Electrode additive and preparation method thereof, positive electrode sheet

By using porous structure titanium aluminum phosphate core and carbon material filled and coated electrode additives in the positive electrode material of lithium-ion batteries, the solid phase dual transmission channel inside the electrode is constructed, and the problem of low electronic conductivity of the positive electrode material is solved. Improves the battery's rate performance and temperature adaptability and enhances battery safety.

CN114649528BActive Publication Date: 2024-11-01SHENZHEN DYNANONIC CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110339657.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-03-30
Publication Date
2024-11-01
Estimated Expiration
2041-03-30

AI Technical Summary

Technical Problem

The electronic conductivity of the positive electrode material of lithium-ion batteries is low, which leads to polarization of the electrode coating during the large-scale charging and discharging process, affecting the cycling and rate performance of the battery. Especially in low-temperature environments, the electrolyte fluidity is weakened, hindering the electrode coating. Internal ion transport efficiency.

Method used

Using an electrode additive, a titanium aluminum phosphate precursor is formed by mixing titanium source, aluminum source, phosphate, lithium source, acid complexing agent and alcohol solvent, and sintering is carried out in an inert atmosphere and an oxygen mixture atmosphere. A porous titanium aluminum lithium phosphate core and carbon material filling and cladding layer are generated to form an ion/electron dual fast conductor additive, and a solid phase dual transmission channel inside the electrode is constructed.

Benefits of technology

It significantly improves the ion and electron transfer rate of the electrode, enhances the rate performance and fast charging capability of the battery, improves the electrochemical performance, improves temperature adaptability, reduces the use of organic electrolyte, enhances battery safety, and suppresses Capacity attenuation in high/low temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114649528B_ABST
    Figure CN114649528B_ABST
Patent Text Reader

Abstract

The present application belongs to the field of battery technology, and in particular, relates to an electrode additive and a preparation method thereof, as well as a positive electrode sheet. The preparation method of the electrode additive comprises the steps of: mixing a titanium source, an aluminum source, a phosphate, a lithium source, an acidic chelating agent, an alkali solution and an alcohol solvent to form a sol, and then drying to obtain a lithium titanium aluminum phosphate precursor; performing a first sintering treatment on the lithium titanium aluminum phosphate precursor under an inert atmosphere, and then performing a second sintering treatment under a mixed atmosphere containing oxygen to obtain an electrode additive; the electrode additive comprises a porous lithium titanium aluminum phosphate core, a carbon material filled in the pores of the lithium titanium aluminum phosphate core, and a carbon shell layer coated on the outer surface of the lithium titanium aluminum phosphate core. The preparation method of the electrode additive of the present application generates a carbon material filling and coating layer in situ while generating lithium titanium aluminum phosphate, and has a simple process and high efficiency, and is suitable for industrial large-scale production and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of battery technology, and in particular relates to an electrode additive and a preparation method thereof, and a positive electrode sheet. Background Art

[0002] As a green and environmentally friendly new energy, lithium-ion batteries have the advantages of good reliability, high safety, small size and light weight. They have been widely used in digital products, electric vehicles, military products and other fields. With the demand and attention of various industries for new energy applications, the service life, safety and low cost of lithium-ion batteries are becoming increasingly higher. At present, lithium-ion batteries are also developing in the direction of long life, high safety, high rate and low cost. At present, due to the low ion conductivity of the positive electrode material of commercial lithium-ion batteries, during the high-rate charge and discharge process, it is very easy to have large polarization on the upper and lower sides of the electrode coating, and the electrode material cannot be fully utilized, resulting in the theoretical capacity of the positive electrode material not being brought into play in the actual application process, and its electrochemical performance is also poor. At the same time, it is difficult for the electrolyte to penetrate into the electrode coating to improve ion transmission; especially in low temperature environments, the electrolyte fluidity is weakened and the conductivity is sharply reduced, which further hinders the ion transmission efficiency inside the electrode coating.

[0003] Lithium aluminum titanium phosphate (LATP) has good ionic conductivity, low electronic conductivity, good chemical compatibility and stable electrochemical properties, and is currently widely used in solid electrolytes. However, fast ion conductor additives used in lithium-ion battery positive electrodes still have the problem of low electronic conductivity. Summary of the invention

[0004] The purpose of the present application is to provide an electrode additive and a preparation method thereof, as well as a positive electrode sheet, which aims to solve the problem that the positive electrode conductivity of existing lithium-ion batteries is low, affecting the battery cycle performance and rate performance to a certain extent.

[0005] In order to achieve the above application purpose, the technical solution adopted in this application is as follows:

[0006] In a first aspect, the present application provides a method for preparing an electrode additive, comprising the following steps:

[0007] A titanium source, an aluminum source, a phosphate radical, a lithium source, an acidic complexing agent, an alkali solution and an alcohol solvent are mixed to form a sol, and then dried to obtain a lithium aluminum titanium phosphate precursor;

[0008] After the lithium titanium aluminum phosphate precursor is subjected to a first sintering treatment under an inert atmosphere, it is subjected to a second sintering treatment under a mixed atmosphere containing oxygen to obtain an electrode additive; the electrode additive includes a porous lithium titanium aluminum phosphate core, a carbon material filling the pores of the lithium titanium aluminum phosphate core, and a carbon shell layer coating the outer surface of the lithium titanium aluminum phosphate core.

