A method for strengthening metal protective coating based on high repetition rate ultrashort pulse laser
The surface of the metal protective coating prepared by arc ion plating is strengthened through high repetition frequency and ultra-short pulse laser technology to form a dense remelting strengthening layer, which solves the problems of surface roughness and insufficient high-temperature oxidation resistance of the coating, and achieves surface Improved purification and anti-corrosion properties.
Patent Information
- Application Number
- CN202210138075.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-15
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-02-15
AI Technical Summary
The metal protective coating prepared by arc ion plating has a rough surface and insufficient high-temperature oxidation and corrosion resistance. Moreover, laser strengthening technology has problems such as micro-cracks, obvious heat-affected zones, and weak coating bonding force.
High repetition frequency ultra-short pulse laser is used to perform surface strengthening treatment on the metal protective coating prepared by arc ion plating. By adjusting laser parameters such as repetition frequency, pulse width, spot diameter and scanning speed, a dense remelting strengthening layer is formed to achieve surface Micro-polishing, purification and grain refinement control the distribution of rare earth elements and eliminate surface defects.
Significantly improve the surface wear resistance, high temperature oxidation resistance and corrosion resistance of the metal coating, eliminate surface ablation and loss, achieve a reduction in surface roughness and extend the long life of the coating.
Smart Images

Figure CN114657517B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal protective coating surface strengthening, in particular to a method for strengthening metal protective coating based on high repetition rate ultrashort pulse laser. Technical Background
[0002] Metal protective coatings, such as NiCrAlY, NiCoCrAlY, and NiAlHf, are widely used in various high-temperature hot end components and bonding layer materials in thermal barrier coating systems due to their excellent high-temperature oxidation resistance and corrosion resistance. Arc ion plating, as a coating preparation technology widely used in industrial production processes, has received increasing attention in the preparation of high-temperature protective coatings. The advantages of this technology are mainly reflected in the following aspects: First, the vacuum preparation environment improves the cleanliness of the coating surface and prevents the coating from being contaminated during the preparation process, so that the coating has stronger interfacial bonding and higher oxidation resistance and corrosion resistance; second, it overcomes the line of sight effect, so that arc ion plating can deposit a uniform coating on complex geometric components such as turbine blades; third, the microstructure of the resulting coating is fine and uniform, which is conducive to the formation of a protective oxide scale on the coating surface at high temperatures. However, the surface of the coating prepared by arc ion plating is still relatively rough, and its high-temperature oxidation resistance and corrosion resistance need to be further improved.
[0003] As a new surface modification technology, laser surface modification technology has been successfully applied to coating surface modification. During the laser remelting process, high-energy-density laser acts on the material surface, remelting the material surface, and the remelted material rapidly solidifies to form a uniform and dense microstructure, which can significantly improve the quality of the coating and extend its service life. However, in general laser strengthening technology, there are microcracks on the surface of the remelted strengthening layer, obvious heat-affected zone, obvious gap between the remelted layer and the substrate, weak coating bonding, and ablation of the coating surface. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a method for strengthening metal protective coatings based on high repetition rate ultrashort pulse lasers, which uses high repetition rate ultrashort pulse lasers to perform surface strengthening treatment on the metal protective coating prepared by arc ion plating, forming a dense remelting strengthening layer on its surface, achieving the beneficial effects of polishing and purifying the coating surface, regulating the surface microstructure, and refining the grains, thereby effectively improving the surface wear resistance, high temperature oxidation resistance and corrosion resistance of the metal coating.
[0005] High repetition rate ultrashort pulse laser technology, using the thermal effect of ultrashort pulse laser, achieves the strengthening and micro-polishing of the material surface through strict adjustment of process parameters. More importantly, this technology does not cause ablation and loss of the material surface. There is no obvious heat-affected zone, no cracks in the remelted layer, and a series of beneficial effects such as surface micro-polishing, surface purification, surface grain refinement, regulation of rare earth element distribution, uniform second phase, and elimination of impurities, large particles, pores, segregation and other defects on the original coating surface are achieved.
[0006] A method for strengthening a metal protective coating based on a high repetition rate ultrashort pulse laser comprises the following steps:
[0007] Step 1: Use acetone, alcohol, and deionized water to clean the surface of the metal protective coating prepared by arc ion plating in sequence, and then dry the surface.
[0008] Step 2: Place the dried coating in a processing chamber, introduce Ar gas, and perform processing after the processing chamber is filled with Ar gas.
[0009] Step 3: Focus the ultrashort pulse laser on the surface of the sample to be processed, and adjust the relevant laser processing parameters: the repetition frequency is 10-40MHz, the pulse width is 10ps-200fs, the spot diameter is 20μm, the laser wavelength is 1030nm, and the laser single pulse energy density is 0.05-1J / cm 2 The scanning speed of the galvanometer is 10 to 200 mm / s, the processing path is a horizontal or orthogonal path, the scanning interval is 5 to 20 μm, the scanning number is 1, and the surface of the metal protective coating is strengthened.
