Method for forming transition metal niobium nitride film on substrate by atomic layer deposition and related semiconductor device structure
By forming a transition metal niobium nitride film on a substrate using the ALD method, the problems of imperfect effective work function of polycrystalline silicon gate electrodes and tilting of DRAM capacitors were solved, realizing a gate electrode structure with ideal work function and a capacitor with enhanced oxidation resistance.
Patent Information
- Application Number
- CN202210306863.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2016-11-01
- Filing Date
- 2017-11-01
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2037-11-01
AI Technical Summary
In the prior art, doped polysilicon as a gate electrode material has problems such as imperfect effective work function and gate depletion in advanced node applications. Furthermore, the aspect ratio of DRAM capacitors causes tilting, requiring alternative materials to prevent capacitor array tilting and device failure.
Atomic layer deposition (ALD) is used to form a transition metal niobium nitride film on a substrate. By alternately contacting the transition metal precursor, niobium precursor, and nitrogen precursor, the deposition process is controlled to form a self-saturating monolayer or sub-monolayer. The thickness and composition of the film are adjusted to achieve the desired properties.
This invention achieves a gate electrode structure with ideal effective work function in advanced node applications, improves the mechanical strength and oxidation resistance of DRAM capacitors, prevents capacitor tilting, and ensures device stability.
Smart Images

Figure CN114657535B_ABST
Abstract
Description
[0001] Divisional Application Instructions
[0002] This application is a divisional application of an invention patent application with a filing date of November 1, 2017, a national application number of 201711057557.9, and titled “Method for forming a transition metal niobium nitride film on a substrate by atomic layer deposition and related semiconductor device structure”.
[0003] CROSS-REFERENCE TO RELATED APPLICATIONS
[0004] This application claims priority to U.S. Provisional Application Serial No. 62 / 415,828, filed on November 1, 2016, the contents of which are incorporated herein by reference. Technical Field
[0005] The present application generally relates to methods of forming transition metal niobium nitride films on substrates by atomic layer deposition and related semiconductor device structures. Background Art
[0006] Metal-Oxide-Semiconductor (MOS) technology typically uses n-type doped polysilicon as the gate electrode material. However, doped polysilicon may not be an ideal gate electrode material for advanced node applications. For example, although doped polysilicon is conductive, there may still be a surface region that may be doped with carriers under bias conditions. This region may appear as additional gate insulator thickness, commonly referred to as gate depletion, and may result in an equal oxide thickness. Although the gate depletion region may be only a few angstroms, The gate oxide thickness is thin in terms of order of magnitude, but it may become significant as the gate oxide thickness decreases in advanced node applications. As another example, polysilicon does not exhibit an ideal effective work function (eWF) for NMOS and PMOS devices. To overcome the imperfect effective work function of doped polysilicon, a threshold voltage adjustment implant may be employed. However, as device geometries decrease in advanced node applications, the threshold voltage adjustment implant process may become increasingly complex and impractical.
[0007] To overcome the problems associated with doped polysilicon gate electrodes, alternative materials, such as transition metal nitrides, may be used to replace the undesirable doped polysilicon gate material. For example, transition metal nitrides may be used to provide a gate electrode structure having an effective work function that is ideal for NMOS and PMOS devices, where the effective work function of the gate electrode structure, i.e., the energy required to extract electrons, must be compatible with the barrier height of the semiconductor material. For example, in the case of a PMOS device, the desired effective work function is about 5.0 eV.
[0008] In addition, as the design rules of dynamic random access memory (DRAM) are reduced, the size of memory cells continues to decrease. Therefore, the height of capacitors associated with DRAM has continued to increase and the thickness has become smaller to maintain the desired charge capacitance. The height of the capacitor has increased and the thickness of the capacitor has decreased because the charge capacitance is proportional to the surface area of the electrode and the dielectric constant of the dielectric layer, and is inversely proportional to the distance between the electrodes, i.e., the thickness of the dielectric layer. The high aspect ratio of the capacitor may cause "leaning" and this "leaning" may vary depending on the properties and / or thickness of the electrodes containing the capacitor. For example, when the aspect ratio of the capacitor is greater than about 15:1, a DRAM capacitor containing titanium nitride as an electrode material may tilt. Therefore, DRAM capacitor electrodes may require alternative materials to prevent tilting of the capacitor array (storage node) and related device failure caused by the tilted structure.
[0009] Atomic layer deposition (ALD) can be used to deposit transition metal nitride films, such as tantalum nitride (TaN), titanium nitride (TiN), tungsten nitride (WN), and niobium nitride (NbN). However, the electronic, crystallographic, and physical properties of known ALD transition metal nitride films may be limited and new ALD transition metal nitride films may be needed. Summary of the invention
[0010] This content is provided to introduce a selection of concepts in a simplified form. These concepts are further described in detail in the detailed description of the exemplary embodiments disclosed below. This summary is not intended to identify key features or essential features of the claimed subject matter, nor is it intended to be used to limit the scope of the claimed subject matter.
[0011] In some embodiments, a method for forming a transition metal niobium nitride film on a substrate by atomic layer deposition is provided. The method may include contacting the substrate with a first reactant comprising a transition metal precursor, contacting the substrate with a second reactant comprising a niobium precursor, and contacting the substrate with a third reactant comprising a nitrogen-containing precursor.
[0012] In some embodiments, a semiconductor device structure is provided. The semiconductor device structure may include a semiconductor body and an electrode including a transition metal niobium nitride deposited on the semiconductor body.
[0013] For the purpose of summarizing the present invention and the benefits achieved relative to the prior art, certain objects and benefits of the present invention are described herein. Of course, it should be understood that any specific embodiment of the present invention does not necessarily achieve all of these objects or advantages. Thus, for example, those skilled in the art will understand that the present invention can be implemented or carried out in the following manner: achieving or optimizing one or more advantages taught or suggested herein without necessarily achieving other objects or advantages that may be taught or suggested herein.
[0014] All of these embodiments are included within the scope of the present invention. These and other embodiments will be apparent to those skilled in the art from the following detailed description of certain embodiments with reference to the accompanying drawings, but the present invention is not limited to any of the disclosed specific embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] While the specification and claims conclude and particularly point out and distinctly claim what are regarded as embodiments of the present invention, it is believed that the advantages of the embodiments of the present invention will be better understood from the description of certain examples thereof taken in conjunction with the accompanying drawings, in which:
[0016] Figure 1 An example of a process for forming a transition metal niobium nitride according to an embodiment of the present invention is shown;
[0017] Figure 2 An example of a process for forming transition metal niobium nitrides of other embodiments of the present invention is shown;
[0018] Figure 3 Schematically shows a semiconductor device structure including a PMOS semiconductor according to an embodiment of the present invention;
[0019] Figure 4 A semiconductor device structure including a DRAM capacitor according to an embodiment of the present invention is schematically shown;
[0020] Figure 5 schematically shows a partially fabricated semiconductor device structure including a transition metal niobium nitride layer deposited in accordance with an embodiment of the present invention;
[0021] Figure 6 A reaction system configured to implement an embodiment of the present invention is schematically shown. DETAILED DESCRIPTION
[0022] The illustrations shown herein are not intended to be actual views of any particular material, structure, or device, but are merely idealized representations used to describe embodiments of the present invention.