[0009] In a second aspect, the present application provides an electrode additive, which includes a porous lithium aluminum titanium phosphate core, a carbon material filling the pores of the lithium aluminum titanium phosphate core, and a carbon shell layer coating the outer surface of the lithium aluminum titanium phosphate core.

[0010] In a third aspect, the present application provides a positive electrode sheet, wherein the positive electrode sheet contains the above-mentioned electrode additive in an amount of 0.1% to 20% by mass.

[0011] The preparation method of the electrode additive provided in the first aspect of the present application generates a carbon material filling and coating layer in situ while generating lithium titanium aluminum phosphate. The process is simple, the efficiency is high, and it is suitable for industrial large-scale production and application. The prepared electrode additive, the lithium titanium aluminum phosphate core, has a high ionic conductivity, and the porous structure can increase the contact specific surface area, increase the active sites, and shorten the transmission path; the carbon material filled in the core and the carbon coating shell have excellent electron transmission efficiency. By filling and coating the core, the electronic conductivity is significantly improved while ensuring the high ionic conductivity of the additive, making it an ion / electron dual fast conductor additive. After being applied to the electrode, an ion / electron solid phase dual transmission channel can be constructed inside the electrode coating, reducing impedance, increasing the ion / electron transmission rate, thereby improving the rate performance and fast charging capability. At the same time, the amount of organic electrolyte injection is reduced, thereby enhancing battery safety, improving the electrochemical properties of the positive electrode of the lithium-ion battery, and improving its high-rate cycle performance. In addition, the electrode additive of the present application has an ion / electron solid phase transmission channel. The solid phase transmission channel constructed in the electrode layer is almost unaffected by temperature changes, which can ensure that the ion / electron transmission in the electrode layer is not affected by temperature, thereby improving the temperature adaptability of the battery and inhibiting capacity decay in high / low temperature environments.

[0012] A second aspect of an embodiment of the present application provides an electrode additive, which includes a porous lithium aluminum titanium phosphate core, a carbon material filling the pores of the lithium aluminum titanium phosphate core, and a carbon shell layer coating the outer surface of the lithium aluminum titanium phosphate core.

[0013] The positive electrode sheet provided in the third aspect of the present application contains 0.1% to 20% of the above-mentioned electrode additive in a mass percentage. The electrode additive can construct an ion / electron solid-phase dual transmission channel inside the positive electrode layer, reduce impedance, and increase the ion / electron transmission rate, thereby improving the rate performance and fast charging capability. At the same time, the amount of organic electrolyte injection is reduced, thereby enhancing battery safety, improving the electrochemical properties of the positive electrode sheet of the lithium-ion battery, and improving its high-rate cycle performance. In addition, the solid-phase transmission channel constructed in the positive electrode layer is almost unaffected by temperature changes, which can ensure that the ion / electron transmission in the positive electrode layer is not affected by temperature, thereby improving the temperature adaptability of the battery and suppressing capacity decay in high / low temperature environments. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0015] Figure 1 It is a 1C cycle performance test diagram of the positive electrode sheets of Examples 3 to 6 of the present application and Comparative Example 1;

[0016] Figure 2 It is a rate performance test diagram of the positive electrode sheets of Examples 3 to 6 of the present application and Comparative Example 1;

[0017] Figure 3 This is the XRD test diagram of the electrode additive in Example 1 of the present application;

[0018] Figures 4-5 This is the SEM morphology of the electrode additive in Example 1 of the present application. DETAILED DESCRIPTION

[0019] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0020] In the present invention, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects before and after are in an "or" relationship.

[0021] In the present invention, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b or c", or "at least one of a, b and c", can all represent: a, b, c, ab (i.e. a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0022] It should be understood that in various embodiments of the present invention, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present invention.

[0023] The terms used in the embodiments of the present invention are only for the purpose of describing specific embodiments, and are not intended to limit the present invention. The singular forms "a", "an" and "the" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0024] The weight of the relevant components mentioned in the description of the embodiments of the present invention may not only refer to the specific content of each component, but also indicate the weight ratio between the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the description of the embodiments of the present invention, it is within the scope disclosed in the description of the embodiments of the present invention. Specifically, the mass in the description of the embodiments of the present invention may be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.

[0025] A first aspect of an embodiment of the present application provides a method for preparing an electrode additive, comprising the following steps:

[0026] S10. After the titanium source, aluminum source, phosphate, lithium source, acidic complexing agent, alkali solution and alcohol solvent are mixed to form a sol, the sol is dried to obtain a lithium aluminum titanium phosphate precursor;

[0027] S20. After the lithium titanium aluminum phosphate precursor is subjected to a first sintering treatment under an inert atmosphere, it is subjected to a second sintering treatment under a mixed atmosphere containing oxygen to obtain an electrode additive; the electrode additive includes a porous lithium titanium aluminum phosphate core, a carbon material filling the pores of the lithium titanium aluminum phosphate core, and a carbon shell layer coating the outer surface of the lithium titanium aluminum phosphate core.

