A high performance rare earth permanent magnetic material with a composite hard magnetic shell structure and a preparation method thereof
By forming a multilayer heavy rare earth-rich hard magnetic shell in sintered NdFeB magnets, the problem of insufficient coercivity was solved, and high-performance rare earth permanent magnet materials with high coercivity and high magnetic energy product were realized.
Patent Information
- Application Number
- CN202210392117.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-14
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-04-14
AI Technical Summary
The low coercivity of existing sintered NdFeB magnets limits their application in high-temperature fields, and the addition of heavy rare earth elements Dy/Tb reduces the magnetic energy product and remanence.
By employing a multi-phase alloying process and a grain boundary diffusion process, a multilayer heavy rare earth-rich hard magnetic shell is formed on the epitaxial layer of the main phase grains. A heavy rare earth alloy thin film is deposited by magnetron sputtering and subjected to grain boundary diffusion and low-temperature tempering heat treatment to form a continuous rare earth-rich grain boundary phase, which isolates the short-range magnetic exchange effect of adjacent main phase grains.
It significantly improves the coercivity of the magnet while maintaining high remanence, achieving a balance between high coercivity and high magnetic energy product, and avoiding the waste of heavy rare earth elements and magnetic dilution effect.
Abstract
Description
Technical Field
[0001] The invention relates to the field of rare earth permanent magnets, and in particular to a high-performance rare earth permanent magnet material with a composite hard magnetic shell structure and a preparation method thereof. Background Art
[0002] The third generation of rare earth permanent magnet NdFeB has a high magnetic energy product that other permanent magnet materials cannot match, which is particularly conducive to the miniaturization, lightness and thinness of instruments and equipment. It is widely used in energy, transportation, information, medical treatment and national defense, and has developed into an indispensable strategic functional material in various fields of modern military and civilian. In particular, sintered NdFeB materials have been developed for more than 30 years, and the magnet performance has been continuously improved. The maximum magnetic energy product (BH) max and remanence B r The experimental values are close to the theoretical values. However, the coercivity H of sintered NdFeB materials cj It is still relatively low, only 1 / 5 to 1 / 3 of the theoretical value, which greatly limits the application of sintered NdFeB materials in high-temperature fields.
[0003] Adding heavy rare earth elements Dy / Tb to partially replace Nd is currently the most common way to increase the coercivity of sintered NdFeB magnets. However, heavy rare earth atoms such as Dy / Tb and Fe atoms are antiferromagnetically coupled, resulting in excessive addition of Dy / Tb to rare earth permanent magnets, which will seriously reduce the maximum magnetic energy product and remanence of the magnet. It is generally believed that the coercivity of sintered NdFeB magnets is determined by the reverse magnetization domain nucleation mechanism, and its theoretical limit is the intrinsic magnetocrystalline anisotropy field H of the ferromagnetic main phase of 2:14:1. A Its actual value is closely related to the composition / defects of the epitaxial layer of the main phase grains and the distribution of the Nd-rich phase between the main phase grains. In actual magnets, the main phase grain epitaxial layer usually has a lower magnetocrystalline anisotropy field H due to the deviation of the composition of the main phase grain epitaxial layer from the positive stoichiometric ratio and structural defects. A , which can easily become the nucleation site for the reverse magnetization domain.
[0004] In order to improve the utilization efficiency of heavy rare earth Dy / Tb and avoid the antiferromagnetic coupling between Dy / Tb atoms and Fe atoms, it is an effective way to form a heavy rare earth-rich magnetic hard shell layer in the epitaxial layer of the main phase grains. The coercivity of sintered rare earth magnets is not only related to the intrinsic magnetocrystalline anisotropy field, but also closely related to the distribution of rare earth-rich grain boundary phases. Optimizing the wettability between the main phase and the rare earth-rich grain boundary phase, forming a continuous grain boundary phase in the magnet, and isolating the short-range magnetic exchange coupling between adjacent main phase grains is also an important way to improve the coercivity of the magnet. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a high-performance rare earth permanent magnet material with a composite magnetic hard shell structure and a preparation method thereof, which fully utilizes the multi-main phase alloy process and the grain boundary diffusion process to form a multi-layer heavy rare earth-rich hard magnetic shell layer in the main phase grain epitaxial layer, form a continuous rare earth-rich grain boundary phase, greatly improve the coercive force of the magnet while maintaining the high remanence of the magnet, and prepare a high-performance rare earth permanent magnet material integrating high coercive force and high magnetic energy product.