[0023] The term "atomic layer deposition" (ALD) as used herein may refer to a vapor deposition process in which a deposition cycle, preferably a plurality of continuous deposition cycles, is performed in a process chamber. Generally speaking, during each cycle, a precursor is chemically absorbed onto a deposition surface (e.g., a substrate surface or a previously deposited lower surface, such as material from a previous ALD cycle), forming a monolayer or sub-monolayer that is not easily reacted with other precursors (i.e., a self-limiting reaction). Then, if desired, a reactant (e.g., another precursor or a reactive gas) may subsequently be introduced into the process chamber for converting the chemically absorbed precursor into the desired material on the deposition surface. Generally speaking, the reactant is capable of further reacting with the precursor. In addition, a purge step may also be used during each cycle to remove excess precursor from the process chamber after conversion of the chemically absorbed precursor and / or to remove excess reactants and / or reaction byproducts from the process chamber. In addition, the term "atomic layer deposition" as used herein is also intended to include processes named by related terms, such as "chemical vapor atomic layer deposition," "atomic layer epitaxy" (ALE), molecular beam epitaxy (MBE), gas source MBE, or organometallic MBE, and chemical beam epitaxy when performed with alternating pulses of alternative precursor compositions, reactive gases, and purge (e.g., inert carrier) gases.
[0024] As used herein, the term "substrate" may refer to any underlying material or materials that may be used or upon which a device, circuit, or film may be formed.
[0025] The present invention includes device structures and methods that can be used to form transition metal niobium nitride films or films containing transition metal niobium nitrides. Existing ALD transition metal nitride films may be limited due to their inability to tune certain characteristics of the ALD transition metal nitride films; these characteristics may include effective work function, resistivity, density, and Young's modulus.
[0026] For example, it is known that the effective work function of a gate electrode structure may vary as its thickness varies, i.e., the effective work function of a gate electrode structure may increase or decrease as the thickness of the material comprising the gate electrode decreases. As device geometries decrease in advanced node applications, the thickness of the corresponding device film, such as the gate electrode, may also decrease as the effective work function of the film changes accordingly. This change in the effective work function of the gate electrode when the thickness is reduced may result in an undesirable effective work function for NMOS and PMOS device structures. In addition, it is also known that the properties of the conductive materials comprising conventional DRAM capacitor electrodes may be undesirable in terms of mechanical strength and oxidation resistance. Therefore, there is a need to provide methods and structures for more ideal transition metal nitride films. Embodiments of such methods and structures are disclosed in further detail below.
[0027] ALD is based on a generally self-limiting reaction in which continuous and alternating pulses of reactants are used to deposit about 1 monolayer of an atom (or molecule) of material per deposition cycle. Deposition conditions and precursors are generally selected to provide a self-saturating reaction, such as an absorber layer of one reactant leaving a surface cap that cannot react with a gas phase reactant of the same reactant. The substrate is then contacted with a different reactant, which reacts with the previous cap to enable continued deposition. Therefore, the alternating pulses of each cycle generally leave no more than about one monolayer of the desired material. However, as described above, the skilled person will recognize that in one or more ALD cycles, more than one monolayer of material may be deposited, for example, if some gas phase reactions occur despite the alternating nature of the process.
[0028] In some embodiments of the present invention, the ALD type process for depositing transition metal niobium nitride films can be referred to as Figure 1 , which shows a non-limiting example ALD-type process 100. After initial surface capping, if necessary or desired, an ALD pulse sequence may be initiated at step 102. The ALD-type process 100 may then continue with at least one deposition cycle, which may include contacting the substrate with a first reactant 104, contacting the substrate with a second reactant 106, and contacting the substrate with a third reactant 108. Once the first, second, and third reactants have been exposed to the substrate, the deposition cycle 108 may be repeated until a predetermined thickness of transition metal niobium nitride is reached 110. When the desired predetermined thickness of transition metal niobium nitride is reached, the deposition cycle ends and the process may be exited 112.
[0029] In some embodiments, the ALD-type process 100 for depositing transition metal niobium nitride may include at least one deposition cycle, wherein at least one deposition cycle may include exposing the substrate to a first reactant, removing any unreacted first reactant and reaction byproducts from the reaction space, exposing the substrate to a second reactant followed by a second removal step, and exposing the substrate to a third reactant followed by a third removal step.
[0030] In some embodiments, the ALD-type process 100 for depositing transition metal niobium nitride may include at least one deposition cycle, wherein at least one deposition cycle may include exposing a substrate to a first reactant, exposing the substrate to a second reactant, removing any unreacted first and second reactants and reaction byproducts, and exposing the substrate to a third reactant followed by a second removal step.
[0031] In some embodiments, an ALD-type process for depositing transition metal niobium nitride may include at least one deposition cycle, wherein at least one deposition cycle may include exposing the substrate to a second reactant, removing any unreacted second reactant and reaction byproducts from the reaction space, exposing the substrate to a first reactant followed by a second removal step, and exposing the substrate to a third reactant followed by a third removal step.
[0032] Additionally, it should be understood that in some embodiments, each contacting step may be repeated one or more times before proceeding to a subsequent processing step, ie, before a subsequent contacting step or a removal / purging step.
[0033] In some embodiments, the first reactant may include a metal precursor, particularly a transition metal precursor. The transition metal precursor or compound may include at least one of a transition metal selected from the group consisting of scandium (Sc), yttrium (Y), titanium (Ti), zirconium (Zr), hafnium (Hf), vanadium (V), niobium (Nb), tantalum (Ta), chromium (Cr), molybdenum (Mo), tungsten (W), manganese (Mn), technetium (Tc), rhenium (Re), iron (Fe), ruthenium (Ru), osmium (Os), cobalt (Co), rhodium (Rh), iridium (Ir), nickel (Ni), palladium (Pd), platinum (Pt), copper (Cu), silver (Ag), gold (Au), zinc (Zn), cadmium (Cd), and mercury (Hg).
[0034] As a non-limiting example embodiment, a transition metal halide reactant, such as titanium tetrachloride (TiCl 4 ) can be used as a transition metal precursor in the ALD process.
[0035] In some embodiments, the second reactant may include a niobium precursor, and in some embodiments, the method may include selecting the niobium precursor to include at least one of: niobium pentachloride (NbCl 5 ), niobium pentafluoride (NbF 5 ), niobium pentaboride (NbB 5 ), niobium pentaiodide (NbI 5 ) and niobium pentabromide (NbBr 5 ).
[0036] In some embodiments, the third reactant may include a nitrogen precursor, and in some embodiments, the method may include selecting the nitrogen precursor to include ammonia (NH 3 ), ammonium salts, hydrogen azide (HN 3 ), alkyl derivatives of hydrogen azide, hydrazine (N 2 H 4 ), hydrazine salts, alkyl derivatives of hydrazine, nitrogen fluoride (NF 3 ), and nitrogen (N 2 ) of the plasma excitation material.