[0010] It can be observed on the surface of the processed coating that the thickness of the remelted strengthening layer is 3 to 10 μm, there are no microcracks on the surface and inside, it is dense and uniform, the heat affected zone is controlled at 0 to 1 μm, and the surface roughness is 0.5 to 1 μm.
[0011] In step 1, the metal protective coating is NiCrAlY, NiCoCrAlY or NiAlHf, with a surface roughness of 2 to 5 μm and a thickness of 20 to 100 μm.
[0012] In step 2, the gas flow rate of Ar gas is 10 to 20 L / min.
[0013] Advantages of the present invention:
[0014] 1. High repetition rate ultrashort pulse laser is used to strengthen the metal protective coating, with a 3-10μm remelting strengthening layer, no cracks in the remelting layer, and an extremely thin heat-affected zone of only 0-1μm.
[0015] 2. Use high-repetition-rate ultrashort pulse laser to strengthen the metal protective coating, achieve micro-polishing of the metal protective coating surface, eliminate spraying defects, micro-cracks, and large particles, and significantly reduce the surface roughness.
[0016] 3. Use high repetition rate ultrashort pulse laser to strengthen the metal protective coating. Only use the thermal effect of ultrashort pulse laser to control the surface temperature between the melting temperature and the evaporation temperature, which will not cause ablation and loss of the coating surface.
[0017] 4. High-repetition-rate ultrashort pulse laser is used to strengthen the metal protective coating, achieving the beneficial effects of surface purification of the metal protective coating, surface grain refinement, regulation of rare earth element distribution, and uniform second phase, greatly improving the high-temperature oxidation resistance of the metal protective coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 Schematic diagram of the NiCoCrAlY coating prepared by arc ion plating in Example 1 before and after high repetition rate ultrashort pulse laser strengthening. (a) Surface morphology and corresponding surface roughness of the untreated NiCoCrAlY coating prepared by arc ion plating; (b) Cross-sectional morphology of the untreated NiCoCrAlY coating prepared by arc ion plating; (c) Surface morphology and corresponding surface roughness of the NiCoCrAlY coating after high repetition rate ultrashort pulse laser treatment; (d) Cross-sectional morphology of the NiCoCrAlY coating after high repetition rate ultrashort pulse laser treatment.
[0019] Figure 2 Schematic diagram of the NiCoCrAlY coating prepared by arc ion plating in Example 1, before and after high-repetition-rate ultrashort pulse laser strengthening, and then oxidized at 1100°C for 20h. (a) Surface morphology of the untreated NiCoCrAlY coating prepared by arc ion plating after oxidized at 1100°C for 20h, with the upper right corner showing a partial enlarged view; (b) Cross-sectional morphology of the untreated NiCoCrAlY coating prepared by arc ion plating after oxidized at 1100°C for 20h; (c) Surface morphology of the NiCoCrAlY coating treated by high-repetition-rate ultrashort pulse laser after oxidized at 1100°C for 20h, with the upper right corner showing a partial enlarged view; (d) Cross-sectional morphology of the NiCoCrAlY coating treated by high-repetition-rate ultrashort pulse laser after oxidized at 1100°C for 20h. DETAILED DESCRIPTION
[0020] The embodiments of the present invention are described below.
[0021] Example 1
[0022] Acetone, alcohol, and deionized water were used to clean the surface of the metal protective coating NiCoCrAlY prepared by arc ion plating with an initial surface roughness of 3.5μm and a thickness of 40μm, and then the surface was dried. The dried coating was placed in a processing chamber, and Ar gas was introduced at a gas flow rate of 20L / min. The processing was carried out after the processing chamber was filled with Ar gas. The ultrashort pulse laser was focused on the surface of the sample to be processed, and the corresponding laser processing parameters were adjusted: the repetition frequency was 20MHz, the pulse width was 250fs, the spot diameter was 20μm, the laser wavelength was 1030nm, and the laser single pulse energy density was 0.2J / cm 2 The scanning speed of the galvanometer is 40mm / s, the processing path is horizontal, the scanning interval is 15μm, and the scanning number is 1. It can be observed on the surface of the processed coating that the thickness of the remelted strengthening layer is 6μm, there are no microcracks on the surface and inside, it is dense and uniform, the heat affected zone is less than 0.5μm, and the surface roughness is 0.9μm. Figure 1 shown.
[0023] The processed and unprocessed samples were subjected to high-temperature oxidation experiments in a high-temperature furnace at 1100°C for 20 hours. The unprocessed coating was obviously peeled off locally, and the thickness of the thermally grown oxide on its surface was 2.5μm. The coating strengthened by high-repetition-rate ultrashort pulse laser remained intact, and the surface oxide was finer and more uniform, and the thickness of the thermally grown oxide on its surface was only 1.5μm. Figure 2 It shows that the oxidation resistance of NiCrAlY coating is significantly improved after high repetition rate ultrashort pulse laser strengthening.
