Method for extracting copper and cobalt from low-grade copper-cobalt sulfide concentrate

By performing boiling roasting and wet leaching treatment in low-grade copper sulfide cobalt concentrate, the problem of low sulfur dioxide concentration in roasted flue gas is solved, the extraction rate of copper and cobalt is improved, the process cost is reduced, and environmental protection is improved, so as to achieve Efficient metal recycling.

CN114657372BActive Publication Date: 2024-11-08CHINA ENFI ENG CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210199939.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-01
Publication Date
2024-11-08
Estimated Expiration
2042-03-01

AI Technical Summary

Technical Problem

When dealing with low-grade copper sulfide concentrate, the existing technology has problems such as high energy consumption, low metal recovery rate, high production cost and unenvironmental protection. In particular, the concentration of sulfur dioxide in the roasted flue gas is low and cannot self-heat and acid production, resulting in the entire The extraction process is costly and not environmentally friendly.

Method used

The ore slurry is made by low-grade copper sulfide cobalt concentrate and water grinding, and the boiling and roasting reaction is carried out in oxygen-rich air to control the slurry concentration and oxygen-rich air surplus coefficient within a specific range to realize the self-heating roasting process, followed by wet method Leach and flue gas dust collection treatment to produce metal copper and cobalt, and use sulfur-containing flue gas to produce acid.

Benefits of technology

It improves the extraction rate of copper and cobalt elements, reduces process costs, reduces flue gas volume and dust, improves environmental protection, and achieves efficient metal recycling and low-cost process flow.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114657372B_ABST
    Figure CN114657372B_ABST
Patent Text Reader

Abstract

The present invention provides a method for extracting copper and cobalt from low-grade copper-cobalt sulfide concentrate. The method for extracting copper and cobalt from low-grade copper-cobalt sulfide concentrate comprises: grinding the low-grade copper-cobalt sulfide concentrate with water to obtain slurry, the concentration of the slurry is 70-80wt%, the D50 of the solid particles is 50-100μm, the copper content in the low-grade copper-cobalt sulfide concentrate is ≤20wt%, and the cobalt content is ≤10wt%; in oxygen-enriched air, the slurry is subjected to a boiling roasting reaction to obtain copper-cobalt roasted sand and sulfur-containing flue gas, wherein the excess coefficient of oxygen-enriched air during the boiling roasting reaction is 1.5-2. Compared with the existing method, the use of the above process to treat the low-grade copper-cobalt sulfide concentrate is conducive to greatly improving the extraction rate of copper and cobalt elements, reducing process costs, and improving environmental protection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of pyrometallurgical copper smelting, and in particular to a method for extracting copper and cobalt elements from low-grade copper-cobalt sulfide concentrate. Background Art

[0002] The pyrometallurgical copper smelting process mainly processes copper sulfide minerals, and generally includes the steps of copper concentrate matte smelting, copper matte blowing, pyrometallurgical refining of blister copper and electrolytic refining of anode copper.

[0003] The enhanced metallurgical process is represented by flash smelting and bath smelting. It has the advantages of mature technology, stable operation, and complete supporting facilities. It is the mainstream process for processing copper sulfide minerals. Both flash smelting and bath smelting require that the sulfur grade in the copper concentrate must be high enough to fully utilize its reaction heat to complete self-heating smelting, reduce energy consumption, improve production efficiency, and reduce production costs. When cobalt-containing copper concentrate is processed by pyrometallurgical process, the recovery rate of cobalt element cannot be guaranteed because the cobalt element enters the smelting slag and is difficult to recover. Therefore, when the pyrometallurgical process is used to treat low-grade copper-cobalt sulfide concentrate, there are disadvantages such as high energy consumption, low metal recovery rate, and high production cost.

[0004] The hydrometallurgical copper smelting process mainly processes copper oxide minerals, generally including leaching, extraction and electrowinning. According to different raw materials, hydrometallurgical copper smelting is divided into a variety of leaching processes such as atmospheric pressure leaching, high pressure oxygen leaching, ammonia leaching and bacterial leaching. For low-grade copper-cobalt sulfide concentrate (the copper content in the concentrate is not higher than 20wt%, and the cobalt content is not higher than 10wt%), high pressure oxygen leaching, ammonia leaching, bacterial leaching and other processes can be used, but these processes are not yet mature, and there are problems such as high equipment investment, long production cycle and high production cost.