[0006] One of the purposes of the present invention is to provide a method for preparing a high-performance rare earth permanent magnet material with a composite hard magnetic shell structure. First, a main phase alloy I without heavy rare earth and one or more main phase alloys II with heavy rare earth added are used to prepare a multi-main phase magnet with a heavy rare earth-rich hard magnetic shell; then a heavy rare earth alloy film is deposited on the surface of the multi-main phase magnet by magnetron sputtering, and a new hard magnetic shell with a higher heavy rare earth content is formed on the surface of the main phase grains through grain boundary diffusion and low-temperature tempering heat treatment.
[0007] Among them, the main phase alloy I without heavy rare earth has a composition of RE in mass percentage. x1 Q bal M y1 B z1 , RE is one or more of the other lanthanide rare earth elements except the heavy rare earth elements Dy and Tb, Q is one or more of the elements Fe, Co, and Ni, M is one or more of the elements Al, Cr, Cu, Ga, Mn, Mo, N, Nb, P, Pb, Si, Ta, Ti, V, and Zr, B is boron, and x1, y1, and z1 satisfy the following relationship: 27≤x1≤36, 0≤y1≤3, and 0.8≤z1≤1.2;
[0008] Among them, the main phase alloy II with heavy rare earth added has the following composition by mass percentage: w HRE 1-w ) x2 Q bal M y2 B z2 , RE is one or more of the other lanthanide rare earth elements except the heavy rare earth elements Dy and Tb, HRE is one or two of the heavy rare earth elements Dy and Tb, Q is one or more of the elements Fe, Co, and Ni, M is one or more of the elements Al, Cr, Cu, Ga, Mn, Mo, N, Nb, P, Pb, Si, Ta, Ti, V, and Zr, B is boron, and x2, y2, z2, and w satisfy the following relationship: 0.2≤w≤0.8, 26≤x2≤35, 0≤y2≤3, and 0.85≤z2≤1.15;
[0009] Among them, the heavy rare earth alloy film is composed of HRE in terms of mass percentage. a RE b Qbal N c , HRE is one or two of the heavy rare earth elements Dy and Tb, RE is one or more of the other lanthanide rare earth elements except the heavy rare earth elements Dy and Tb, Q is one or more of the elements Fe, Co, and Ni, N is one or more of the elements Al, Cu, Ga, Zn, Mn, and Mg, and a, b, and c satisfy the following relationship: 20≤a≤70, 2≤b≤15, and 0≤c≤10.
[0010] Preferably: specifically comprising the following steps:
[0011] 1) According to the composition of main phase alloy I without heavy rare earth and main phase alloy II with heavy rare earth, the ingredients are prepared respectively, and the vacuum degree is ≤10 -2 Different main phase alloys were melted in a vacuum medium frequency induction furnace at 10000 Pa, and main phase alloy flakes with a thickness of 0.2-0.6 mm were obtained by rapid solidification casting technology. Main phase alloy I and main phase alloy II powders with an average particle size of 2-4 μm were prepared by hydrogen crushing and air flow grinding.