[0028] The preparation method of the electrode additive provided in the first aspect of the present application is to mix a titanium source, an aluminum source, a phosphate, a lithium source, an acidic complexing agent, an alkali solution and an alcohol solvent to prepare a lithium aluminum titanium phosphate precursor; the lithium aluminum titanium phosphate precursor is sintered in an inert atmosphere and an oxygen-containing atmosphere respectively, and the organic matter is carbonized during the inert atmosphere sintering process to form a light carbon material, a part of which is doped in the lithium aluminum titanium phosphate, and most of it is coated on the outer surface of the lithium aluminum titanium phosphate particles, and then part of the carbon material is converted into carbon dioxide by sintering in an oxygen-containing atmosphere to remove it, so that the thickness of the coated carbon material is moderate, the electron and ion transmission properties of the electrode additive are balanced, and a stable crystallized lithium aluminum titanium phosphate porous core is formed, and the carbon material is filled in the pores of the core, and a carbon material coating shell is formed on the outer surface of the core to obtain an electrode additive. The preparation method of the electrode additive in the embodiment of the present application generates a carbon material filling and coating layer in situ while generating lithium aluminum titanium phosphate, and the process is simple and efficient, and it is suitable for industrial large-scale production and application. The prepared electrode additive, lithium aluminum titanium phosphate core, has high ionic conductivity, and the ionic conductivity reaches 1×10 -4 S / cm, and the porous structure can increase the contact specific surface area, increase the active sites, and shorten the transmission path; the carbon material filled in the core and the carbon coating shell have excellent electron transmission efficiency. By filling and coating the core, the electronic conductivity is significantly improved while ensuring the high ionic conductivity of the additive, making it an ion / electron dual fast conductor additive. After being applied to the electrode, an ion / electron solid-phase dual transmission channel can be constructed inside the electrode coating to reduce impedance and increase the ion / electron transmission rate, thereby improving the rate performance and fast charging capability. At the same time, the amount of organic electrolyte injection is reduced, thereby enhancing battery safety, improving the electrochemical properties of the positive electrode of the lithium-ion battery, and improving its high-rate cycle performance. In addition, the present application has an electrode additive with an ion / electron solid-phase transmission channel, and the solid-phase transmission channel constructed in the electrode layer is almost unaffected by temperature changes, which can ensure that the ion / electron transmission in the electrode layer is not affected by temperature, thereby improving the temperature adaptability of the battery and inhibiting capacity decay in high / low temperature environments.

[0029] In some embodiments, in the above step S10, the step of preparing a lithium aluminum titanium phosphate precursor further includes mixing at least one dopant selected from a silicon source, a germanium source, a tin source, a scandium source, a gallium source, a yttrium source, and a lanthanum source with an acidic complexing agent such as a titanium source, an aluminum source, a phosphate, a lithium source, a citric acid, an alkali solution such as ammonia or lithium hydroxide, and an alcohol solvent to form a sol, and then drying to obtain a lithium aluminum titanium phosphate precursor. The embodiment of the present application further improves the crystal structure and defects of the material on the basis of Al doping by adding at least one dopant selected from a silicon source, a germanium source, a tin source, a scandium source, a gallium source, a yttrium source, and a lanthanum source, further increases the ion transmission channel and the electronic structure, and further improves the ion / electronic conductivity on the basis of Al / Ti element optimization, thereby improving the performance of the dual conductor material. In some embodiments, dopants such as silicon source, germanium source, tin source, scandium source, gallium source, yttrium source, and lanthanum source use salts that are easily soluble in an alcohol solvent system.

[0030] In some embodiments, the acidic complexing agent is selected from at least one of citric acid, malic acid, malonic acid, succinic acid, succinic acid, glycolic acid, aminoacetic acid, lactic acid, tartaric acid, and ethylenediaminetetraacetic acid. These acidic complexing agents can ionize and chelate with metal cations in the mixed solution, so that the metal cations can be evenly dispersed and compounded according to the stoichiometric ratio to form a precursor. In some preferred embodiments, the acidic complexing agent is selected from citric acid.

[0031] In some embodiments, the alkali solution is selected from at least one of ammonia water, lithium hydroxide, sodium hydroxide, and potassium hydroxide, and these alkali solutions have a good regulating effect on the pH value of the reaction system and do not introduce impurities. In some preferred embodiments, the alkali solution is selected from ammonia water or lithium hydroxide.

[0032] In some embodiments, in the above step S10, the drying step includes: making the mixed sol viscous under negative pressure at a temperature of 50 to 90° C., and then drying it at a temperature of 90 to 200° C. to obtain a dry lithium aluminum titanium phosphate precursor.

[0033] In some embodiments, in the above step S10, the titanium source is selected from: tetrabutyl titanate and / or titanium tetrachloride. In some embodiments, the aluminum source is selected from: at least one of aluminum nitrate, aluminum phosphate, aluminum chloride, and aluminum hydroxide. In some embodiments, the phosphate radical is selected from: at least one of phosphoric acid, ammonium hydrogen phosphate, and diammonium aluminum phosphate. In some embodiments, the lithium source is selected from: at least one of lithium carbonate, lithium hydroxide, lithium phosphate, lithium nitrate, and lithium aluminum sulfate. In some embodiments, the alcohol solvent is selected from: at least one of methanol, ethanol, ethylene glycol, propanol, and glycerol. These raw material components used in the embodiments of the present application have good solubility in alcohol solvents.

[0034] In some embodiments, in the sol, the addition ratio of the titanium source, aluminum source, phosphate, and lithium source is based on the stoichiometric ratio of lithium titanium aluminum phosphate, that is, the raw material components are added according to the ratio of each element in the lithium titanium aluminum phosphate crystal to be prepared.

