] The positive electrode layer in the present disclosure is a layer having at least a positive electrode active material. In addition, the positive electrode layer may contain at least one of a solid electrolyte, a conductive material, and a binder as necessary.
[0064] Examples of the positive electrode active material include oxide active materials. Examples of the oxide active material include LiCoO2, LiMnO2, LiNiO2, LiVO2, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 and other rock salt layered active materials, LiMn2O4, Li4Ti5O 12 、Li(Ni 0.5 Mn 1.5 )O4 and other spinel active materials, LiFePO4, LiMnPO4, LiNiPO4, LiCoPO4 and other olivine active materials.
[0065] A coating containing a Li ion conductive oxide may be formed on the surface of the oxide active material. This is because the reaction between the oxide active material and the solid electrolyte (especially the sulfide solid electrolyte) can be suppressed. Examples of Li ion conductive oxides include LiNbO3, Li4Ti5O 12 The thickness of the coating layer is, for example, not less than 1 nm and not more than 30 nm. In addition, as the positive electrode active material, for example, Li2S can also be used.
[0066] The types of solid electrolyte, conductive material and binder used in the positive electrode layer are the same as those described in the above-mentioned "(1) Negative electrode layer", so the description here is omitted. It should be noted that when the positive electrode layer contains a solid electrolyte, the weight ratio of the positive electrode active material to the solid electrolyte (positive electrode active material: solid electrolyte) is, for example, 85:15 to 30:70, and can be 80:20 to 50:50.
[0067] The thickness of the positive electrode layer is, for example, 0.1 μm or more and 1000 μm or less, 1 μm or more and 100 μm or less, or 30 μm or more and 100 μm or less.
[0068] (3) Solid electrolyte layer
[0069] The solid electrolyte layer in the present disclosure is a layer formed between the positive electrode layer and the negative electrode layer, and contains at least a solid electrolyte. In addition, the solid electrolyte layer may further contain a binder as required. The type of binder is the same as that described in the above-mentioned "(1) negative electrode layer", so the description here is omitted.
[0070] As solid electrolytes, inorganic solid electrolytes such as sulfide solid electrolytes, oxide solid electrolytes, nitride solid electrolytes, and halide solid electrolytes can be cited. As sulfide solid electrolytes, for example, solid electrolytes containing Li element, X element (X is at least one of P, As, Sb, Si, Ge, Sn, B, Al, Ga, In) and S element can be cited. In addition, the sulfide solid electrolyte may further contain at least one of O element and halogen element. As halogen elements, for example, F element, Cl element, Br element, and I element can be cited. The sulfide solid electrolyte can be glass (amorphous) or glass ceramic. As sulfide solid electrolytes, for example, Li2S-P2S5, LiI-Li2S-P2S5, LiI-LiBr-Li2S-P2S5, Li2S-SiS2, Li2S-GeS2, and Li2S-P2S5-GeS2 can be cited.
[0071] The thickness of the solid electrolyte layer is, for example, 0.1 μm to 1000 μm, may be 0.1 μm to 300 μm, or may be 0.1 μm to 100 μm.
[0072] (4) Constraint fixture
[0073] The all-solid battery in the present disclosure may further have a constraint fixture that imparts a constraint pressure along the thickness direction of the all-solid battery, or may not have it. In particular, the all-solid battery in the present disclosure preferably does not have a constraint fixture. In the absence of a constraint fixture, the structure of the all-solid battery is more simplified, and the energy density of the battery as a whole is further improved.
[0074] The constraint pressure when the all-solid battery does not have a constraint fixture is usually 0MPa. On the other hand, the constraint pressure when the all-solid battery has a constraint fixture is usually greater than 0MPa. It should be noted that even with a constraint fixture, the constraint pressure can be 0MPa. Regarding the specific constraint pressure, it is the same as the content recorded in "1. Constraint pressure and capacity ratio", so the record here is omitted.
