A method for evaluating the permeability of asphalt pavement sealing materials
By measuring void ratio changes and weighting assignment calculations on cylindrical specimens of asphalt pavement sealing materials, the problem of difficulty in evaluating permeability performance in the existing technology is solved, and rapid, unified evaluation and effective permeability assessment of sealing materials are achieved. .
Patent Information
- Application Number
- CN202210320439.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-29
- Publication Date
- 2024-10-25
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
It is difficult to effectively evaluate the permeability performance of asphalt pavement seal materials with existing technology, resulting in the material remaining on the road surface, making it impossible to restore the performance degradation of old asphalt pavement.
By preparing a cylindrical specimen, apply the sealing material and let it stand for 24 hours, take cores and cut thin slices, measure the change in void ratio, calculate the permeability value, and use the weight assignment method for unified evaluation.
It achieves a rapid and unified evaluation of the permeability of sealing material, and can intuitively compare the permeability of each sealing material to ensure that the material can effectively penetrate into the road surface and restore the performance of aging asphalt.
Smart Images

Figure CN114636656B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for evaluating the permeability of an asphalt pavement sealing material. Background Art
[0002] With the rapid development of highway construction in my country, the road maintenance mileage continues to increase, resulting in a relative shortage of maintenance funds and a low maintenance level. To change the current passive maintenance situation, the most effective way is to implement preventive maintenance. Preventive maintenance is a periodic maintenance measure. It is a planned and relatively economical maintenance strategy for the existing road system when the road surface is in good condition. The purpose is to prevent the further development of early minor road diseases and delay the attenuation of road performance. It is usually suitable for roads that are not damaged or have only minor defects and diseases. It can also be said that preventive maintenance refers to the application of the most appropriate preventive maintenance measures at the most appropriate time in the early stage of road condition attenuation, with the minimum life cycle cost, to the greatest extent possible to delay road condition degradation.
[0003] Common preventive maintenance technologies such as regeneration seal, fog seal, asphalt regeneration, etc., are achieved by spraying the above materials onto the asphalt pavement, which then penetrates into the interior of the pavement. Through the physical and chemical action of the seal material and the aged asphalt, the properties of the aged asphalt binder are restored, and the functional damage of the asphalt pavement is improved. It closes micro-cracks in the pavement, prevents the fall of loose stones, and blocks the infiltration of water, thereby significantly improving the appearance of the pavement, extending the service life of the asphalt pavement, and extending the major and medium repair cycle of the pavement.
[0004] The basic premise for these materials and technologies to work is that they must have good permeability and be able to penetrate into the asphalt pavement. Poor permeability will cause the material to remain on the road surface, reduce the pavement structure depth, and fail to achieve the effect of restoring the performance degradation of the old asphalt pavement. Therefore, it is very important to uniformly evaluate the permeability of sealing materials. Summary of the invention
[0005] The purpose of the present invention is to solve the defects in the prior art and provide a method for quickly and uniformly evaluating the permeability of sealing materials.
[0006] In order to achieve the above object, the present invention provides a method for evaluating the permeability of asphalt pavement sealing materials, the evaluation method comprising the following steps:
[0007] (1) Two groups of cylindrical specimens were prepared according to the standard gradation of the asphalt pavement to be sealed;
[0008] (2) Two groups of cylindrical specimens, one group is used as test specimens, and the sealing material to be tested is evenly applied to the center of the top surface of the specimens. The evenly applied specimens are left to cure at room temperature for 24 hours; the other group is used as standard specimens and is not treated in any way;
[0009] (3) According to the smeared part of the test sample, the two groups of test pieces are cored and cut respectively:
[0010] The core sample of each test piece is cut to remove the 10mm thick part of the surface, and then two layers of thin sheets with a thickness of 15mm are cut from top to bottom. The average value of the porosity of the two layers of thin sheets of each group of samples is tested respectively, and the change of the porosity of the two layers of thin sheets of the test sample relative to the standard sample is calculated to evaluate the permeability of the sealing material:
[0011] The greater the reduction in the void ratio of the two thin sheets of the test sample, the better the permeability of the sealing material to be tested.
[0012] The present invention evaluates the permeability performance by the influence of the sealing material on the porosity of the road test piece; and according to the requirements for the permeability performance of the sealing material, comprehensively considers the influence on the porosity of the 10-40mm thickness part below the surface of the road test piece, calculates the porosity reduction value after applying the sealing material by layer, and uniformly evaluates the permeability performance of the sealing material.