[0035] In some embodiments, in the sol, the molar ratio of the acidic complexing agent to the metal cations in the sol is (0.5-8): 1. In step S10 of the embodiment of the present application, in the liquid phase, the acidic complexing agent is first ionized to chelate with the metal cations so that the metal cations can be evenly dispersed, compounded according to the stoichiometric ratio to form a precursor, and then esterified and cross-linked with alcohols to prevent ester hydrolysis, so sufficient acidic complexing agent will promote the reaction, but too much acidic complexing agent will cause the pH to be too acidic and cause side reactions. Too low and too high a molar ratio will affect the purity of lithium aluminum titanium phosphate, so the molar ratio of the acidic complexing agent to the metal cations in the present application is (0.5-8): 1, preferably (1-4): 1.

[0036] In some embodiments, in the sol, the molar ratio of the acidic complexing agent to the alcohol solvent is (0.5-2):1. The acidic complexing agent and alcohol in the embodiment of the present application are both organic reagents, which will be carbonized during the sintering process, so the molar ratio has little effect on the lithium aluminum titanium phosphate product. However, during the aging and evaporation process, due to the influence of temperature, the acidic complexing agent and the alcohol will undergo esterification, forming cross-links, and limiting the metal cations so that they can maintain the uniformity of concentration and be compounded according to the stoichiometric ratio. The molar ratio of the acidic complexing agent to the alcohol solvent is (0.5-2):1, which not only provides a suitable solvent environment for the reaction system, but also ensures the esterification reaction between the acidic complexing agent and the alcohol. In some specific embodiments, the molar ratio of the acidic complexing agent to the alcohol solvent is preferably 1:1. This stoichiometric ratio will make the acid and alcohol esterification more thorough and minimize the remaining monomers.

[0037] In some embodiments, the pH value of the sol is 3 to 7. In the embodiment of the present application, the pH is used to control the liquid phase reaction environment. Different metal ions start to react at different pH values. The pH is adjusted to make the liquid phase environment satisfy the range of all reactants as much as possible. In the process of the reaction of the raw material components of the present application to generate the lithium aluminum titanium phosphate precursor, if the acidity is too strong and the pH is lower than 3, AlPO is easily generated. 4 In some preferred embodiments, the pH value of the sol is 5-7.

[0038] In some embodiments, in the above step S20, the conditions for the first sintering treatment include: sintering for 1 to 15 hours in an inert atmosphere at a temperature of 600 to 1000°C, so that the lithium source, aluminum source, titanium source and phosphate react to form a stable lithium aluminum titanium phosphate crystalline phase; at the same time, the acidic chelating agent and organic phases such as alcohols are carbonized to form an amorphous carbon template, which is coated on the surface of the lithium aluminum titanium phosphate particles and embedded in the gaps between the lithium aluminum titanium phosphate particles, providing a carbon template for forming a porous lithium aluminum titanium phosphate core.

[0039] In some embodiments, the conditions of the second sintering treatment include: sintering for 1 to 15 hours at a temperature of 600 to 1000°C and a mixed atmosphere with an oxygen content of 1% to 20%. Since the carbon material content in the composite material of the carbon material and lithium titanium aluminum phosphate obtained after the first sintering is often too high, an excessively thick carbon material coating layer will affect the ionic conductivity of the lithium titanium aluminum phosphate, and the lithium titanium aluminum phosphate crystal form is not stable enough. Therefore, the second sintering of the embodiment of the present application is carried out in a mixed atmosphere with an oxygen content of 1% to 20%. On the one hand, the second sintering treatment makes the lithium titanium aluminum phosphate crystal form more stable. On the other hand, sintering in an oxygen-containing mixed atmosphere can convert part of the carbon material in the composite material into carbon dioxide for removal, thereby forming a carbon coating shell layer of appropriate thickness on the surface of the lithium titanium aluminum phosphate, while having both the ionic and electronic conductivity of the additive. If the oxygen content in the mixed atmosphere is too high, or the sintering temperature is too high, or the sintering time is too long, it may cause the carbon material in the composite material to be oxidized to carbon dioxide and removed; if the content is too low, or the sintering temperature is too low, or the sintering time is too short, it will lead to insufficient oxidation of the carbon material, so that the carbon material content in the additive is too high, limiting the ionic conductivity of lithium aluminum titanium phosphate. In some specific embodiments, the conditions for the second sintering treatment include: sintering treatment for 1h, 3h, 5h, 8h, 10h, 12h, 14h, 15h, etc. at a temperature of 600°C, 700°C, 800°C, 900°C, 1000°C, etc., and an oxygen content of 1% to 5%, 5% to 10%, 10% to 15%, 15% to 20%, etc.

[0040] In some embodiments, the lithium aluminum titanium phosphate core has the general chemical formula Li 1+x+y Al x M y N z Ti 2-x-y-z (PO 4 ) 3; Wherein, N is selected from at least one of Si, Ge, and Sn, M is selected from at least one of Sc, Ga, Y, and La, 0≤y≤0.5, 0≤z≤0.5, 0≤x+y≤0.5, preferably, 0.2≤x+y≤0.4. The lithium aluminum titanium phosphate core of the embodiment of the present application, on the one hand, optimizes the ratio of Al and Ti elements, adjusts the crystal structure and doping defects of the material, thereby expanding the ion transmission channel, improving the electronic structure, and further improving the ion / electronic conductivity. On the other hand, multi-metal elements are synergistically doped at the M and N positions, and the material crystal structure and defects are further improved on the basis of Al doping, and the ion transmission channel and electronic structure are further increased. On the basis of Al / Ti element optimization, the ion / electronic conductivity is further improved, and the performance of the dual-conductor material is improved.