[0012] 2) Under nitrogen or argon protection, the main phase alloy I and the main phase alloy II powders with different compositions are uniformly mixed according to a proportion to obtain mixed main phase powders with different heavy rare earth addition amounts;
[0013] 3) Orienting and pressing the obtained mixed main phase powder in a 1.5-2.0T magnetic field to obtain a green body;
[0014] 4) After vacuum packaging the obtained green body, cold isostatic pressing is performed at 150-250 MPa, and then sintering is performed in a high vacuum positive pressure sintering furnace to obtain a sintered magnet;
[0015] 5) Pre-treating the surface of the obtained sintered magnet to ensure that the surface roughness Ra of the magnet is less than or equal to 0.1 μm and the surface is free of oil stains;
[0016] 6) Activate the target and evacuate to 1×10 -3 ~1×10 -4 Pa, and then high-purity argon gas was introduced to adjust the vacuum degree to 1.5×10 -2 ~1.0Pa, adjust the target power to 60~140W, the bias voltage to 70~130V, and the working time to 5~15min; then turn on the DC power supply, bombard the target surface for 5~15min to remove the oxide layer on the target surface;
[0017] 7) performing magnetron sputtering on the surface of the magnet treated in step 5) to deposit a heavy rare earth alloy film, introducing high-purity argon gas, with a gas flow rate of 15 to 60 sccm, a sputtering power of 60 to 220 W, and a sputtering time of 0.5 to 6 hours, and controlling the thickness of the deposited heavy rare earth alloy film to be 1 to 30 μm;
[0018] 8) The deposited magnet is subjected to grain boundary diffusion treatment and low temperature tempering heat treatment in a high vacuum annealing furnace to obtain a high performance rare earth permanent magnet material with a composite hard magnetic shell structure.
[0019] Preferably, in step 8), the grain boundary diffusion treatment system is: performing grain boundary diffusion in the range of 650 to 1000° C. for 0.5 to 12 h, and the low-temperature tempering heat treatment system is: performing heat treatment in the range of 420 to 650° C. for 2 to 5 h.
[0020] The second object of the present invention is to provide a high-performance rare earth permanent magnet material with a composite hard magnetic shell structure, which is prepared using the above-mentioned preparation method.
[0021] Preferably: the final magnet main phase crystal grain epitaxial layer has multiple layers of heavy rare earth-rich hard magnetic shells, including two or more low heavy rare earth content n1 main phase crystal grain cores and high heavy rare earth content n2 main phase crystal grain cores, as well as high heavy rare earth content n3 main phase crystal grain hard magnetic shells, and the outermost layer of higher heavy rare earth content n4 main phase crystal grain hard magnetic shells. Where n1<n3<n2 and n1<n3<n4, the coercive force of the magnet is improved and the remanence of the magnet is maintained.
[0022] Preferably, the final magnet has a continuous rare earth-rich grain boundary phase, which effectively isolates the short-range magnetic exchange between adjacent grains and improves the coercive force of the magnet.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] 1) The present invention synergistically innovates multi-main phase alloy technology and grain boundary diffusion technology, innovatively designs the composition of multi-main phase alloy and grain boundary diffusion alloy, and the main phase grain epitaxial layer of the magnet has a multi-layer heavy rare earth-rich hard magnetic shell layer, which can effectively improve the nucleation field of the anti-magnetization domain in the magnet, inhibit the nucleation of the anti-magnetization domain, and thus improve the coercive force of the magnet.
[0025] 2) The diffusion source designed in the grain boundary diffusion technology is a heavy rare earth alloy HRE a RE b Q bal N c , optimize the design of the ratio of heavy rare earth and other rare earths, optimize the design of the ratio of 3d transition metals Fe / Co / Ni and other alloy elements, regulate the physical and chemical properties and diffusion efficiency of the diffusion source, control the composition and distribution of the new hard magnetic shell, and control the thickness of the deposited heavy rare earth alloy film to 1-30μm, effectively improve the utilization efficiency of heavy rare earth elements, and do not introduce too many non-magnetic elements to cause magnetic dilution effect, and form a continuous grain boundary phase after grain boundary diffusion and heat treatment, isolating the short-range magnetic exchange effect of adjacent main phase grains, which can greatly improve the coercive force of the magnet while maintaining its remanence.
[0026] 3) Compared with the existing magnets with a single hard magnetic shell, the rare earth permanent magnet material with a composite hard magnetic shell structure provided by the present invention has a more reasonable distribution of heavy rare earth, which contributes more to improving the coercive force of the magnet and can also maintain the remanence of the magnet.