[0013] In some embodiments, as a preferred method, the calculation method of the porosity change of the two-layer thin sheets of the test sample relative to the standard sample in step (3) is as follows: the porosity of the sampled thin sheets of each core sample is tested respectively, and the average value thereof is calculated, and the average porosity of the first layer (after removing the 10 mm thick portion of the surface) of the sampled thin sheet of the standard sample is recorded as V1V b The average porosity of the second layer of sample slices is recorded as V2V b The average porosity of the first layer of the sample is recorded as V1V a The average gap ratio of the second layer of sample slices is recorded as V2V a , V1V a 、V2V a 、V1V b 、V2V b The unit is %, and the permeability value is calculated by measuring the change of void ratio;
[0014] The calculation formula of the permeability value n is as follows:
[0015] n=K1×(10×(V1V b -V1V a )+60)+K2×(10×(V2V b -V2V a )+60),
[0016] Wherein, K1 and K2 represent the weights of the change of the void ratio of the first layer and the change of the void ratio of the second layer, respectively.
[0017] The present invention examines the requirements of the sealing material on the permeability of each layer and assigns weights to the change values of the void ratio of each layer, thereby achieving a unified and intuitive evaluation of the permeability performance of the sealing material.
[0018] In some embodiments, preferably, K1 takes a value of 0.6 and K2 takes a value of 0.4.
[0019] Furthermore, in step (1), the cylindrical specimen is formed by a rotary compaction method, the void ratio is 4%, the diameter of the cylindrical specimen is 150 mm, and the height is 100-120 mm; in step (2), the sealing material to be tested is applied to a circular portion with a diameter of 100 mm and a center at the center of the top surface of the test sample; and in step (3), a coring machine with a diameter of 100 mm is used to coring the applied portion of the test sample and the corresponding portion of the standard sample.
[0020] The present invention applies sealing material to the central part of the cylindrical test piece, thereby avoiding the influence of penetration from the peripheral side of the test piece on the porosity after the sealing material is completely applied to the top surface, so that the calculation of the permeability value is more accurate.
[0021] Compared with the prior art, the present invention has the following advantages:
[0022] The present invention uniformly and quickly evaluates the permeability of the sealing material by calculating the change in the porosity of the pavement sample after the sealing material is applied; and calculates the permeability value of the sealing material by assigning weights to the change in the porosity of each layer, thereby intuitively and effectively comparing the permeability of each sealing material. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a schematic diagram of the core sample cutting according to the present invention. DETAILED DESCRIPTION
[0024] The present invention is described in detail below with reference to specific embodiments.
[0025] Example 1
[0026] The evaluation method of the permeability of the asphalt pavement sealing material of the present invention is as follows:
[0027] 1. Select a standard gradation of asphalt surface layer, and use the rotary compaction method to form 12 cylindrical specimens with a void ratio of 4%, a diameter of 150 mm, and a height of 100-120 mm. The theoretical maximum relative density is calculated to be 2.635.
[0028] Gradation composition
[0029]
[0030] 2. Use chalk to draw a circle with a diameter of 100 mm at the center of the top surface of each specimen.
[0031] 3. Randomly divide the 12 specimens into 2 groups, each with 6 specimens. Number the two groups of specimens as Group A and Group B respectively.
[0032] 4. Take the sealing material (emulsion, the concentration of the emulsion is suitable for direct construction on the road surface) and pour it into a measuring cup, and measure the required amount (the required amount is determined by the sealing material and the properties of the road surface, and it is appropriate to have a little residue on the surface after evenly applying it for 15 minutes). Group A specimens are used as test samples, and the weighed sealing emulsion is poured into a circle with a central diameter of 100mm, and evenly applied with a brush. The evenly applied specimens are left to stand at room temperature for 24 hours. Group B specimens are used as standard samples and are not treated in any way.
[0033] 5. Use a coring machine with a diameter of 100 mm to coring the two groups of specimens A and B respectively (the coring part is the part covered by the 100 mm circle drawn in step 2), and cut them, such as Figure 1 As shown. Cut off the top surface with a thickness of 10 mm, cut the upper two layers of circular slices according to 15 mm per layer, collect the two layers of slices, and measure their void ratios VV respectively (wherein, the void ratio VV test is carried out in accordance with the T0706-2011 compacted asphalt mixture density test (water weight method) test in JTG E20-2011 "Test Procedures for Asphalt and Asphalt Mixtures for Highway Engineering").
[0034] 6. Calculate the average porosity V1V of the first and second thin sheets of group A specimens and the first and second thin sheets of group B specimens respectively. a 、V2V a 、V1V b 、V2V b , calculate the change of the void ratio VV of the first and second thin sheets of group A specimens relative to the void ratio VV of the original group B specimen sheet. When the void ratio VV of each layer decreases by more than 1%, it indicates that the permeable sealing material emulsion sample has good permeability.