[0075] The type of the restraining jig is not particularly limited, and examples thereof include a restraining jig that applies a restraining torque using a bolt.
[0076] (5) Other components
[0077] The all-solid-state battery disclosed in the present invention preferably has a positive electrode collector for collecting the positive electrode layer, a negative electrode collector for collecting the negative electrode layer, and a battery case for accommodating the above-mentioned components. As the material of the positive electrode collector, SUS, Ni, Cr, Au, Pt, Al, Fe, Ti, Zn, etc. can be mentioned. In addition, a coating of Ni, Cr, C, etc. can be formed on the surface of the positive electrode collector. The coating can be, for example, a plating layer or a vapor-deposited layer. On the other hand, as the material of the negative electrode collector, for example, Cu and Cu alloys can be mentioned. A coating of Ni, Cr, C, etc. can be formed on the surface of the negative electrode collector. The coating can be, for example, a plating layer or a vapor-deposited layer. As the battery case, a conventionally known case can be used.
[0078] (6) All-solid-state batteries
[0079] The type of all-solid-state battery in the present disclosure is not particularly limited, and is typically a lithium-ion battery. In addition, the all-solid-state battery in the present disclosure may be a primary battery or a secondary battery, wherein a secondary battery is preferred. This is because it can be repeatedly charged and discharged, and is useful, for example, as a vehicle-mounted battery.
[0080] The all-solid battery in the present disclosure may be a single cell or a stacked battery. The stacked battery may be a monopolar stacked battery (parallel-connected stacked battery) or a bipolar stacked battery (series-connected stacked battery). As the shape of the all-solid battery, for example, a coin-shaped, laminated, cylindrical, or square shape may be cited.
[0081] It should be noted that the present disclosure is not limited to the above-mentioned embodiments. The above-mentioned embodiments are illustrative, and embodiments having substantially the same structure and achieving the same effects as the technical concept described in the patent claims of the present disclosure are all within the technical scope of the present disclosure.
[0082] Example
[0083] [Example 1]
[0084] (Preparation of negative electrode active material)
[0085] Si particles and Na particles were mixed in a molar ratio of 1:1 and heated at 700°C to synthesize NaSi (Zintl compound). Then, the Zintl compound was heated at 340°C to remove Na. Then, additional heating was performed at 430°C to further remove Na. Thus, a negative electrode active material was prepared.
[0086] (Production of negative electrode)
[0087] A dispersion medium (butyl butyrate), a binder (5 wt% butyl butyrate solution of a PVDF-based binder), the above-prepared negative electrode active material, a sulfide solid electrolyte (Li2S-P2S5-based glass ceramic) and a conductive material (VGCF) were added to a polypropylene (PP) container and stirred for 30 seconds using an ultrasonic dispersion device (UH-50 manufactured by Esumetech). Next, the container was vibrated for 30 minutes using a vibrator (TTM-1 manufactured by Shibata Science Co., Ltd.) to prepare a negative electrode composition. The negative electrode composition was applied to a negative electrode collector (Cu foil, manufactured by UACJ) using a doctor blade method using an applicator to form a coating layer. The coating layer was dried on a hot plate at 100°C for 30 minutes. Thus, a negative electrode having a negative electrode collector and a negative electrode layer was prepared. In addition, when the negative electrode was prepared, the thickness of the negative electrode layer was adjusted in such a way as to obtain a specified capacity ratio A.
[0088] (Production of positive electrode)
[0089] A dispersion medium (butyl butyrate), a binder (5 wt% butyl butyrate solution of a PVDF-based binder), a positive electrode active material (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, average particle size 6μm), sulfide solid electrolyte (Li2S-P2S5 glass ceramic) and conductive material (VGCF), stirred for 30 seconds with an ultrasonic disperser (UH-50 manufactured by Esu Emtech). Next, the container was vibrated for 3 minutes with a vibrator (TTM-1 manufactured by Shibata Science Co., Ltd.), stirred for 30 seconds with an ultrasonic disperser, and then vibrated for 3 minutes with an oscillator, thereby preparing a positive electrode composition. The positive electrode composition was applied to the positive electrode collector (Al foil, manufactured by Showa Denko) by a doctor blade method using an applicator to form a coating layer. Thereafter, the coating layer was dried on a hot plate at 100°C for 30 minutes. Thus, a positive electrode having a positive electrode collector and a positive electrode layer was produced. It is to be noted that the positive electrode area is made smaller than the negative electrode area.