[0005] The pyrometallurgical-wet metallurgical combined process (i.e., a combination of roasting and leaching processes) is also commonly used to process complex copper concentrates, but for low-grade copper-cobalt sulfide concentrates (the copper content in the concentrate is not higher than 20wt%, and the cobalt content is not higher than 10wt%), there are many shortcomings. For example, the traditional air roasting has a complex dry feeding system, large dust and high mechanical losses; the concentrate has a low sulfur content and the roasting process cannot be self-heated; the roasting flue gas volume is large, the sulfur dioxide concentration is low, and the flue gas treatment is difficult; the roasted sand produced in the oxidative roasting process consumes a large amount of acid during leaching, etc.

[0006] In view of the above problems, it is necessary to provide a treatment method for low-grade copper-cobalt sulfide concentrate, which has the advantages of high metal recovery rate, low cost, and good environmental protection. Summary of the invention

[0007] The main purpose of the present invention is to provide a method for extracting copper and cobalt from low-grade copper-cobalt sulfide concentrate, so as to solve the problems that the existing method for extracting copper and cobalt from low-grade copper-cobalt sulfide ore cannot be self-heated and the sulfur dioxide concentration in the roasting flue gas is low and acid cannot be produced, which further leads to the problem that the entire extraction process is high in cost and is not environmentally friendly.

[0008] In order to achieve the above object, the present invention provides a method for extracting copper and cobalt from a low-grade copper-cobalt sulfide concentrate, wherein the copper content in the low-grade copper-cobalt sulfide concentrate is ≤20wt%, and the cobalt content is ≤10wt%. The method for extracting copper and cobalt from the low-grade copper-cobalt sulfide concentrate comprises: grinding the low-grade copper-cobalt sulfide concentrate with water to obtain slurry, wherein the concentration of the slurry is 70-80wt%, and the D50 of the solid particles is 50-100μm; and in oxygen-enriched air, subjecting the slurry to a fluidized bed roasting reaction to obtain copper-cobalt roasted sand and sulfur-containing flue gas, wherein the excess coefficient of the oxygen-enriched air during the fluidized bed roasting reaction is 1.5-2.

[0009] Furthermore, a dispersant is added during the grinding process; preferably, the pH of the slurry is 5-7.

[0010] Furthermore, the concentration of the slurry is 75-80wt%.

[0011] Furthermore, during the fluidized bed roasting reaction, the air flow rate is 0.3-0.7 m / s, and the boiling height is 1-1.8 m.

[0012] Furthermore, the temperature of the fluidized bed roasting reaction process is 750-900°C.

[0013] Furthermore, the method for extracting copper and cobalt from low-grade copper-cobalt sulfide concentrate also includes: wet leaching the copper-cobalt roasted sand to obtain metallic copper and metallic cobalt.

[0014] Furthermore, the method for extracting copper and cobalt from low-grade copper-cobalt sulfide concentrate also includes: collecting dust from sulfur-containing flue gas to obtain flue dust and flue gas containing sulfur dioxide; and using the flue gas containing sulfur dioxide as a raw material to produce acid to obtain sulfuric acid.

[0015] Furthermore, the low-grade copper-cobalt sulfide concentrate includes 12-20wt% Cu and 0.5-10wt% Co in terms of weight percentage of the low-grade copper-cobalt sulfide concentrate.

[0016] The technical solution of the present invention is applied to prepare low-grade copper-cobalt sulfide concentrate and water into slurry, and by limiting the slurry concentration and the excess coefficient of oxygen-enriched air within a specific range, the heat in the roasting process can be used as a heat source for the boiling roasting reaction, and it is in a thermal equilibrium state to achieve self-heating. This is conducive to greatly improving energy utilization and saving process costs; at the same time, the boiling roasting reaction process under the excess coefficient of the above-mentioned oxygen-enriched air can cause the low-grade copper-cobalt sulfide concentrate to be deeply oxidized, thereby improving the extraction rate of copper and cobalt elements in the low-grade copper-cobalt sulfide concentrate to a certain extent. In addition, there will be no dust in the above-mentioned entire process, the amount of flue gas is small, the sulfur content is high, and it is convenient to carry out centralized acid production treatment, so it has good environmental protection. In summary, the use of the above-mentioned process to treat low-grade copper-cobalt sulfide concentrate is conducive to improving the extraction rate of copper and cobalt elements to a certain extent, greatly reducing process costs, and improving environmental protection. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0018] Figure 1 A schematic process flow diagram of a method for extracting copper and cobalt from a low-grade copper-cobalt concentrate provided in Example 1 of the present invention is shown. DETAILED DESCRIPTION