[0037] The precursors can be separated by an inert gas such as argon (Ar) or nitrogen (N 2 ) to prevent gas phase reactions between the reactants and to enable the surface reaction to self-saturate. However, in some embodiments, the substrate may be moved to separately contact the first transition metal reactant, the second niobium reactant, and the third nitrogen reactant. Since the reactions are self-saturating, strict temperature control of the substrate and precise dosage control of the precursors are generally not required. However, the substrate temperature may be such that the gaseous species do not condense into a monolayer or decompose on the surface. Before the substrate is contacted with the next reactive chemical, excess chemicals and reaction byproducts, if any, may be removed from the surface of the substrate, such as by purging the reaction space or by moving the substrate. With the assistance of an inert purge gas, unwanted gas molecules may be effectively exhausted from the reaction space. A vacuum pump may be used to assist in purging.
[0038] According to some embodiments, an ALD-type process can be used to form a transition metal niobium nitride film, such as a titanium niobium nitride film, on a substrate, such as an integrated circuit workpiece. Each ALD cycle may include three distinct deposition steps or phases. In the first phase ("transition metal phase") of the deposition cycle, the substrate surface on which deposition is desired is contacted with a first reactant (i.e., a titanium source material or chemical) comprising a transition metal, such as titanium, which is chemically absorbed onto the substrate surface, to form no more than about one monolayer of reactant species on the substrate surface.
[0039] In some embodiments, the transition metal (e.g., titanium) source chemical (also referred to herein as a "transition metal compound," or in some embodiments, a "titanium compound") is a halide, and the absorbed monolayer is terminated with a halogen ligand. In some embodiments, the titanium halide may be titanium tetrachloride (TiCl 4 ).
[0040] In some embodiments, for example, excess transition metal (e.g., titanium, tantalum, or tungsten) source material and reaction byproducts (if present) can be removed from the substrate surface by purging with an inert gas. Excess transition metal source material and any reaction byproducts can be removed with the aid of a vacuum created by a purge system.
[0041] In the second stage of the deposition cycle (the "niobium stage"), the substrate is contacted with a niobium precursor. In some embodiments, the niobium precursor may include niobium pentachloride (NbCl 5 ), niobium pentafluoride (NbF 5 ), niobium pentaboride (NbB 5 ), niobium pentaiodide (NbI 5 ) and niobium pentabromide (NbBr 5 ) at least one of.
[0042] The second niobium reactant can be absorbed on the substrate surface by inserting or replacing the titanium-containing molecules remaining on the substrate surface. Thus, the substrate surface includes a mixture of metal-containing molecules remaining on the substrate surface, which includes a mixture of transition metal species (e.g., titanium) and niobium species.
[0043] In some embodiments, for example, a purge gas pulse and / or vacuum generated by a pumping system removes excess second source chemical and reaction byproducts, if present, from the substrate surface. The purge gas is preferably any inert gas, such as, but not limited to, argon (Ar), nitrogen (N 2 ) or helium (He). One stage is generally considered to be immediately followed by another if a purge (ie, a purge gas pulse) or other reactant removal step intervenes.
[0044] In the third phase (“nitrogen phase”) of the deposition cycle, the substrate is contacted with a nitrogen precursor. In some embodiments, the nitrogen precursor may include ammonia (NH 3 ), ammonium salts, hydrogen azide (HN 3 ), alkyl derivatives of hydrogen azide, hydrazine (N 2 H 4 ), hydrazine salts, alkyl derivatives of hydrazine (e.g., tert-butylhydrazine (C 4 H 9 N 2 H 3 ), methylhydrazine (CH 3 NHNH 2 ), dimethylhydrazine ((CH 3 ) 2 N 2 H 2 )), Nitrogen fluoride (NF 3 ) and nitrogen (N 2 ) of the plasma excitation material.
[0045] The third reactant comprising a nitrogen precursor can react with the titanium and niobium containing molecules left on the surface of the substrate. Preferably, in the third stage, the third stage nitrogen is incorporated into the film by the interaction of the third nitrogen containing reactant with the monolayer left by the transition metal (e.g., titanium) source material and the niobium source material. In some embodiments, the reaction between the third nitrogen containing precursor and the chemically adsorbed transition metal and niobium species produces a transition metal niobium nitride thin film on the substrate.
[0046] In some embodiments, for example, a purge gas pulse and / or vacuum generated by a pumping system removes excess third source chemical and reaction byproducts, if present, from the substrate surface. The purge gas may be any inert gas, such as, but not limited to, argon (Ar), nitrogen (N 2) or helium (He). One stage is generally considered to be immediately followed by another if a purge (ie, a purge gas pulse) or other reactant removal step intervenes.
[0047] In some embodiments, the ALD process of method 100 may include a plasma enhanced atomic layer deposition (PEALD) process. In such embodiments, the third reactant may include a nitrogen precursor and may also include nitrogen (N 2 In some embodiments, the third reactant may include a nitrogen precursor and may also include a plasma-excited species of any reactant including a nitrogen component. In some embodiments, the third reactant may be prepared by adding additional plasma-excited species, such as hydrogen (H 2 ) of the plasma excitation material, and the third reactant, such as nitrogen (N 2 ) of the plasma-excited species is supplied to the substrate.
[0048] In embodiments where the ALD process comprises a plasma enhanced atomic layer deposition method utilizing plasma excited species, the substrate temperature during deposition may include a temperature between about 250° C. and about 400° C. In embodiments where the ALD process comprises a thermal atomic layer deposition method (i.e., in the absence of plasma excited species), the substrate temperature during deposition may include a temperature between about 350° C. and about 450° C.
[0049] In some embodiments, the transition metal niobium nitride film formed according to one or more processes described herein is not a nanolaminated film. That is, separate and distinct layers may not be visible within the transition metal niobium nitride film. For example, a continuous or substantially continuous transition metal niobium nitride film may be formed.
[0050] Usually expressed as The deposition rate of thin films using ALD with pulse cycles depends on many factors, including, for example, the number of reactive surface sites or active sites available on the surface and the bulkiness of the chemically adsorbed molecules. In some embodiments, the deposition rate of such films can be between about 0.3 and about In some embodiments, the deposition rate may be about 0.3, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, / Pulse cycle.
[0051] In some embodiments of the present disclosure, reference may be made to Figure 2200. An ALD-type process for depositing transition metal niobium nitride films is illustrated, which shows a non-limiting example method 200. After initial surface capping, if necessary or desired, an ALD pulse sequence may be initiated at step 202. The ALD-type process 200 may then continue for at least one complete deposition cycle 203.
[0052] In some embodiments, a process for depositing a transition metal niobium nitride film includes a deposition process for depositing a transition metal nitride component (e.g., multiple deposition cycles for depositing a transition metal nitride, such as multiple transition metal nitride sub-cycles), and a deposition process for adding a niobium component to the growing film (e.g., multiple deposition cycles including a precursor comprising niobium, such as multiple niobium nitride sub-cycles). For example, a process for making a transition metal niobium nitride film may include multiple complete deposition cycles, each complete deposition cycle including multiple transition metal nitride sub-cycles and multiple niobium nitride sub-cycles.