[0027] 4) The present invention utilizes magnetron sputtering technology to deposit a heavy rare earth alloy film, which has a strong bonding force with the substrate, is uniform and dense, and promotes the grain boundary diffusion process; the magnetron sputtering technology can accurately control the thickness of the film, and use it as a diffusion source, and can accurately control the number of diffusion sources, avoiding waste caused by excessive enrichment of heavy rare earth elements on the magnet surface. DETAILED DESCRIPTION
[0028] The present invention is further described below in conjunction with specific embodiments, but the present invention is not limited to the following embodiments:
[0029] Embodiment 1:
[0030] 1) The main phase components are prepared according to the designed main phase components. In terms of mass percentage, the main phase alloy I without heavy rare earth is composed of (Pr 0.2 Nd 0.8 ) 32.0 Fe bal Co 0.5 Nb 0.2 Ga 0.3 Al 0.3 Cu 0.2 B 1.05 The main phase alloy II with heavy rare earth addition has a composition of [(Pr 0.2 Nd 0.8 ) 0.25 Dy 0.75 ] 32.0 Fe bal Co 0.5 Nb 0.2 Ga 0.3 Al 0.3 Cu 0.2 B 1.05 , at vacuum degree ≤10 -2 The main phase alloy I and the main phase alloy II were melted in a vacuum medium frequency induction furnace at 1000 Pa, and the main phase alloy flakes with a thickness of 0.35 mm were obtained by rapid solidification casting technology. The main phase alloy I and the main phase alloy II powders with an average particle size of 3.3 μm were prepared by hydrogen crushing and air flow grinding.
[0031] 2) Under nitrogen protection, the main phase alloy I and the main phase alloy II powders with different compositions were uniformly mixed in a mass ratio of 23:1 to obtain a main phase alloy having a composition of (Pr 0.2 Nd 0.8 ) 31.0 Dy 1.0 Fe bal Co0.5 Nb 0.2 Ga 0.3 Al 0.3 Cu 0.2 B 1.05 A mixed main phase powder;
[0032] 3) Orienting and pressing the obtained mixed main phase powder in a magnetic field of 1.8 T to obtain a green body;
[0033] 4) After vacuum packaging, the green body is cold isostatically pressed at 200 MPa, and then sintered in a high vacuum positive pressure sintering furnace at a sintering temperature of 1065°C for 3 hours to obtain a sintered magnet;
[0034] 5) Pre-treating the surface of the obtained sintered magnet to ensure that the surface roughness Ra of the magnet is less than or equal to 0.1 μm and the surface is free of oil stains;
[0035] 6) In terms of mass percentage, the target material composition is Dy 60 Pr 10 Fe 30 , activate the target and evacuate to 2×10 -4 Pa, and then high-purity argon was introduced to adjust the vacuum degree to 4×10 -2 Pa, adjust the target power to 110W, bias voltage to 110V, and working time to 5min; then turn on the DC power supply and bombard the target surface for 5min to remove the oxide layer on the target surface;
[0036] 7) performing magnetron sputtering on the surface of the magnet treated in step 5) to deposit a heavy rare earth alloy film, introducing high-purity argon gas, with a gas flow rate of 30 sccm, a sputtering power of 100 W, and a sputtering time of 1 h, and controlling the thickness of the deposited rare earth alloy film to be 4 μm;
[0037] 8) The deposited magnet is subjected to a 900°C grain boundary diffusion treatment for 6 hours and a 500°C low temperature tempering heat treatment for 4 hours in a high vacuum annealing furnace to obtain a high performance rare earth permanent magnet material with a composite hard magnetic shell structure.
[0038] The EPMA element surface distribution results show that there is a composite hard magnetic shell structure in the epitaxial layer of the main phase grains of the magnet, namely the Dy-rich hard magnetic shell introduced by the multi-main phase technology and the outermost Dy-rich hard magnetic shell introduced by the grain boundary diffusion technology; the test results of the AMT-4 permanent magnet characteristic measuring instrument show that the magnetic properties of the magnet are B r =13.7kG, H cj =28.1kOe, (BH) max =47.1MGOe.
[0039] Comparative Example 1:
[0040] The difference from Example 1 is that the magnet is not subjected to magnetron sputtering. The EPMA element surface distribution results show that there is only a single-layer Dy-rich hard magnetic shell structure in the epitaxial layer of the main phase grain of the magnet; the test results of the AMT-4 permanent magnet property measuring instrument show that the magnetic properties of the magnet are B r =13.7kG, H cj =20.5kOe, (BH) max =45.9MGOe.