[0019] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0020] As described in the background technology, the existing method of extracting copper and cobalt from low-grade copper-cobalt sulfide ores has the problems of high cost of metal element extraction and environmental pollution. In order to solve the above technical problems, the present application provides a method for extracting copper and cobalt from low-grade copper-cobalt sulfide concentrate, wherein the copper content in the low-grade copper-cobalt sulfide concentrate is ≤20wt%, and the cobalt content is ≤10wt%. The method comprises: grinding the low-grade copper-cobalt sulfide concentrate with water to obtain a pulp, wherein the concentration of the pulp is 70-80wt%, and the D50 of the solid particles is 50-100μm; in oxygen-enriched air, the pulp is subjected to a fluidized bed roasting reaction to obtain copper-cobalt roasted sand and sulfur-containing flue gas, wherein the excess coefficient of the oxygen-enriched air during the fluidized bed roasting reaction is 1.5-2.

[0021] As described in the background technology, there are problems in the extraction process of low-grade copper-cobalt sulfide concentrate, such as inability to self-heat and inability to produce acid due to low sulfur dioxide concentration in roasting flue gas, which leads to high cost and environmental problems in the entire extraction process. Based on many years of creative work, the inventors found that by preparing low-grade copper-cobalt sulfide concentrate and water into slurry, and by limiting the slurry concentration and the excess coefficient of oxygen-enriched air within a specific range, the heat in the roasting process can be used as a heat source for the boiling roasting reaction, and it can be in a thermal equilibrium state to achieve self-heating. This is conducive to greatly improving energy utilization and saving process costs; at the same time, the boiling roasting reaction process under the excess coefficient of the above-mentioned oxygen-enriched air can cause the low-grade copper-cobalt sulfide concentrate to be deeply oxidized, thereby improving the extraction rate of copper and cobalt elements in the low-grade copper-cobalt sulfide concentrate to a certain extent. In addition, there will be no dust in the above-mentioned entire process, the flue gas volume is small, the sulfur content is high, and it is convenient for centralized acid production, so it has good environmental protection. In summary, the use of the above process to treat low-grade copper-cobalt sulfide concentrate is beneficial to improving the extraction rate of copper and cobalt elements to a certain extent, and greatly reducing process costs and improving environmental protection.

[0022] The stability of the slurry and the dispersibility of the mineral raw materials will affect the effect of the subsequent boiling roasting reaction process. In order to further improve the stability of the slurry and the dispersibility of the mineral raw materials, preferably, a dispersant is added during the grinding process. More preferably, the pH of the slurry is 5 to 7. By adjusting the pH of the slurry, it is beneficial to further improve the stability of the slurry, and it has a high economic value with industrial promotion. Preferably, the above-mentioned dispersant includes but is not limited to one or more of the group consisting of sodium pyrophosphate, carboxymethyl cellulose, lime, and calcium chloride, and the amount of the dispersant accounts for 1 to 5wt% of the total weight of the slurry.

[0023] In a preferred embodiment, the concentration of the slurry is 75-80 wt %. The concentration of the slurry includes but is not limited to the above range, and limiting it within the above range is beneficial to further improve the processing efficiency of the fluidized bed roasting reaction process.