[0024] Example 2
[0025] Acetone, alcohol, and deionized water were used in turn to prepare the metal protective coating NiCrAlY by arc ion plating with an initial surface roughness of 5μm and a thickness of 50μm. The surface was cleaned and then dried. The dried coating was placed in a processing chamber, and Ar gas was introduced at a gas flow rate of 15L / min. The processing was carried out after the processing chamber was filled with Ar gas. The ultrashort pulse laser was focused on the surface of the sample to be processed, and the corresponding laser processing parameters were adjusted: the repetition frequency was 20MHz, the pulse width was 300fs, the spot diameter was 20μm, the laser wavelength was 1030nm, and the laser single pulse energy density was 0.16J / cm 2 The scanning speed of the galvanometer is 50 mm / s, the processing path is horizontal, the scanning interval is 20 μm, and the number of scans is 1.
[0026] It can be observed on the surface of the processed coating that the thickness of the remelted strengthening layer is 8μm, there are no microcracks on the surface and inside, it is dense and uniform, the heat affected zone is less than 0.5μm, and the surface roughness is 1μm.
[0027] The processed and unprocessed samples were subjected to high-temperature oxidation experiments in a high-temperature furnace at 1100°C for 20 hours. The unprocessed coating was obviously peeled off locally, and the thickness of the thermally grown oxide on its surface was 3.9μm. The coating strengthened by high-repetition-rate ultrashort pulse laser remained intact, and the surface oxide was finer and more uniform, and the thickness of the thermally grown oxide on its surface was only 1.9μm. This shows that the oxidation resistance of the NiCrAlY coating has been significantly improved after high-repetition-rate ultrashort pulse laser strengthening.
[0028] Example 3
[0029] Acetone, alcohol, and deionized water were used in turn to prepare the metal protective coating NiAlY with an initial surface roughness of 3.8μm and a thickness of 60μm by arc ion plating. The surface was cleaned and then dried. The dried coating was placed in a processing chamber, and Ar gas was introduced at a gas flow rate of 18L / min. The processing was carried out after the processing chamber was filled with Ar gas. The ultrashort pulse laser was focused on the surface of the sample to be processed, and the corresponding laser processing parameters were adjusted: the repetition frequency was 20MHz, the pulse width was 1ps, the spot diameter was 20μm, the laser wavelength was 1030nm, and the laser single pulse energy density was 0.38J / cm 2 The scanning speed of the galvanometer is 20 mm / s, the processing path is horizontal, the scanning interval is 20 μm, and the number of scans is 1.
[0030] It can be observed on the surface of the processed coating that it is a 7μm thick remelted strengthening layer with no microcracks on the surface and inside, dense and uniform, its heat affected zone is less than 0.5μm, and its surface roughness is 1.2μm.
[0031] The processed and unprocessed samples were subjected to high-temperature oxidation experiments in a high-temperature furnace at 1100°C for 20 hours. The unprocessed coating was obviously peeled off locally, and the thickness of the thermally grown oxide on its surface was 2.8μm. The coating strengthened by high-repetition-rate ultrashort pulse laser remained intact, and the surface oxide was finer and more uniform, and the thickness of the thermally grown oxide on its surface was only 1.4μm. This shows that the oxidation resistance of the NiCrAlY coating has been significantly improved after high-repetition-rate ultrashort pulse laser strengthening.
Claims
1. A method for strengthening metal protective coating based on high repetition rate ultrashort pulse laser, characterized in that: The specific steps are as follows: Step 1: using acetone, alcohol, and deionized water to clean the surface of the metal protective coating prepared by arc ion plating in sequence, and then drying the surface; the metal protective coating is NiCrAlY, NiCoCrAlY or NiAlHf, with a surface roughness of 2-5 μm and a thickness of 20-100 μm; Step 2: Place the dried coating in a processing chamber, introduce Ar gas, and perform processing after the processing chamber is filled with Ar gas; Step 3: Focus the ultrashort pulse laser on the surface of the sample to be processed, and adjust the relevant laser processing parameters: the repetition frequency is 10 ~ 40 MHz, the pulse width is 10 ps ~ 200 fs, the spot diameter is 20 μm, the laser wavelength is 1030nm, and the laser single pulse energy density is 0.05 ~ 1 J / cm 2 The scanning speed of the galvanometer is 10~200 mm / s, the processing path is a horizontal or orthogonal path, the scanning interval is 5~20 μm, the scanning number is 1, and the surface strengthening treatment of the metal protective coating is performed.
2. The method for strengthening metal protective coating based on high repetition rate ultrashort pulse laser according to claim 1, characterized in that: After surface strengthening treatment, the thickness of the remelted strengthening layer on the surface of the metal protective coating is 3~10 μm, there are no microcracks on the surface and inside, it is dense and uniform, its heat affected zone is controlled at 0~1 μm, and its surface roughness is 0.5~1 μm.
3. The method for strengthening metal protective coating based on high repetition rate ultrashort pulse laser according to claim 1, characterized in that: In step 2, the gas flow rate of Ar gas is 10-20 L / min.
Citation Information
Cited By