[0090] (Fabrication of Solid Electrolyte Layer)
[0091] A dispersion medium (heptane), a binder (5wt% heptane solution of a BR-based binder) and a sulfide solid electrolyte (Li2S-P2S5-based glass ceramic) were added to a PP container and stirred for 30 seconds using an ultrasonic disperser (UH-50 manufactured by Esumetech). Next, the container was vibrated for 30 minutes using a vibrator (TTM-1 manufactured by Shibata Science Co., Ltd.) to prepare a solid electrolyte composition. The solid electrolyte composition was applied to a release sheet (Al foil) using an applicator by a doctor blade method to form a coating layer. Thereafter, the coating layer was dried on a hot plate at 100°C for 30 minutes. Thus, a transfer component having a release sheet and a solid electrolyte layer was obtained.
[0092] (Fabrication of all-solid-state batteries)
[0093] A solid electrolyte layer for bonding was placed on the positive electrode layer of the positive electrode, and the mixture was placed on a roll press and pressed at 20 kN / cm (about 710 MPa) and 165° C. Thus, a first laminate was obtained.
[0094] Next, the negative electrode was placed on a roller press and pressed at 20 kN / cm (about 630 MPa) and 25°C. Thereafter, the solid electrolyte layer for bonding and the transfer member were sequentially arranged starting from the negative electrode layer side. At this time, the solid electrolyte layer for bonding was arranged in a manner opposite to the solid electrolyte layer in the transfer member. The obtained laminate was placed on a flat uniaxial press and pre-pressed at 100 MPa and 25°C for 10 seconds. Thereafter, the release sheet was peeled off from the solid electrolyte layer. Thus, a second laminate was obtained.
[0095] Next, the solid electrolyte layer for bonding in the first stack and the solid electrolyte layer in the second stack were arranged in a manner opposite to each other, and were placed in a flat uniaxial press and pressed at 200 MPa and 135° C. for 1 minute. Thus, a fully solid-state battery was obtained. It should be noted that the fully solid-state battery produced was not constrained by a constraining fixture.
[0096] [Examples 2 to 4]
[0097] Except that the capacity ratio A was changed to the value shown in Table 1, the same operation as in Example 1 was carried out to produce an all-solid-state battery.
[0098] [Comparative Example 1]
[0099] An all-solid-state battery was produced in the same manner as in Example 1 except that Si particles (diamond-type Si) were used as the negative electrode active material, the capacity ratio A was changed to the value shown in Table 1, and the restraining jig was used to restrain the battery at a restraining pressure of 5 MPa.
[0100] [Comparative Example 2]
[0101] An all-solid-state battery was produced in the same manner as in Comparative Example 1 except that the restraining jig was not used.
[0102] [Comparative Example 3]
[0103] Except that the capacity ratio A was changed to the value shown in Table 1, the same operation as in Comparative Example 2 was carried out to produce an all-solid-state battery.
[0104] [Comparative Example 4]
[0105] Except that the capacity ratio A was changed to the value shown in Table 1, the same operation as in Example 1 was carried out to produce an all-solid-state battery.
[0106] [Comparative Examples 5 and 6]
[0107] An all-solid-state battery was produced in the same manner as in Example 1 except that the capacity ratio A was changed to a value shown in Table 1 and the restraining jig was used for restraining at a restraining pressure of 5 MPa.