[0024] During the fluidized bed roasting reaction, the solid material is fully in contact with the gas, shortening the transfer and reaction distance inside the particles. At the same time, during the reaction process, the existence state of the low-grade copper-cobalt sulfide concentrate can be adjusted by the airflow. In a preferred embodiment, during the fluidized bed roasting reaction, the airflow rate is 0.3-0.7 m / s, and the boiling height is 1-1.8 m. During the liquid roasting process, the solid material is in a suspended state, and limiting the airflow rate and boiling height within the above range can make the solid material more evenly dispersed during the fluidized bed roasting reaction, reduce the temperature difference during the roasting process, and further deepen the roasting process, thereby further improving the extraction rate of copper and cobalt elements. For example, during the fluidized bed roasting reaction, the airflow rate is 0.3 m / s, 0.4 m / s, 0.5 m / s, 0.6 m / s, 0.7 m / s, and the boiling height is 1 m, 1.2 m, 1.5 m, 1.6 m, 1.8 m.

[0025] In a preferred embodiment, the temperature of the fluidized bed roasting reaction process is 750-900°C. Compared with other temperature ranges, limiting the temperature of the fluidized bed roasting reaction process to the above range can make the solid material react more fully, thereby further improving the extraction rate of copper and cobalt elements; at the same time, it can also further increase the concentration of sulfur dioxide in the flue gas. For example, the temperature of the fluidized bed roasting reaction process is 750°C, 800°C, 850°C, and 900°C.

[0026] In order to facilitate subsequent targeted utilization, in a preferred embodiment, the method for extracting copper and cobalt elements from low-grade copper-cobalt sulfide concentrate also includes: wet leaching the copper-cobalt roasted sand to obtain metallic copper and metallic cobalt; dust collection treatment of sulfur-containing flue gas to obtain smoke dust and flue gas containing sulfur dioxide; and mixing the flue gas containing sulfur dioxide with water to obtain sulfuric acid.

[0027] Since the above-mentioned extraction process can achieve deep oxidation of low-grade copper-cobalt sulfide concentrate, it is beneficial to improve the extraction rate of copper and cobalt elements. Due to the complex composition of low-grade copper-cobalt sulfide concentrate, it is difficult to oxidize it using the existing extraction process, and the extraction rate of copper and cobalt elements is not high. Compared with the existing process, the above-mentioned process provided in the present application can achieve deep oxidation, so the above-mentioned process is very suitable for extracting copper and cobalt elements from low-grade copper-cobalt sulfide concentrate. Preferably, the low-grade copper-cobalt sulfide concentrate includes 12-20% Cu and 0.5-10% Co, measured in weight percentage of the low-grade copper-cobalt sulfide concentrate. The weight percentage of copper element can be selected as 12%, 12.6%, 13%, 15%, 16.4%, 18.3%, 19%, and 20%, and the weight percentage of cobalt element can be selected as 0.5%, 0.8%, 1.2%, 2.1%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%.

[0028] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0029] Example 1

[0030] The main chemical compositions of low-grade copper-cobalt concentrate are shown in Table 1.

[0031] Table 1

[0032] element Cu Co Fe S Content (wt%) 16.4 1.2 12.5 15.0

[0033] Low-grade copper-cobalt concentrate and water are prepared into a slurry with a slurry concentration of 72wt% (D50 of solid particles in the slurry is 60μm), and the slurried slurry is added to the boiling roaster from the top of the furnace. Oxygen-enriched air with an oxygen-enriched concentration of 28vol% is blown into the boiling roaster, and the excess coefficient of oxygen-enriched air is controlled to be 1.5. The slurry in the boiling roaster reacts with the oxygen-enriched air in the furnace, wherein the air flow velocity is 0.45m / s, the boiling layer height is 1.2m, and the roasting temperature is 720℃ to obtain roasted sand and flue gas, and the sulfur dioxide concentration in the flue gas produced by the roaster is 2.8wt%.

[0034] The flue gas is sent to the flue gas acid system after dust collection and cooling, and the collected flue dust is sent to the wet leaching system. The roasted sand discharged from the roasting furnace is also sent to the wet leaching system, and the roasted sand and flue dust are mixed and then acid leached, with a leaching rate of Cu 97.31wt% and Co 95.65wt%.

[0035] Example 2

[0036] The main chemical compositions of low-grade copper-cobalt concentrate are shown in Table 2.