[0053] In some embodiments, a process for making a transition metal niobium nitride film having desired properties may include a plurality of complete deposition cycles, wherein each complete deposition cycle includes a ratio of a plurality of transition metal nitride sub-cycles to a plurality of niobium nitride sub-cycles optimized to obtain desired properties, such as Young's modulus, density, stoichiometry, resistivity, and crystal orientation. The ratio of the number of transition metal nitride sub-cycles to the number of niobium nitride sub-cycles for a complete deposition cycle may be expressed as a percentage having niobium nitride sub-cycles (e.g., niobium nitride sub-cycle percentage or niobium nitride deposition sub-cycle percentage). For example, a complete deposition cycle for depositing a transition metal niobium nitride film including one deposition cycle for depositing a transition metal nitride component (e.g., one transition metal nitride sub-cycle) and four deposition cycles for adding a niobium component (e.g., four niobium nitride sub-cycles) may have a niobium nitride sub-cycle percentage of about 80%. In some embodiments, a complete deposition cycle may have a niobium nitride sub-cycle percentage of about 10% to about 100%, including about 25% to about 98%, about 50% to about 95%, and about 75% to about 85%.
[0054] In some embodiments, one or more parameters of a transition metal nitride sub-cycle may be different from one or more parameters of another transition metal nitride sub-cycle. In some embodiments, one or more parameters of a transition metal nitride sub-cycle may be similar or identical to one or more parameters of another transition metal nitride sub-cycle, such that the transition metal nitride sub-cycles are performed under similar or identical processing conditions.
[0055] In some embodiments, one or more parameters of the niobium nitride sub-cycle may be different from one or more parameters of another niobium nitride sub-cycle. In some embodiments, one or more parameters of the niobium nitride sub-cycle may be similar or identical to one or more parameters of another niobium nitride sub-cycle, such that the niobium nitride sub-cycles are performed under similar or even identical processing conditions.
[0056] In some embodiments, the transition metal niobium nitride film formed according to one or more processes described herein is a nanolaminate film. That is, separate and distinct layers can be seen within the transition metal niobium nitride film. For example, the transition metal niobium nitride film can include a nanolaminate and can also include at least one layer of transition metal nitride and at least one layer of niobium nitride.
[0057] In some embodiments, the transition metal niobium nitride film formed according to one or more processes described herein is not a nanolaminated film. That is, separate and distinct layers may not be visible within the transition metal niobium nitride film. For example, a continuous or substantially continuous transition metal niobium nitride film may be formed.
[0058] As described above, in some embodiments, a process for forming a transition metal niobium nitride film of a desired thickness and / or composition may include an ALD deposition process (e.g., a transition metal nitride deposition sub-cycle and / or a niobium nitride deposition sub-cycle may include an ALD process). ALD-type processes are based on controlled surface reactions and are generally self-limiting. Although there may be some overlap in some cases, gas phase reactions are avoided by alternating and sequentially contacting the substrate with the precursors. The gas phase precursors are separated from each other in the reaction chamber, for example by removing excess precursors and / or precursor byproducts from the reaction chamber between precursor pulses. For example, an ALD deposition process may include contacting the substrate with a first reactant (e.g., a transition metal precursor for a transition metal nitride deposition sub-cycle) and a second reactant comprising niobium for a niobium nitride deposition sub-cycle, such that the first and / or second reactants are adsorbed onto the base surface, and contacting the substrate with a third reactant (e.g., a nitrogen precursor for a transition metal nitride deposition sub-cycle or a nitrogen precursor for a niobium nitride deposition sub-cycle). The substrate can be repeatedly exposed to the first precursor, the second precursor, and the third precursor to achieve the desired number of times for the film of the desired thickness and composition. After each contact step, excess precursor can be removed from the vicinity of the substrate, for example, by evacuating the reaction chamber and / or purging from the reaction space with an inert gas. For example, excess reactants and / or reaction byproducts can be removed from the reaction chamber between precursor pulses by evacuating the reaction chamber to discharge the excess reactants and / or reaction byproducts. In some embodiments, the reaction chamber can be purged between precursor pulses. The flow rate and time of each precursor are adjustable, and the purging step is also adjustable, allowing control of the dopant concentration and depth profile in the film.
[0059] Each cycle of the ALD process may include at least two different processes or stages. Providing and removing a precursor from the reaction space may be considered a stage. In the first process or stage of the ALD process of the transition metal nitride deposition sub-cycle, for example, a first precursor comprising a transition metal is provided and forms no more than about one monolayer on the surface of the substrate. The precursor is also referred to herein as a "transition metal precursor" or "transition metal reactant". In the second process or stage of the ALD process of the transition metal nitride deposition sub-cycle, for example, a nitrogen-containing precursor compound is provided and reacts with the adsorbed transition metal precursor to form a transition metal nitride. The third precursor may also be referred to as a "nitrogen precursor" or "nitrogen reactant". As described herein, the third precursor may include ammonia (NH 3 ) and / or another suitable nitrogen-containing compound capable of reacting with the adsorbed first reactant under processing conditions. The reaction preferably leaves an end cap, which is further reacted with the first precursor or another precursor for different stages.
[0060] Additional processes or stages may be added, and stages removed as needed, to adjust the composition of the final transition metal niobium nitride film. In some embodiments, the additional processes or stages may include one or more precursors that are different from the precursors of the first and second processes or stages. For example, one or more other precursors may be provided in the additional processes or stages. In some embodiments, the additional processes or stages may have similar or identical process conditions as the first and second processes or stages. In some embodiments, for a transition metal nitride deposition sub-cycle, one or more deposition sub-cycles typically begin by providing a transition metal precursor followed by a nitrogen precursor. In some embodiments, one or more deposition sub-cycles begin by providing a nitrogen precursor followed by a transition metal precursor. The deposition sub-cycles may be provided by a carrier gas such as nitrogen (N 2 ), argon (Ar) and / or helium (He) to provide one or more precursors. In some embodiments, the carrier gas may include another inert gas.
[0061] In some embodiments, during a first process or stage of the ALD process of the niobium nitride deposition sub-cycle, for example, a second precursor comprising niobium is provided and forms no more than about a monolayer on the substrate surface. This precursor is also referred to herein as a "precursor comprising niobium" or a "reactant comprising niobium". During a second process or stage of the ALD process of the niobium nitride deposition sub-cycle, for example, a third precursor comprising a nitrogen-containing compound is provided and reacts with the adsorbed precursor comprising niobium to form niobium nitride, thereby introducing niobium into the transition metal nitride film. This third precursor may also be referred to as a "nitrogen precursor" or a "nitrogen reactant". As described herein, the third precursor may comprise ammonia (NH 3) and / or another suitable nitrogen-containing compound or nitrogen-activated species. The nitrogen precursor for the niobium nitride deposition sub-cycle may be the same as or different from the nitrogen precursor for the transition metal nitride deposition sub-cycle.