[0035] This example uses LRS-1 (Sujiaoke Group Co., Ltd.) as the sealing material to evaluate the permeability performance:
[0036] V1V a % = 1.1%, V1V b % = 4.1%, the porosity of the first layer of sample slice changes to V1V b %-V1V a % = 4.1% - 1.1% = 3.0%;
[0037] V2Va % = 1.7%, V2V b % = 4.2%, the porosity of the second layer of sample slice changes to V2V b %–V2V a % = 2.5%;
[0038] The porosity changes of the above two layers of sampling slices are both greater than 1%, indicating that the sealing material has good permeability.
[0039] Example 2
[0040] The following examples use two sealing materials, LRS-1 (Sujiaoke Group Co., Ltd.) and SBS modified emulsified asphalt, to evaluate the permeability performance. The preparation, grouping, coring, slice cutting and average porosity calculation of the samples are the same as those in Example 1.
[0041] The permeability value (n) of each sealing material is calculated. The larger the permeability value (n), the better the permeability effect of the sealing material.
[0042] n=K1*A1+K2*A2
[0043] Where:
[0044] The value of K1 is 0.60, and the value of K2 is 0.40
[0045] A1 and A2 refer to the reduction in the void ratio of each layer of the test sample relative to the standard sample, and take the value according to the table below. When the calculated reduction in void ratio is not an integer, the corresponding score is determined by interpolation.
[0046]
[0047]
[0048] The calculation formula is as follows:
[0049] n=K1×(10×(V1V b -V1V a )+60)+K2×(10×(V2V b -V2V a )+60),
[0050] Among them, the porosity reduction value of the first layer of the modified emulsified asphalt sealing material test sample and the porosity reduction value of the second layer of the sheet are 1.5 and 1.0 respectively (corresponding to the scores A1 and A2 are 75 and 70 respectively), then the permeability value n of the sealing material 甲 (%) = 0.6*75+0.4*70 = 73%.
[0051] The porosity reduction values of the first and second layers of the LRS-1 sealing material test sample are 3.0 and 2.5 respectively (corresponding to the scores A1 and A2 of 90 and 85 respectively). The permeability value of the sealing material is n 乙 (%) = 0.6*90+0.4*85 = 88%.
[0052] Cause 甲 <n 乙 Therefore, the permeability of Brand B’s sealing material is better than that of Brand A.
Claims
1. A method for evaluating the permeability of asphalt pavement sealing materials, characterized in that: The evaluation method comprises the following steps: (1) Two groups of cylindrical specimens were prepared according to the standard gradation of the asphalt pavement to be sealed; (2) Two groups of cylindrical specimens, one group is used as the test specimen, and the sealing material to be tested is evenly applied to the center of the top surface of the specimen. The evenly applied specimens are left to cure at room temperature for 24 hours; the other group is used as the standard specimen and is not treated in any way; (3) According to the smeared part of the test sample, the two groups of test samples are cored and cut: the core sample of each test sample is cut to remove the 10 mm thick part of the surface, and then two layers of thin sheets with a thickness of 15 mm are cut from top to bottom. The average value of the porosity of the two layers of thin sheets of each group of samples is tested respectively, and the change in the porosity of the two layers of thin sheets of the test sample relative to the standard sample is calculated to evaluate the permeability of the sealing material: the greater the decrease in the porosity of the two layers of thin sheets of the test sample, the better the permeability of the sealing material to be tested; The calculation method of the porosity change of the two-layer thin sheet of the test sample relative to the standard sample in step (3) is as follows: the porosity of the sampling thin sheets of each core sample is tested respectively, and the average value thereof is calculated. The average porosity of the first layer of the sampling thin sheet of the standard sample is recorded as V1V b The average porosity of the second layer of sample slices is recorded as V2V b The average porosity of the first layer of the sample is recorded as V1V a The average gap ratio of the second layer of sample slices is recorded as V2V a , V1V a 、V2V a 、V1V b 、V2V b The unit is %, and the permeability value is calculated by measuring the change in the void ratio of the two layers of sampling slices; The calculation formula of the permeability value n is as follows: K1×(10×(V1V b -V1V a )+60)+K2×(10×(V2V b -V2V a )+60), Wherein, K1 and K2 represent the weights of the change of the void ratio of the first layer and the change of the void ratio of the second layer, respectively.
2. The evaluation method according to claim 1, characterized in that: The K1 is 0.6, and the K2 is 0.
4.
3. The evaluation method according to claim 2, characterized in that: In the step (1), the cylindrical test piece is formed by a rotary compaction method, the void ratio is 4%, the diameter of the cylindrical test piece is 150 mm, and the height is 100-120 mm; in the step (2), the sealing material to be tested is applied to a circular portion with a diameter of 100 mm and a center at the top surface center of the test sample; in the step (3), a coring machine with a diameter of 100 mm is used to coring the applied portion of the test sample and the corresponding portion of the standard sample.