[0037] Table 2

[0038] element Cu Co Fe S Content (wt%) 12.6 0.8 10.9 13.5

[0039] Low-grade copper-cobalt concentrate and water are prepared into a slurry with a slurry concentration of 77wt% (D50 of solid particles in the slurry is 60μm), and the slurried slurry is added to the boiling roaster from the top of the furnace. Oxygen-enriched air with an oxygen-enriched concentration of 30vol% is blown into the boiling roaster, and the excess coefficient of oxygen-enriched air is controlled to be 1.55. The slurry in the boiling roaster reacts with the oxygen-enriched air in the furnace, wherein the air flow velocity is 0.6m / s, the boiling layer height is 1.5m, and the roasting temperature is 750℃, and roasted sand and flue gas are obtained. The sulfur dioxide concentration of the flue gas produced by the roaster is 3.1wt%.

[0040] The flue gas is sent to the flue gas acid system after dust collection and cooling, and the collected flue dust is sent to the wet leaching system. The roasted sand discharged from the roasting furnace is also sent to the wet leaching system, and the roasted sand and flue dust are mixed and then acid leached, with a leaching rate of Cu 96.72wt% and Co 94.26wt%.

[0041] Example 3

[0042] The main chemical components of low-grade copper-cobalt concentrate are shown in Table 3.

[0043] Table 3

[0044] element Cu Co Fe S Content (wt%) 18.3 2.1 16.6 16.8

[0045] Low-grade copper-cobalt concentrate and water are prepared into a slurry with a slurry concentration of 72wt% (D50 of solid particles in the slurry is 60μm), and the slurried slurry is added to the boiling roaster from the top of the furnace. Oxygen-enriched air with an oxygen-enriched concentration of 28vol% is blown into the boiling roaster, and the excess coefficient of oxygen-enriched air is controlled to be 1.6. The slurry in the boiling roaster reacts with the oxygen-enriched air in the furnace, wherein the air flow velocity is 0.5m / s, the boiling layer height is 1.5m, and the roasting temperature is 750℃, and roasted sand and flue gas are obtained. The sulfur dioxide concentration in the flue gas produced by the roaster is 3.2wt%.

[0046] The flue gas is sent to the flue gas acid system after dust collection and cooling, and the collected flue dust is sent to the wet leaching system. The roasted sand discharged from the roasting furnace is also sent to the wet leaching system, and the roasted sand and flue dust are mixed and then acid leached, with a leaching rate of Cu 97.93wt% and Co 94.83wt%.

[0047] Example 4

[0048] The difference from Example 2 is that a dispersant (sodium pyrophosphate, 2 wt% of the slurry) is added during the slurry preparation process. The leaching rate is 97.64 wt% for Cu and 96.55 wt% for Co, and the concentration of SO2 in the flue gas is 3.45 wt%.

[0049] Example 5

[0050] The difference from Example 4 is that the air flow velocity is 0.3 m / s, the boiling height is 1 m, the leaching rate is Cu 96.85 wt%, Co 95.12 wt%, and the concentration of SO2 in the flue gas is 3.0 wt%.

[0051] Example 6

[0052] The difference from Example 4 is that the air flow velocity is 0.7 m / s, the boiling height is 1.8 m, the leaching rate is Cu 97.06 wt%, Co 94.87 wt%, and the concentration of SO2 in the flue gas is 3.6 wt%.

[0053] Example 7

[0054] The difference from Example 4 is that the air flow velocity is 0.8 m / s, the boiling height is 2 m, the leaching rate is Cu 93.44 wt%, Co 92.15 wt%, and the concentration of SO2 in the flue gas is 2.8 wt%.

[0055] Example 8

[0056] The difference from Example 4 is that the roasting process is 750° C. The leaching rate is 98.02wt% for Cu and 96.23wt% for Co, and the concentration of SO2 in the flue gas is 3.7wt%.

[0057] Example 9

[0058] The difference from Example 4 is that the roasting process is at 900° C. The leaching rate is 97.79wt% for Cu and 95.01wt% for Co, and the concentration of SO2 in the flue gas is 3.9wt%.

[0059] Example 10

[0060] The difference from Example 4 is that the roasting process is 600° C. The leaching rate is 95.31wt% for Cu and 93.22wt% for Co, and the concentration of SO2 in the flue gas is 2.7wt%.

[0061] Embodiment 11

[0062] The difference from Example 4 is that the excess coefficient of oxygen-enriched air is 2.