[0041] Embodiment 2:
[0042] 1) The main phase components are prepared according to the designed main phase components. In terms of mass percentage, the main phase alloy I without heavy rare earth is composed of (Pr 0.1 Nd 0.85 Ho 0.05 ) 32.0 Fe bal Co 0.3 Zr 0.2 Ga 0.3 Al 0.35 Cu 0.15 B 1.02 The main phase alloy II with heavy rare earth addition has a composition of [(Pr 0.1 Nd 0.85 Ho 0.05 ) 0.25 Dy 0.75 ] 32.0 Fe bal Co 0.3 Zr 0.2 Ga 0.3 Al 0.35 Cu 0.15 B 1.02 , at vacuum degree ≤10 - 2 The main phase alloy I and the main phase alloy II were melted in a vacuum medium frequency induction furnace at 1000 Pa, and the main phase alloy flakes with a thickness of 0.35 mm were obtained by rapid solidification casting technology. The main phase alloy I and the main phase alloy II powders with an average particle size of 3.3 μm were prepared by hydrogen crushing and air flow grinding.
[0043] 2) Under argon protection, the main phase alloy I and the main phase alloy II powders with different compositions were uniformly mixed in a mass ratio of 11:1 to obtain a main phase alloy having a composition of (Pr 0.2 Nd 0.75 Ho 0.05 ) 31.0 Dy 2.0 Fe bal Co 0.3 Zr 0.2 Ga 0.3 Al 0.35 Cu 0.15 B1.02 A mixed main phase powder;
[0044] 3) Orienting and pressing the obtained mixed main phase powder in a magnetic field of 1.8 T to obtain a green body;
[0045] 4) After vacuum packaging, the green body is cold isostatically pressed at 180 MPa, and then sintered in a high vacuum positive pressure sintering furnace at a sintering temperature of 1070°C for 3 hours to obtain a sintered magnet;
[0046] 5) performing surface pretreatment on the magnet obtained in step 4) so that the surface roughness of the magnet Ra is less than or equal to 0.1 μm and the surface is free of oil stains;
[0047] 6) In terms of mass percentage, the target material composition is Tb 70 Pr5Fe 15 Al 10 , activate the target material and evacuate it to 1×10 -4 Pa, and then high-purity argon gas was introduced to adjust the vacuum degree to 1.5×10 -2 Pa, adjust the target power to 120W, bias voltage to 120V, and working time to 8min; then turn on the DC power supply and bombard the target surface for 15min to remove the oxide layer on the target surface;
[0048] 7) performing magnetron sputtering on the surface of the magnet treated in step 5) to deposit a heavy rare earth alloy film, introducing high-purity argon gas at a pressure of 25 sccm, a sputtering power of 110 W, and a sputtering time of 3.5 h, and controlling the thickness of the deposited rare earth alloy film to be 15 μm;
[0049] 8) The deposited magnet is subjected to a grain boundary diffusion treatment at 890°C for 9 hours and a low temperature tempering heat treatment at 480°C for 3 hours in a high vacuum annealing furnace to obtain a high performance rare earth permanent magnet material with a composite hard magnetic shell structure.
[0050] The EPMA element surface distribution results show that there is a composite hard magnetic shell structure in the epitaxial layer of the main phase grains of the magnet, namely the Dy-rich hard magnetic shell introduced by the multi-main phase technology, and the outermost Tb-rich hard magnetic shell introduced by the grain boundary diffusion technology; the test results of the AMT-4 permanent magnet property measuring instrument show that the magnetic properties of the magnet are B r =13.4kG, H cj =35.5kOe, (BH) max =44.6MGOe.
[0051] Comparative Example 2:
[0052] The difference from Example 2 is that the magnet is not subjected to magnetron sputtering. The EPMA element surface distribution results show that there is only a single-layer Dy-rich hard magnetic shell structure in the epitaxial layer of the main phase grain of the magnet; the test results of the AMT-4 permanent magnet property measuring instrument show that the magnetic properties of the magnet are B r =13.5kG, H cj =23.8kOe, (BH) max =43.9MGOe.