[0041] In some embodiments, the particle size of the lithium aluminum titanium phosphate core is 50nm to 20μm. The lithium aluminum titanium phosphate core particles of the present application embodiment are micro-nano particle sizes, which shorten the solid-phase diffusion path of ions. When the additive is applied to the positive electrode material, the gaps between the particles of the filled positive electrode material are made smaller, and as many solid-phase conductor channels as possible are constructed. In some specific embodiments, the particle size of the lithium aluminum titanium phosphate core includes distributions in different intervals such as 10-20μm, 50nm-10μm, 50nm-5μm, 50-200nm, 200-800nm, and 200nm-2μm. There will always be gaps when multiple particles are in contact. Through the coordinated distribution of multi-level particle sizes, multi-level gaps of different scales can be effectively filled, and as many solid-phase conductor channels as possible can be constructed to reduce channel breakpoints.

[0042] In some embodiments, the pore size distribution of the lithium aluminum titanium phosphate core is 5 to 200 nm; the porous structure of the lithium aluminum titanium phosphate core can increase the specific surface contact area, increase the active sites, and shorten the transmission path. In some specific embodiments, the pore size distribution of the lithium aluminum titanium phosphate core can be 5 to 10 nm, 10 to 50 nm, 50 to 80 nm, 80 to 100 nm, 100 to 150 nm, 150 to 200 nm, etc.

[0043] In some embodiments, the pore size distribution of the carbon shell layer is 0.5-2 nm; the porous carbon shell layer provides a channel for the transmission of lithium aluminum titanium phosphate ions in the core, which is more conducive to ensuring the ion conductivity of the lithium aluminum titanium phosphate core. In some specific embodiments, the pore size distribution of the carbon shell layer can be 0.5-1 nm, 1-1.5 nm or 1.5-2 nm, etc.

[0044] In some embodiments, the thickness of the carbon shell layer is 1 to 500 nm. In the electrode additive of the embodiment of the present application, the thicker the thickness of the carbon shell layer, the better the encapsulation effect, the higher the electronic conductivity of the additive, but at the same time, the greater the obstruction to the in and out channels of ion transmission, which will reduce the ionic conductivity of the additive to a certain extent, so it is necessary to optimize and balance the two. When the thickness of the carbon shell layer is 1 to 500 nm, it can effectively improve the electronic conductivity of the additive and have little effect on the ionic conductivity of the additive.

[0045] In some embodiments, the mass percentage of carbon material in the electrode additive is 1% to 30%. This content of carbon material not only ensures the filling and coating effect of carbon material on lithium aluminum titanium phosphate to obtain an ion / electron dual-fast conductor additive, but also avoids excessive carbon material content hindering the lithium aluminum titanium phosphate ion transmission channel, and takes into account the electron and ion transmission efficiency of the additive.

[0046] A second aspect of an embodiment of the present application provides an electrode additive, which includes a porous lithium aluminum titanium phosphate core, a carbon material filling the pores of the lithium aluminum titanium phosphate core, and a carbon shell layer coating the outer surface of the lithium aluminum titanium phosphate core.

[0047] The electrode additive provided in the second aspect of the present application constructs an ion / electron solid-phase dual transport channel through the synergistic effect of a porous lithium aluminum titanium phosphate core, a carbon material filled in the core pores, and a carbon coating shell, reduces electrode impedance, and increases the electrode ion / electron transmission rate, thereby improving the battery rate performance and fast charging capability, and enhancing battery safety.

[0048] In some embodiments, the particle size of the lithium aluminum titanium phosphate core is 50 nm to 20 μm.

[0049] In some embodiments, the pore size distribution of the lithium aluminum titanium phosphate core is 5 to 200 nm.

[0050] In some embodiments, the pore size distribution of the carbon shell layer is 0.5-2 nm.

[0051] In some embodiments, the thickness of the carbon shell layer is 1 to 500 nm.

[0052] In some embodiments, the mass percentage of the carbon material in the electrode additive is 1% to 30%.

[0053] The electronic additives in the embodiments of the present application can be prepared by the above method. The beneficial effects of the above embodiments have been discussed in the previous text and will not be repeated here.

[0054] A third aspect of an embodiment of the present application provides a positive electrode sheet, which contains 0.1% to 20% by mass of the electrode additive prepared by the above method.

[0055] The positive electrode sheet provided in the third aspect of the present application contains 0.1% to 20% of the above-mentioned electrode additive in a mass percentage. The electrode additive can construct an ion / electron solid-phase dual transmission channel inside the positive electrode layer, reduce impedance, and increase the ion / electron transmission rate, thereby improving the rate performance and fast charging capability. At the same time, the amount of organic electrolyte injection is reduced, thereby enhancing battery safety, improving the electrochemical properties of the positive electrode sheet of the lithium-ion battery, and improving its high-rate cycle performance. In addition, the solid-phase transmission channel constructed in the positive electrode layer is almost unaffected by temperature changes, which can ensure that the ion / electron transmission in the positive electrode layer is not affected by temperature, thereby improving the temperature adaptability of the battery and suppressing capacity decay in high / low temperature environments.