[0062] Additional processes or stages may be added, and stages removed as needed, to adjust the composition of the final film. In some embodiments for depositing transition metal niobium nitride films, one or more niobium nitride deposition sub-cycles typically begin by providing a precursor comprising niobium, followed by a nitrogen precursor. In some embodiments, one or more deposition sub-cycles begin by providing a nitrogen precursor, followed by a precursor comprising niobium. The deposition may be performed with the aid of a carrier gas such as nitrogen (N 2 ), Ar and / or He to provide one or more precursors for the niobium nitride sub-cycle. In some embodiments, the carrier gas may include another inert gas.
[0063] Figure 2 A flow chart of an example of a process 200 for forming a transition metal niobium nitride film on a substrate is shown. In some embodiments, the method is a thermal ALD process, while in other embodiments, the method is a plasma enhanced ALD process. The ALD process 200 may include a complete deposition cycle 203 with a transition metal nitride sub-cycle 204. Figure 2 As shown, the ALD process 200 may include a niobium nitride sub-cycle 206 for adding a niobium component to the growing transition metal niobium nitride film. In some embodiments, the transition metal nitride sub-cycle 204, the niobium nitride sub-cycle 206, and / or the full deposition cycle 203 may be repeated multiple times to form a transition metal niobium nitride film having a desired composition and / or thickness. The ratio of the transition metal nitride sub-cycle 204 to the niobium nitride sub-cycle 206 may be varied to adjust the concentration of niobium in the film and thereby obtain a film having desired properties. For example, the number of times the niobium nitride sub-cycle 206 is repeated relative to the number of times the transition metal sub-cycle 204 is repeated may be selected to provide a transition metal nitride film having desired properties (e.g., desired resistivity, density, and mechanical properties).
[0064] The transition metal nitride sub-cycle 204 may include blocks 208 and 210. In block 208, the substrate may be exposed to a first reactant that may include a transition metal precursor. In block 210, the substrate may be exposed to a third reactant that may include a nitrogen precursor. In some embodiments, the transition metal nitride sub-cycle 204 may be repeated multiple times (e.g., the number of repetitions of block 208 followed by 210). In some embodiments, block 208 or block 210 may be repeated multiple times before performing the other block one or more times. For example, block 208 may be repeated multiple times before performing block 210.
[0065] In some embodiments, the pulses of the transition metal precursor for exposing the substrate to the transition metal precursor and the pulses of the nitrogen precursor for exposing the substrate to the nitrogen precursor are separated by a step of removing excess transition metal precursor from a reactor (not shown). In some embodiments, excess nitrogen precursor is removed prior to repeating the transition metal nitride sub-cycle 204. In some embodiments, the transition metal nitride sub-cycle 204 is an ALD process. In some embodiments, the pulses of the transition metal and nitrogen precursors may at least partially overlap. In some embodiments, no additional precursors are provided to the reaction chamber between blocks 208 and 210, or prior to starting blocks 208 and 210.
[0066] The niobium nitride sub-cycle 206 for introducing the niobium component into the transition metal nitride film may include blocks 212 and 214. In block 212, the substrate may be exposed to a second precursor comprising niobium. In block 214, the substrate may be exposed to a nitrogen precursor. In some embodiments, the niobium nitride sub-cycle 206 may be repeated multiple times. In some embodiments, either block 212 or block 214 may be repeated multiple times before performing the other block one or more times. For example, block 212 may be repeated multiple times before performing block 214.
[0067] In some embodiments, excess nitrogen precursor is removed prior to repeating the niobium nitriding sub-cycle 206. In some embodiments, excess precursor comprising niobium from block 212 may be removed prior to exposing the substrate to the nitrogen precursor in block 214. In some embodiments, the niobium nitriding sub-cycle 206 is an ALD process. In some embodiments, pulses of the niobium-containing precursor and the nitrogen precursor may at least partially overlap. In some embodiments, no additional precursor is provided to the reaction chamber between blocks 212 and 214, or prior to starting blocks 212 and 214.
[0068] Once at least one transition metal nitride sub-cycle and at least one niobium nitride sub-cycle have been performed, the full deposition cycle 203 may be repeated 216 until a predetermined thickness of transition metal niobium nitride is reached 218. When the desired predetermined thickness of transition metal niobium nitride is reached, the full deposition cycle ends and the process may be exited 220.
[0069] In some embodiments, the transition metal nitride subcycle 204 may utilize a first reactant, and the first reactant may include a metal precursor, particularly a transition metal precursor. The transition metal precursor or compound may include at least one of the transition metals selected from the group consisting of scandium (Sc), yttrium (Y), titanium (Ti), zirconium (Zr), hafnium (Hf), vanadium (V), niobium (Nb), tantalum (Ta), chromium (Cr), molybdenum (Mo), tungsten (W), manganese (Mn), technetium (Tc), rhenium (Re), iron (Fe), ruthenium (Ru), osmium (Os), cobalt (Co), rhodium (Rh), iridium (Ir), nickel (Ni), palladium (Pd), platinum (Pt), copper (Cu), silver (Ag), gold (Au), zinc (Zn), cadmium (Cd), and mercury (Hg).
[0070] As a non-limiting example embodiment, a transition metal halide reactant, such as titanium tetrachloride (TiCl 4 ) can be used as a transition metal precursor in the ALD process described herein.
[0071] In some embodiments, the transition metal nitride sub-cycle 204 may utilize a third reactant, and the third reactant may include a nitrogen precursor. The method of embodiments of the present invention may include selecting the nitrogen precursor to include ammonia (NH 3 ), ammonium salts, hydrogen azide (HN 3 ), alkyl derivatives of hydrogen azide, hydrazine (N 2 H 4 ), hydrazine salts, alkyl derivatives of hydrazine (e.g., tert-butylhydrazine (C 4 H 9 N 2 H 3 ), methylhydrazine (CH 3 NHNH 2 ), dimethylhydrazine ((CH 3 ) 2 N 2 H 2 )), Nitrogen fluoride (NF 3 ) and nitrogen (N 2 ) of the plasma excitation material.
[0072] In some embodiments, the niobium nitride sub-cycle 206 may utilize a second reactant, and the second reactant may include a niobium precursor. The method of embodiments of the present invention may include selecting a niobium precursor to include niobium pentachloride (NbCl 5 ), niobium pentafluoride (NbF 5 ), niobium pentaboride (NbB 5 ), niobium pentaiodide (NbI 5 ) and niobium pentabromide (NbBr 5 ) at least one of.
[0073] In some embodiments, the niobium nitride sub-cycle 206 may utilize a third reactant, and the third reactant may include a nitrogen precursor. The method of embodiments of the present invention may include selecting the nitrogen precursor to include ammonia (NH 3 ), ammonium salts, hydrogen azide (HN 3 ), alkyl derivatives of hydrogen azide, hydrazine (N 2 H 4 ), hydrazine salts, alkyl derivatives of hydrazine, nitrogen fluoride (NF 3 ) and nitrogen (N 2 ) of the plasma excitation material.
[0074] In some embodiments, the ALD process of method 200 may include a plasma enhanced atomic layer deposition (PEALD) process. In such embodiments, the nitrogen precursor may include nitrogen (N 2 ) or any plasma excited species containing nitrogen reactants. In some embodiments, the plasma excited species may be added by adding additional plasma excited species, such as hydrogen (H 2 ) of the plasma excitation material, and the third reactant, such as nitrogen (N 2 ) of the plasma-excited species is supplied to the substrate.