[0063] The leaching rates were 96.98wt% for Cu and 95.35wt% for Co, and the content of SO2 in the flue gas was 4.0wt%.

[0064] Example 12

[0065] The difference from Example 2 is that the D50 of the solid particles in the slurry is 100 μm.

[0066] The leaching rates were 95.62wt% for Cu and 94.05wt% for Co, and the concentration of SO2 in the flue gas was 2.7wt%.

[0067] Comparative Example 1

[0068] The difference from Example 2 is that the D50 of the solid particles in the slurry is 150 μm.

[0069] The leaching rate is 91.89wt% for Cu and 90.75wt% for Co. The concentration of SO2 in the flue gas is 2.3wt%, and additional heat supplementation is required.

[0070] Comparative Example 2

[0071] The difference from Example 2 is that the D50 of the solid particles in the slurry is 30 μm.

[0072] The leaching rate is 92.45wt% for Cu and 91.90wt% for Co. The concentration of SO2 in the flue gas is 2.5wt%, and additional heat supplementation is required.

[0073] Comparative Example 3

[0074] The difference from Example 2 is that during the fluidized bed roasting reaction, the excess coefficient of oxygen-enriched air is 1.3.

[0075] The leaching rate is 90.11wt% for Cu and 89.35wt% for Co, and the concentration of SO2 in the flue gas is 2.7wt%. Additional heating is also required.

[0076] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects: using the above process to treat low-grade copper-cobalt sulfide concentrate is beneficial to improving the extraction rate of copper and cobalt elements to a certain extent, and greatly reducing the process cost and improving environmental protection.

[0077] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for extracting copper and cobalt from low-grade copper-cobalt sulfide concentrate, characterized in that: The copper content in the low-grade copper-cobalt sulfide concentrate is ≤20wt%, and the cobalt content is ≤10wt%. The method for extracting copper and cobalt from the low-grade copper-cobalt sulfide concentrate comprises: Grinding the low-grade copper-cobalt sulfide concentrate with water to obtain a pulp, wherein the concentration of the pulp is 70-80wt%, and the D50 of the solid particles is 50-100 μm; The ore pulp is subjected to a fluidized bed roasting reaction in oxygen-enriched air to obtain copper-cobalt roasted sand and sulfur-containing flue gas, wherein the excess coefficient of the oxygen-enriched air during the fluidized bed roasting reaction is 1.5 to 2; Adding a dispersant during the grinding process; the amount of the dispersant is 1 to 5 wt% of the total weight of the slurry; During the fluidized bed roasting reaction, the air flow rate is 0.6-0.7 m / s, and the boiling height is 1.5-1.8 m.

2. The method for extracting copper and cobalt from low-grade copper-cobalt sulfide concentrate according to claim 1, characterized in that: The pH of the slurry is 5-7.

3. The method for extracting copper and cobalt from low-grade copper-cobalt sulfide concentrate according to claim 1 or 2, characterized in that: The concentration of the ore pulp is 75-80wt%.

4. The method for extracting copper and cobalt from low-grade copper-cobalt sulfide concentrate according to claim 1 or 2, characterized in that: The temperature of the fluidized bed roasting reaction process is 750-900°C.

5. The method for extracting copper and cobalt from low-grade copper-cobalt sulfide concentrate according to claim 3, characterized in that: The method for extracting copper and cobalt elements from low-grade copper-cobalt sulfide concentrate also includes: wet leaching the copper-cobalt roasted sand to obtain metallic copper and metallic cobalt.

6. The method for extracting copper and cobalt from low-grade copper-cobalt sulfide concentrate according to claim 5, characterized in that: The method for extracting copper and cobalt from low-grade copper-cobalt sulfide concentrate also includes: The sulfur-containing flue gas is subjected to dust collection treatment to obtain smoke dust and flue gas containing sulfur dioxide; and The sulfur dioxide-containing flue gas is used as a raw material to produce acid to obtain sulfuric acid.

7. The method for extracting copper and cobalt from low-grade copper-cobalt sulfide concentrate according to claim 1, characterized in that: The low-grade copper-cobalt sulfide concentrate comprises 12-20% Cu and 0.5-10% Co in terms of weight percentage of the low-grade copper-cobalt sulfide concentrate.