[0056] The greater the amount of additive added to the positive electrode sheet of the embodiment of the present application, the better the cycle life, rate performance and low temperature performance of the battery will be. However, an increase in the amount added will also compress the proportion of the positive electrode active material, so excessive addition will lead to a decrease in the nominal capacity of the battery and a decrease in energy density.

[0057] In some embodiments, the electrode additives have a good matching relationship with different types of positive electrode active materials. The positive electrode active material in the positive electrode sheet can be lithium iron phosphate LFP, lithium cobalt oxide LCO, nickel cobalt manganese oxide ternary NCM and nickel cobalt aluminum ternary NCA and other positive electrode materials, which have good universality and a wide range of applications.

[0058] In order to enable the above implementation details and operations of the present application to be clearly understood by those skilled in the art, as well as to demonstrate the significant improvement in the performance of the electrode additives and their preparation, and the positive electrode sheets of the embodiments of the present application, the above technical solutions are illustrated by means of multiple embodiments below.

[0059] Example 1

[0060] An electrode additive, the preparation of which comprises the steps of:

[0061] ①According to Li 1.3 Al 0.3 Ti 1.7 (PO 4 ) 3 Weigh aluminum nitrate, lithium nitrate and ammonium dihydrogen phosphate in a stoichiometric ratio and weigh the total metal cations (Li + 、Al 3+ 、Ti 4+ ) citric acid in a molar ratio of 2:1 is completely dissolved in water. Tetrabutyl titanate in a stoichiometric ratio is added to the solution and stirred for 3 hours until it is completely uniform. Ammonia water is added to the solution to adjust the pH to 5, and then ethylene glycol in a molar ratio of 1:1 to citric acid is added and stirred to mix evenly. Rotary evaporation is performed at 80°C for 10 hours to form a gel, and then the solvent is evaporated in a drying oven at 100°C to form a dry gel.

[0062] ② After the dry gel is crushed into powder, it is sintered in a tubular furnace, using argon atmosphere protection, flow rate 200mL / min, heating to 550℃ at 5℃ / min and holding at this temperature for 1h, then continue to heat to 850℃ at 5℃ / min and hold at this temperature for 5h. Then the atmosphere is changed from argon to argon mixed atmosphere with 5% oxygen content, and the temperature is kept at 850℃ for 1h. After the sintering is completed, it naturally cools to room temperature, and the product is taken out to obtain Li 1.3 Al 0.3 Ti 1.7 (PO 4 ) 3 The ionic conductivity of the material was measured to be 1.03×10 -3 S / cm.

[0063] Example 2

[0064] An electrode additive, the preparation of which comprises the steps of:

[0065] ①According to Li 1.4 Al 0.4 Ti 1.6 (PO 4 ) 3 Weigh aluminum nitrate, lithium nitrate and ammonium dihydrogen phosphate in a stoichiometric ratio and weigh the total metal cations (Li + 、Al 3+ 、Ti 4+ ) citric acid in a molar ratio of 2:1 is completely dissolved in water. Tetrabutyl titanate in a stoichiometric ratio is added to the solution and stirred for 3 hours until it is completely uniform. Ammonia water is added to the solution to adjust the pH to 5, and then ethylene glycol in a molar ratio of 1:1 to citric acid is added and stirred to mix evenly. Rotary evaporation is performed at 80°C for 10 hours to form a gel, and then the solvent is evaporated in a drying oven at 100°C to form a dry gel.

[0066] ② After the dry gel is crushed into powder, it is sintered in a tubular furnace, using argon atmosphere protection, with a flow rate of 200 mL / min, and the temperature is raised to 550°C at 5°C / min and kept constant for 1 hour, and then continued to rise to 850°C at 5°C / min and kept constant for 5 hours. Then the atmosphere is changed from argon to an argon mixed atmosphere with an oxygen content of 2%, and the temperature is continued to be kept constant at 850°C for 1 hour. After the sintering is completed, it naturally drops to room temperature, and the product is taken out to obtain a stoichiometric ratio of Li 1.4 Al 0.4 Ti 1.6 (PO 4 ) 3 The ionic conductivity of the material was measured to be 6.96×10 -4 S / cm.

[0067] Example 3

[0068] An electrode additive, the preparation of which comprises the steps of:

[0069] ①According to Li 1.5 Al 0.5 Ti 1.5 (PO 4 ) 3 Weigh aluminum nitrate, lithium nitrate and ammonium dihydrogen phosphate in a stoichiometric ratio and weigh the total metal cations (Li + 、Al 3+ 、Ti 4+ ) citric acid in a molar ratio of 2:1 is completely dissolved in water. Tetrabutyl titanate in a stoichiometric ratio is added to the solution and stirred for 3 hours until it is completely uniform. Ammonia water is added to the solution to adjust the pH to 5, and then ethylene glycol in a molar ratio of 1:1 to citric acid is added and stirred to mix evenly. Rotary evaporation is performed at 80°C for 10 hours to form a gel, and then the solvent is evaporated in a drying oven at 100°C to form a dry gel.