[0075] In embodiments where the ALD process 200 includes a plasma enhanced atomic layer deposition method utilizing plasma excited species, the substrate temperature during deposition may include a temperature between about 250° C. and about 400° C. In embodiments where the ALD process 200 includes a thermal atomic layer deposition method (i.e., without the presence of plasma excited species), the substrate temperature during deposition may include a temperature between about 350° C. and about 450° C.
[0076] Usually expressed as The deposition rate of thin films using ALD with pulse cycles depends on many factors, including, for example, the number of reactive surface sites or active sites available on the surface and the bulkiness of the chemically adsorbed molecules. In some embodiments, the deposition rate of such films can be between about 0.3 and about In some embodiments, the deposition rate may be about 0.3, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, / Pulse cycle.
[0077] In some embodiments of the present disclosure, the ALD process described herein may be used to form a transition metal niobium nitride film on a substrate. The transition metal niobium nitride film may include at least one of the transition metals selected from the group consisting of scandium (Sc), yttrium (Y), titanium (Ti), zirconium (Zr), hafnium (Hf), vanadium (V), tantalum (Ta), chromium (Cr), molybdenum (Mo), tungsten (W), manganese (Mn), technetium (Tc), rhenium (Re), iron (Fe), ruthenium (Ru), cobalt (Co), rhodium (Rh), iridium (Ir), nickel (Ni), palladium (Pd), platinum (Pt), copper (Cu), silver (Ag), gold (Au), cadmium (Cd), and mercury (Hg). In some embodiments, the transition metal niobium nitride may include at least one of titanium niobium nitride, tantalum niobium nitride, and tungsten niobium nitride.
[0078] In a non-limiting exemplary embodiment of the present invention, the transition metal niobium nitride may include titanium niobium nitride. In some embodiments, the method may include forming the tin niobium nitride to have a Young's modulus greater than about 390 gigapascals. In some embodiments, the method may include forming the titanium niobium nitride to have a Young's modulus greater than about 5.4 g / cm 3 In some embodiments, a method may include forming the titanium niobium nitride to have a resistivity between about 200 μΩ-cm and about 1000 μΩ-cm.
[0079] In some embodiments of the present invention, the transition metal niobium nitride may include titanium niobium nitride and may have a deposited rms surface roughness (R a ), which is less than 8 angstroms, or less than 6 angstroms, or even less than 4 angstroms. It has been found that the surface roughness of the deposited transition metal niobium nitride can decrease as the niobium nitride content in the film decreases from 100%, so in some embodiments of the present invention, the method can involve reducing the surface roughness of the transition metal niobium nitride by reducing the niobium nitride content in the film. In some embodiments of the present invention, a minimum value of the surface roughness of the transition metal niobium nitride can be found for a niobium nitride sub-cycle percentage of 50%, which can correspond to a transition metal niobium nitride film having a surface roughness of less than 4 angstroms.
[0080] The transition metal niobium nitride films, such as titanium niobium nitride films, formed by the ALD process disclosed herein can be used in a variety of situations. In one non-limiting exemplary embodiment, the transition metal niobium nitride can be used to form a gate electrode structure. Those skilled in the art will recognize that the process described herein can be applied to many situations, including the manufacture of PMOS transistors including planar devices and multiple gate transistors such as FinFETs. In another non-limiting exemplary embodiment, the transition metal niobium nitride can be used as an electrode in a DRAM device structure. In another non-limiting exemplary embodiment, the transition metal niobium nitride can be used as a barrier material and / or capping layer in electrical interconnect applications.
[0081] As a non-limiting example, and with reference to Figure 3 , the semiconductor device structure 300 may include a semiconductor body 316 and an electrode 310 including a transition metal niobium nitride disposed on the semiconductor body 316. In more detail, the semiconductor device structure may include a transistor structure, and may also include a source region 302, a drain region 304, and a channel region 306 therebetween. The transistor gate structure 308 may include an electrode 310, i.e., a gate electrode, which may be separated from the channel region 306 by a gate dielectric 312. In accordance with the teachings of the present disclosure, the gate electrode 310 may include a transition metal niobium nitride film, such as titanium niobium nitride, formed by an atomic layer deposition process as described herein. Figure 3 As shown, in some embodiments, the transistor gate structure 308 may further include one or more additional conductive layers 314 formed on the gate electrode 310. The one or more additional conductive layers 314 may include at least one of polysilicon, refractory metal, transition metal carbide, and transition metal nitride.
[0082] In some embodiments, semiconductor device structure 300 may include a PMOS transistor, which may also include a transistor gate structure 308. PMOS transistor gate structure 308 may include a gate electrode 310 including a transition metal niobium nitride film and a gate dielectric 312 deposited between the transition metal nitride film and a semiconductor body 316.
[0083] In some embodiments, the gate electrode 310 may include a transition metal niobium nitride film, such as titanium niobium nitride, tantalum niobium nitride, and tungsten niobium nitride. As a non-limiting example of an embodiment of the present disclosure, the semiconductor device structure may include a silicon body 316, a hafnium oxide (2nm) gate dielectric 312, and one of titanium niobium nitride (niobium nitride sub-cycle percentage is 50%), niobium nitride, and titanium nitride as the gate electrode 310. The additional conductive layer deposited on the gate electrode 310 may include platinum. Table 1 below shows non-limiting example measured effective work functions for various thicknesses of the gate electrode 310. In some embodiments, the transistor gate structure 308 may include a titanium niobium nitride gate electrode, and the transistor gate structure may have an effective work function greater than about 4.6eV, or greater than 4.7eV, or even greater than 4.85eV.
[0084] Table 1
[0085]
[0086] It should be noted that embodiments of the present disclosure allow for the formation of a gate electrode structure comprising a thin metal niobium nitride film having an increased effective work function, for example, in some embodiments, a method may include forming a gate electrode structure comprising a transition metal niobium nitride gate electrode having a thickness of less than 100 angstroms and an effective work function greater than 4.85 eV. In other embodiments, a method may include forming a gate electrode structure comprising a transition metal niobium nitride gate electrode having a thickness of less than 30 angstroms and an effective work function greater than 4.6 eV.
[0087] As non-limiting examples, the transition metal niobium nitride film comprising gate electrode 310 may have a thickness of less than 50 angstroms in some embodiments, or less than 30 angstroms in some embodiments, or even less than 20 angstroms in some embodiments.