[0108] [evaluate]
[0109] (XRD measurement)
[0110] The negative electrode active material obtained in Example 1 was subjected to X-ray diffraction (XRD) measurement using CuKα rays. As a result, characteristic peaks of silicon inclusion compound type II were obtained, confirming that the negative electrode active material obtained in Example 1 had silicon inclusion compound type II crystal phase as the main phase. In addition, I was obtained from the XRD data. A / I M and I B / I M , are all greater than 1.
[0111] (Charge and discharge test)
[0112] For each all-solid-state battery prepared in Examples 1 to 4 and Comparative Examples 1 to 6, a constant current-constant voltage charge was performed to 4.55V at a rate of 1 / 10C for 10 hours, and a constant current-constant voltage discharge was performed to 3.0V at a rate of 1C for 1 hour. Thereafter, a constant current-constant voltage charge was performed to 4.35V at a rate of 3 hours (1 / 3C), and a constant current-constant voltage discharge was performed to 3.00V at a rate of 3 hours (1 / 3C), and the initial discharge capacity was calculated. This cycle was repeated 5 times, and the discharge capacity after 5 cycles was calculated. The discharge capacity after 5 cycles was divided by the initial discharge capacity to calculate the capacity retention rate. The results are shown in Table 1.
[0113]
Table 1
[0114]
[0115] As shown in Table 1, in Comparative Example 1 using conventional Si (diamond-type Si), the capacity retention rate was high because the constraint pressure of 5 MPa was applied, but in Comparative Example 2, the capacity retention rate was greatly reduced because the constraint pressure was not applied. In addition, in Comparative Example 3, since the capacity ratio A was made smaller than that in Comparative Example 2, Si underwent a large volume change during charge and discharge, and the capacity retention rate was further reduced.
[0116] On the other hand, in Examples 1 to 4 using Si having a clathrate II-type crystal phase and no constraint pressure, the capacity retention rate was slightly lower than that of Comparative Examples 5 and 6 having a constraint pressure of 5 MPa, but a good capacity retention rate of more than 94% was obtained. Therefore, by using a negative electrode active material having a silicon clathrate II-type crystal phase and making the capacity ratio A within a specified range, an all-solid-state battery with a good capacity retention rate can be obtained even when no constraint pressure is applied or a low constraint pressure is applied.
Claims
1. All-solid-state battery, which is an all-solid-state battery with a positive electrode layer, a solid electrolyte layer and a negative electrode layer stacked in sequence, wherein: The negative electrode layer contains a negative electrode active material having a silicon inclusion compound II type crystal phase as a main phase, The above negative electrode active material is composed of Na x Si 136 means, where 0≤x≤24, The all-solid-state battery is given a constraint pressure of 0 MPa or more and less than 5 MPa in the stacking direction. When the capacity ratio of the negative electrode capacity to the positive electrode capacity is represented by A, the capacity ratio A is 2.5 or more and 4.8 or less.
2. The all-solid-state battery according to claim 1, wherein: The above-mentioned restraint pressure is 2.5 MPa or less.
3. The all-solid-state battery according to claim 1 or 2, wherein: The above-mentioned capacity ratio A is 4.1 or less.
4. The all-solid-state battery according to claim 1 or 2, wherein: The above-mentioned capacity ratio A is 3.0 or more.
5. The all-solid-state battery according to claim 1 or 2, wherein: The all-solid-state battery does not have a restraining jig for applying the restraining pressure.
6. The all-solid-state battery according to claim 1 or 2, wherein: When the negative electrode active material was subjected to X-ray diffraction measurement using CuKα rays, peaks were observed at positions of 2θ=20.09°±0.50° and 31.72°±0.50°.
Citation Information
Patent Citations
Battery system
JP2017112029A
All-solid-state battery and manufacturing method therefor
CN110249467A
Active material, battery and method for producing active material
CN111261867A
Lithium ion secondary battery and method for manufacturing the same
JP2011054324A
All-solid-state lithium ion battery
JP2018106984A