[0070] ② After the dry gel is crushed into powder, it is sintered in a tubular furnace, using argon atmosphere protection, with a flow rate of 200 mL / min, and the temperature is raised to 550°C at 5°C / min and kept constant for 1 hour, and then continued to rise to 850°C at 5°C / min and kept constant for 5 hours. Then the atmosphere is changed from argon to an argon mixed atmosphere with an oxygen content of 10%, and the temperature is continued to be kept constant at 850°C for 1 hour. After the sintering is completed, it naturally drops to room temperature, and the product is taken out to obtain a stoichiometric ratio of Li 1.5 Al 0.5 Ti 1.5 (PO 4 ) 3 The ionic conductivity of the material was measured to be 4.53×10 -4 S / cm.

[0071] Example 4

[0072] A positive electrode sheet is prepared with the LATP additive of Example 1, wherein the slurry material composition is 93% of lithium cobalt oxide (LCO) positive electrode material, 2% of the LATP additive of Example 1, 3% of a binder polyvinylidene fluoride (PVDF), and 2% of a conductive additive conductive carbon black (SP); button half-cells are assembled to test the cycle performance at 1C rate and the rate performance at different rates.

[0073] Example 5

[0074] A positive electrode sheet is prepared with the LATP additive of Example 2, wherein the slurry material composition is 93% of lithium cobalt oxide (LCO) positive electrode material, 2% of the LATP additive of Example 2, 3% of a binder polyvinylidene fluoride (PVDF), and 2% of a conductive additive conductive carbon black (SP); button half-cells are assembled to test the cycle performance at 1C rate and the rate performance at different rates.

[0075] Example 6

[0076] A positive electrode sheet is prepared with the LATP additive of Example 3, wherein the slurry material composition is 93% of lithium cobalt oxide (LCO) positive electrode material, 2% of the LATP additive of Example 2, 3% of a binder polyvinylidene fluoride (PVDF), and 2% of a conductive additive conductive carbon black (SP); button half-cells are assembled to test the cycle performance at 1C rate and the rate performance at different rates.

[0077] Comparative Example 1

[0078] A positive electrode sheet is prepared without additives, wherein the slurry material composition is 95% of lithium cobalt oxide (LCO) positive electrode material, 3% of binder polyvinylidene fluoride (PVDF), and 2% of conductive additive conductive carbon black (SP); button half-cells are assembled to test the cycle performance at 1C rate and the rate performance at different rates.

[0079] Further, in order to verify the progress of the embodiments of the present application, the ionic conductivity, electronic conductivity and mass percentage of the carbon material of the electrode additives prepared in Examples 1 to 3 were tested, and the test results are shown in Table 1 below:

[0080] 1. The ionic conductivity of lithium aluminum titanium phosphate (LATP) electrode additive is measured by the following method: After the electrode additive fast ion conductor material is ball-milled and nano-sized, it is pressed into a disc with a certain diameter D and thickness L using a tablet press, and then placed in a tube furnace and sintered at 850°C for 2 hours; the two sides of the sintered electrode additive disc are subjected to gold spraying conductive treatment, and finally the two sides of the electrode additive disc are connected to the electrochemical workstation for AC impedance testing, and the test frequency range is 0.01Hz~100KHz. The impedance value of the electrode additive disc is obtained based on the equivalent circuit fitting of the impedance diagram. The calculation of ionic conductivity is based on the formula σ=L / RS, where σ is the ionic conductivity size, in units of S / cm; L is the thickness of the electrode additive disc, in units of cm; R is the impedance value of the LATP electrode additive disc measured by the electrochemical workstation, in units of Ω; S=π(D / 2) 2 , is the circular surface area of ​​the LATP electrode additive disc, in cm 2 .

[0081] 2. Analyze the mass percentage of carbon material in electrode additives by thermogravimetric analysis (TGA).

[0082] 3. Test method for the electronic conductivity of electrode additives: Use a tablet press to press the additive powder into dense discs, and use a four-probe tester to test the electronic conductivity of the discs.

[0083] Table 1

[0084] Ionic conductivity Electronic conductivity Carbon material content Example 1 <![CDATA[1.03×10 -3 S / cm]]> <![CDATA[5.72×10 3 S / cm]]> 11.2% Example 2 <![CDATA[6.96×10 -4 S / cm]]> <![CDATA[1.09×10 4 S / cm]]> 26.5% Example 3 <![CDATA[4.53×10 -4 S / cm]]> <![CDATA[3.49×10 3 S / cm]]> 3.4%

[0085] In addition, after the positive electrodes provided in Examples 4 to 6 and Comparative Example 1 were assembled into button-type half-cells, the cycle performance at 1C rate and the rate performance at different rates were tested. The test results are shown in the attached Figures 1-2 shown.

[0086] By the attached Figure 1 (Cycling performance at 1C rate) and Figure 2 (Rate performance at different rates) It can be seen from the test chart that, compared with the comparative example 1 without additives, the positive electrode sheets of Examples 4 to 6 of the present application with the LATP additives of Examples 1 to 3 have better cycle performance and rate performance.

[0087] Furthermore, the LATP additive prepared in Example 1 was subjected to X-ray diffraction analysis, and the XRD pattern is shown in the attached figure. Figure 3 As shown in Figure 1, the characteristic peaks of the LATP additive match those of the LTP material. In addition, due to the presence of metal element doping, the unit cell parameters change slightly, and the unit cell volume decreases accordingly.

[0088] Furthermore, the morphology of the LATP additive prepared in Example 1 was observed by scanning electron microscopy. The SEM image is shown in the attached figure. Figure 4 and 5 As shown, the additive is a porous core-shell structure particle.

[0089] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.