[0088] In some embodiments of the present disclosure, the gate electrode 310 may include a metal bilayer including a first metal layer of transition metal niobium nitride and a second metal layer deposited on the first metal layer at a selected MOS device location by patterning and etching steps, the second metal layer including, for example, a metal nitride. As a non-limiting example, the bilayer metal gate electrode 310 may include a titanium niobium nitride film having a thickness of 10-30 angstroms and an overlying adjacent titanium nitride film having a thickness of 10-30 angstroms. In some embodiments of the present disclosure, the transition metal niobium nitride film may be used as an etch stop to prevent over-etching and protect the underlying gate dielectric. Therefore, in some embodiments, the transition metal niobium nitride may have an etch selectivity, i.e., a relative etch rate of the overlying metal nitride film greater than 2:1, or greater than 5:1, or even greater than 10:1 compared to the transition metal niobium nitride film. For example, the bilayer metal gate electrode may be etched by a combination of wet etching chemistry (e.g., using hydrofluoric acid) and dry etching chemistry (using fluorine-based etching chemistry). In some embodiments of the present disclosure, it is found that the etching rate of transition metal niobium nitride increases with the decrease of niobium nitride content, so the etching selectivity of transition metal niobium nitride can be customized for specific applications by adjusting the composition of transition metal niobium nitride. In some embodiments of the present disclosure, the etching of the metal double-layer gate electrode can be performed so that the thickness of the overlying metal nitride and / or the thickness of the transition metal niobium nitride varies across the surface of the substrate (or integrated circuit). The thickness variation of the double-layer metal gate electrode produces a gate electrode with different effective work functions, and thus it is possible to produce multiple MOS devices with different threshold voltages in the integrated circuit, i.e., multiple V t MOS device.
[0089] As another non-limiting exemplary embodiment, transition metal niobium nitrides may be used as Figure 4 The electrodes in the DRAM device structure shown. In more detail, Figure 4 A semiconductor device structure 400 is shown including a semiconductor body 402 and an electrode 404 including a transition metal niobium nitride deposited on the semiconductor body.
[0090] Figure 4 A cross-sectional view of a partially fabricated DRAM device structure is shown and a process for forming such a DRAM device structure is described in U.S. Patent No. 7,910,452 to Roh et al. and is incorporated herein by reference. Figure 4, an insulating layer 406 may be formed on a semiconductor body 402 including a semi-finished substrate. A storage node contact hole is formed in the insulating layer 406, and a storage node contact plug 408 is formed in the storage node contact hole. The insulating layer 406 may include undoped silicate glass (USG) and may be formed to a thickness ranging from about 1000 angstroms to about 3000 angstroms. A patterned etch stop layer 410 may be formed on the insulating layer 406. The conductive layer for forming the storage node may include an electrode 404, and the electrode 404 may include a transition metal niobium nitride and may include a cylindrical storage node in structure. In some embodiments, the electrode 404 may include at least one of titanium niobium nitride, tantalum niobium nitride, and tungsten niobium nitride.
[0091] In a non-limiting exemplary embodiment of the present disclosure, the electrode 404 may include titanium niobium nitride. In some embodiments, the method may include forming the titanium niobium nitride to have a Young's modulus greater than about 390 gigapascals. In some embodiments, the method may include forming the titanium niobium nitride to have a Young's modulus greater than about 5.4 g / cm 3 In some embodiments, a method may include forming the titanium niobium nitride to have a resistivity of less than about 1000 μΩ-cm.
[0092] As another non-limiting exemplary embodiment, transition metal niobium nitrides may be used as barrier materials and / or capping layers in back-end-of-line (BEOL) metallization applications, such as Figure 5 In more detail, Figure 5A partially fabricated semiconductor device structure 500 is shown, comprising: a substrate 502, which may include a partially fabricated and / or fabricated semiconductor device structure, such as a transistor and a memory element (not shown). The partially fabricated semiconductor device structure 500 may include a dielectric material 504 formed on the substrate 502, which may include a low dielectric constant material, i.e., a low-k dielectric, such as a silicon-containing dielectric or a metal oxide. A trench may be formed in the dielectric material 504, and a barrier material 506 may be deposited on the surface of the trench, which prevents or substantially prevents metal interconnect material 508 from diffusing into the surrounding dielectric material 504. In some embodiments of the present disclosure, the barrier material 506 may include a transition metal niobium nitride, such as titanium niobium nitride. In some embodiments of the present disclosure, the transition metal niobium nitride may have a thickness of less than 35 angstroms, or 25 angstroms, or even 15 angstroms. Without being bound by any theory, it is believed that the transition metal niobium nitride barrier material may be able to prevent diffusion of metal interconnect material 508 at a significantly lower thickness than commonly used barrier materials currently used to fabricate integrated circuits. The partially fabricated semiconductor structure 500 may also include a metal interconnect material 508 for electrically interconnecting a plurality of device structures deposited in the substrate 502. In some embodiments, the metal interconnect material 508 may include one or more of copper or cobalt. In addition to using transition metal niobium nitride as a barrier material, the transition metal niobium nitride may also be used as a capping layer. Therefore, reference Figure 5 , the partially fabricated semiconductor device structure 500 may further include a capping layer 510 deposited directly on the upper surface of the metal interconnect material 508. The capping layer 510 may be used to prevent oxidation of the metal interconnect material 508, and importantly, to prevent diffusion of the metal interconnect material 508 in additional dielectric materials formed on the partially fabricated semiconductor structure 500 during subsequent fabrication processes (i.e., for multi-layer interconnect structures). In some embodiments of the present disclosure, the capping layer 510 may further include a transition metal niobium nitride, such as titanium niobium nitride having a thickness of less than 20 angstroms, or less than 15 angstroms, or even less than 10 angstroms. In some embodiments, the metal interconnect material 508, the barrier material 506, and the capping layer 510 may collectively form an electrode for electrical interconnection of multiple semiconductor devices deposited in the substrate 502.
[0093] Embodiments of the present disclosure may also include a reaction system configured to perform the method of the present disclosure. In more detail, Figure 6Schematically shows a reaction system 600 including a reaction chamber 602, which also includes a substrate (not shown) for maintaining a predetermined pressure, temperature and environmental conditions, and for selectively exposing the substrate to various gas mechanisms. Precursor source 604 can be coupled to reaction chamber 602 by pipeline or other suitable device 604A, and can also be coupled to manifold, valve control system, mass flow control system, or mechanism to control the gaseous precursor derived from precursor source 604. Precursors (not shown) and reactants (not shown) supplied by precursor source 604 can be liquid or solid under room temperature and standard atmospheric pressure conditions. Such a precursor can evaporate in a reactant source vacuum container, and the reactant source vacuum container can be maintained at an evaporation temperature equal to or higher than that in the precursor source chamber. In such an embodiment, the evaporated precursor can be transported with a carrier gas (e.g., inactive or inert gas), and then fed into reaction chamber 602 by conduit 604A. In other embodiments, under standard conditions, the precursor can be a vapor. In such an embodiment, the precursor does not need to evaporate and may not need a carrier gas. For example, in one embodiment, the precursors may be stored in gas cylinders.Reaction system 600 may also include additional precursor reactant sources, which may also be coupled to the reaction chamber via conduits 606A and 608A, respectively, as described above.
[0094] Purge gas source 610 may also be coupled to reaction chamber 602 via conduit 610A and selectively supply various inert or noble gases to reaction chamber 602 to assist in removing precursor gases or exhaust gases from the reaction chamber. The various inert or noble gases that may be provided may be derived from solid, liquid or stored gaseous forms.
[0095] Figure 6 The reaction system 600 may also include a system operation and control mechanism 612, which provides electronic circuits and mechanical components to selectively operate valves, manifolds, pumps and other equipment included in the reaction system 600. Such circuits and components operate to introduce precursors, purge gases from corresponding precursor sources 604, 606, 608 and purge gas sources 610. The system operation and control mechanism 612 also controls the timing of gas pulse sequences, the temperature of substrates and reaction chambers, and the pressure of reaction chambers and various other operations required for the proper operation of the reaction system 400. The operation and control mechanism 612 may include control software and electric or pneumatically controlled valves to control the flow of precursors, reactants and purge gases entering and leaving the reaction chamber 602. The control system may include modules such as software or hardware components, for example, FPGAs or ASICs, which perform certain tasks. The modules can be advantageously arranged to reside on an addressable storage medium of the control system and be arranged to perform one or more processes.
[0096] In some embodiments, Figure 6The reaction system 600 may include a plasma enhanced atomic layer deposition system, and may also include a plasma generation component, which in some embodiments may be "local", i.e., an integral part of the reaction chamber 602, or in some embodiments may be "remote", i.e., the plasma and associated plasma-excited species are generated remotely from the reaction chamber and subsequently fed to the reaction chamber using a suitable conduit.
[0097] Those skilled in the relevant art will recognize that other configurations of the reaction system of the present invention are possible, including precursor reactant sources and purge gas sources of different numbers and types. In addition, such persons will also appreciate that there are many arrangements of valves, pipelines, precursor sources, and purge gas sources for achieving the purpose of selectively feeding gases into the reaction chamber 602. In addition, as a schematic diagram of the reaction system, many components have been omitted for simplicity of description, and these components may include, for example, various valves, manifolds, purifiers, heaters, containers, vents, and / or bypasses.
[0098] The exemplary embodiments of the above disclosure do not limit the scope of the present invention, as these embodiments are merely examples of embodiments of the present invention as defined by the appended claims and their legal equivalents. Any equivalent embodiments are intended to be within the scope of the present invention. In fact, various modifications of the present disclosure, such as alternative useful combinations of the described parts, in addition to those shown and described herein, may become apparent to those skilled in the art from the description. These modifications and variations are also within the scope of the appended claims.
Claims
1. A method for forming a transition metal niobium nitride film on a substrate by atomic layer deposition, the method include: A transition metal nitride sub-cycle, the transition metal nitride sub-cycle comprising: contacting the substrate with a first reactant comprising a transition metal halide precursor; and contacting the substrate with a third reactant, the third reactant comprising a nitrogen precursor, A niobium nitride subcycle, wherein the niobium nitride subcycle comprises: contacting the substrate with a second reactant comprising a niobium precursor to form a mixture of a transition metal species and a niobium species; and contacting the substrate with a third reactant comprising a nitrogen precursor, To form transition metal niobium nitride, The ratio of the transition metal nitride sub-cycle to the niobium nitride sub-cycle is varied to adjust the niobium concentration in the film.
2. The method of claim 1, wherein the method comprises performing at least one deposition cycle wherein the substrate is contacted sequentially with the first reactant, the third reactant, the second reactant, and the third reactant. The method of claim 2 , wherein the deposition cycle is repeated 2 or more times.
4. The method of claim 1, wherein the transition metal halide comprises at least one of a transition metal selected from the group consisting of scandium (Sc), yttrium (Y), titanium (Ti), zirconium (Zr), hafnium (Hf), vanadium (V), tantalum (Ta), chromium (Cr), molybdenum (Mo), tungsten (W), manganese (Mn), technetium (Tc), rhenium (Re), iron (Fe), ruthenium (Ru), osmium (Os), cobalt (Co), rhodium (Rh), iridium (Ir), nickel (Ni), palladium (Pd), platinum (Pt), copper (Cu), silver (Ag), gold (Au), zinc (Zn), cadmium (Cd), and mercury (Hg).
5. The method of claim 1, wherein the second reactant is selected from the group consisting of niobium pentafluoride (NbF 5 ), niobium pentaboride (NbB 5 ), niobium pentaiodide (NbI 5 ) and niobium pentabromide (NbBr 5 ).
6. The method of claim 1, further comprising selecting the transition metal precursor to include at least one of a titanium precursor, a tantalum precursor, and a tungsten precursor.
7. The method of claim 6, further comprising selecting the titanium precursor to comprise a titanium halide.
8. The method of claim 7 further comprising selecting the titanium halide to include titanium tetrachloride (TiCl 4 ).
9. The method of claim 1 further comprising selecting the niobium precursor to include niobium pentachloride (NbCl 5 ), niobium pentafluoride (NbF 5 ), niobium pentaboride (NbB 5 ), niobium pentaiodide (NbI 5 ) and niobium pentabromide (NbBr 5 ) at least one of.
10. The method of claim 1, further comprising selecting the nitrogen precursor to include ammonia (NH 3 ), ammonium salts, hydrogen azide (HN 3 ), alkyl derivatives of hydrogen azide, hydrazine (N 2 H 4 ), hydrazine salts, alkyl derivatives of hydrazine, nitrogen fluoride (NF 3 ) and nitrogen (N 2 ) of the plasma excitation material.
11. The method of claim 1, wherein contacting the substrate with the third reactant further comprises contacting the substrate with hydrogen (H 2 ) of plasma-excited matter.
12. The method of claim 1, wherein the method is a plasma enhanced atomic layer deposition process.
13. The method of claim 1, further comprising heating the substrate to a temperature between 250°C and 450°C.
14. The method of claim 1 further comprising forming the transition metal niobium nitride to have a Young's modulus greater than 390 GPa.
15. The method of claim 1, further comprising: include: removing any unreacted first reactant, Wherein the step of contacting the substrate with a third reactant is performed after removing any unreacted first reactant.
16. The method of claim 1, wherein contacting the substrate with a first reactant comprises flowing the first reactant for a first reactant pulse period, wherein contacting the substrate with a third reactant comprises flowing the third reactant for a third reactant pulse period, wherein the first reactant pulse period at least partially overlaps with the third reactant pulse period.
17. The method of claim 1, further comprising forming a gate electrode structure comprising the transition metal niobium nitride.
18. The method of claim 17, wherein the gate electrode structure has an effective work function greater than 4.6 eV.
19. The method of claim 1 further comprising forming a dynamic random access memory (DRAM) capacitor comprising the transition metal niobium nitride.
20. The method of claim 1, further comprising forming a barrier material comprising the transition metal niobium nitride.
21. The method of claim 1, further comprising forming a capping layer comprising the transition metal niobium nitride.
22. The method of claim 1, wherein forming the transition metal niobium nitride further comprises forming a nanolaminated structure comprising a transition metal nitride layer and a niobium nitride-containing layer.
23. The method of claim 1, wherein the ratio of the etch rate of the capping metal nitride film to the etch rate of the transition metal niobium nitride film is greater than 10:
1.
24. The method of claim 1, wherein the transition metal niobium nitride has an rms surface roughness (R a ).
25. A reaction system configured to carry out the method of claim 1.