Claims

1. A method for preparing an electrode additive, characterized in that: The following steps are involved: At least one doping source selected from the group consisting of a silicon source, a germanium source, a tin source, a scandium source, a gallium source, a yttrium source, and a lanthanum source is mixed with a titanium source, an aluminum source, a phosphate, a lithium source, an acidic complexing agent, an alkali solution, and an alcohol solvent to form a sol, and then dried to obtain a lithium aluminum titanium phosphate precursor; the pH value of the sol is 3 to 7; After the lithium titanium aluminum phosphate precursor is subjected to a first sintering treatment in an inert atmosphere, a second sintering treatment is carried out for 1 to 15 hours in a mixed atmosphere containing oxygen at a temperature of 600 to 1000° C. and an oxygen content of 1% to 20%, to obtain an electrode additive; the electrode additive comprises a porous lithium titanium aluminum phosphate core, a carbon material filled in the pores of the lithium titanium aluminum phosphate core, and a carbon shell layer coated on the outer surface of the lithium titanium aluminum phosphate core; the carbon shell layer is a porous structure; the mass percentage of the carbon material filled and coated in the electrode additive is 1% to 30%; The general chemical formula of the lithium aluminum titanium phosphate core is Li 1+x+y Al x M y N z Ti 2-x-y-z (PO4)3; wherein N is selected from at least one of Si, Ge, and Sn, M is selected from at least one of Sc, Ga, Y, and La, 0≤y≤0.5, 0≤z≤0.5, and 0≤x+y≤0.5; the particle size of the lithium aluminum titanium phosphate core includes distributions in different intervals of 10-20μm, 50nm-10μm, 50nm-5μm, 50-200nm, 200-800nm, and 200nm-2μm, and the electrode additive has an ion / electron solid-phase dual transport channel, and is applied as an additive in an electrode coating to form a multi-level particle size coordinated distribution in the electrode coating.

2. The method for preparing the electrode additive according to claim 1, characterized in that: The conditions of the first sintering treatment include: sintering treatment for 1 to 15 hours in an inert atmosphere at a temperature of 600 to 1000°C.

3. The method for preparing the electrode additive according to claim 1 or 2, characterized in that: The drying step includes: making the mixed sol viscous under negative pressure at a temperature of 50 to 90° C., and then drying it at a temperature of 90 to 200° C. to obtain the dried lithium aluminum titanium phosphate precursor.

4. The method for preparing the electrode additive according to claim 3, characterized in that: The titanium source is selected from: tetrabutyl titanate and / or titanium tetrachloride; And / or, the aluminum source is selected from at least one of aluminum nitrate, aluminum phosphate, aluminum chloride, and aluminum hydroxide; And / or, the phosphate radical is selected from at least one of phosphoric acid, ammonium hydrogen phosphate, and aluminum diammonium phosphate; And / or, the lithium source is selected from at least one of lithium carbonate, lithium hydroxide, lithium phosphate, lithium nitrate, and lithium aluminum sulfate; And / or, the alcohol solvent is selected from at least one of methanol, ethanol, ethylene glycol, propanol and glycerol; And / or, the alkali solution is selected from at least one of: aqueous ammonia, lithium hydroxide, sodium hydroxide, and potassium hydroxide; And / or, the acidic complexing agent is selected from at least one of citric acid, malic acid, malonic acid, succinic acid, succinic acid, glycolic acid, aminoacetic acid, lactic acid, tartaric acid, and ethylenediaminetetraacetic acid.

5. The method for preparing the electrode additive according to claim 4, characterized in that: In the sol, the addition ratio of the titanium source, the aluminum source, the phosphate, the lithium source and the doping source is in accordance with the stoichiometric ratio in the general chemical formula of the lithium titanium aluminum phosphate core; and / or, in the sol, the molar ratio of the acidic complexing agent to the metal cation in the sol is (0.5-8):1; And / or, in the sol, the molar ratio of the acidic complexing agent to the alcohol solvent is (0.5-2):

1.

6. The method for preparing the electrode additive according to claim 5, characterized in that: The particle size of the lithium aluminum titanium phosphate core is 50nm to 20μm; and / or, the pore size distribution of the carbon shell layer is 0.5 to 2 nm; And / or, the thickness of the carbon shell layer is 1 to 500 nm; And / or, the alkali solution is selected from ammonia water or lithium hydroxide; And / or, the acidic complexing agent is selected from citric acid.

7. An electrode additive prepared by the method according to any one of claims 1 to 6, characterized in that: The electrode additive comprises a porous lithium titanium aluminum phosphate core, a carbon material filled in the pores of the lithium titanium aluminum phosphate core, and a carbon shell layer coated on the outer surface of the lithium titanium aluminum phosphate core.

8. The electrode additive according to claim 7, characterized in that The particle size of the lithium aluminum titanium phosphate core is 50nm to 20μm; and / or, the pore size distribution of the lithium aluminum titanium phosphate core is 5 to 200 nm; and / or, the pore size distribution of the carbon shell layer is 0.5 to 2 nm; And / or, the thickness of the carbon shell layer is 1 to 500 nm; And / or, the mass percentage of the carbon material in the electrode additive is 1% to 30%.

9. A positive electrode sheet, characterized in that: The positive electrode sheet contains 0.1% to 20% by mass of an electrode additive prepared by the method according to any one of claims 1 to 6 or an electrode additive according to any one of claims 7 to 8.