[0053] Embodiment 3:
[0054] 1) The main phase components are prepared according to the designed main phase components. In terms of mass percentage, the main phase alloy I component without heavy rare earth is Nd 30.0 Fe bal Co 0.3 Nb 0.2 Ta 0.05 Ti 0.1 Al 0.25 Cu 0.2 Ga 0.1 B 1.0 The main phase alloy II with heavy rare earth addition has the composition of (Nd 0.5 Dy 0.5 ) 30.0 Fe bal Co 0.3 Nb 0.2 Ta 0.05 Ti 0.1 Al 0.25 Cu 0.2 Ga 0.1 B 1.0 , at vacuum degree ≤10 -2 The main phase alloy I and the main phase alloy II were melted in a vacuum medium frequency induction furnace at 1000 Pa, and the main phase alloy flakes with a thickness of 0.28 mm were obtained by rapid solidification casting technology. The main phase alloy I and the main phase alloy II powders with an average particle size of 3.0 μm were prepared by hydrogen crushing and air flow grinding processes;
[0055] 2) Under nitrogen protection, the main phase alloy I and the main phase alloy II powders were uniformly mixed in a mass ratio of 9:1 to obtain a Nd 28.5 Dy 1.5 Fe bal Co 0.3 Nb 0.2 Ta 0.05 Ti 0.1 Al 0.25 Cu 0.2 Ga 0.1 B 1.0 A mixed main phase powder;
[0056] 3) Orienting and pressing the obtained mixed main phase powder in a magnetic field of ~1.6T to obtain a green body;
[0057] 4) After vacuum packaging, the green body is cold isostatically pressed at 190 MPa, and then sintered in a high vacuum positive pressure sintering furnace at a sintering temperature of 1075°C for 3 hours to obtain a sintered magnet;
[0058] 5) performing surface pretreatment on the magnet obtained in step 4) so that the surface roughness of the magnet Ra is less than or equal to 0.1 μm and the surface is free of oil stains;
[0059] 6) In terms of mass percentage, the target material composition is Dy 30 Tb 50 Pr2Fe 10 Ga8, the target material is activated and first vacuumed to 8×10 -4 Pa, and then high-purity argon gas was introduced to adjust the vacuum degree to 8×10 -2 Pa, adjust the target power to 100W, bias voltage to 100V, and working time to 6min; then turn on the DC power supply and bombard the target surface for 6min to remove the oxide layer on the target surface;
[0060] 7) performing magnetron sputtering on the surface of the magnet after the treatment in step 5) to deposit a heavy rare earth alloy film, introducing high-purity argon gas, with a gas flow rate of 20 sccm, a sputtering power of 95 W, and a sputtering time of 3 h, and controlling the thickness of the deposited rare earth alloy film to be ~10 μm;
[0061] 8) The deposited magnet is subjected to a grain boundary diffusion treatment at 850°C for 9 hours and a low temperature tempering heat treatment at 480°C for 4 hours in a high vacuum annealing furnace to obtain a high performance rare earth permanent magnet material with a composite hard magnetic shell structure.
[0062] The EPMA element surface distribution results show that there is a composite hard magnetic shell structure in the epitaxial layer of the main phase grains of the magnet, namely the Dy-rich hard magnetic shell introduced by the multi-main phase technology, and the outermost Dy / Tb-rich hard magnetic shell introduced by the grain boundary diffusion technology; the test results of the AMT-4 permanent magnet characteristic measuring instrument show that the magnetic properties of the magnet are B r =13.6kG, H cj =30.1kOe, (BH) max =46.0MGOe.
[0063] Comparative Example 3:
[0064] The difference from Example 3 is that the magnet is not subjected to magnetron sputtering. The EPMA element surface distribution results show that there is only a single-layer Dy-rich hard magnetic shell structure in the epitaxial layer of the main phase grain of the magnet; the test results of the AMT-4 permanent magnet property measuring instrument show that the magnetic properties of the magnet are B r =13.6kG, Hcj =22.5kOe, (BH) max =44.7MGOe.
[0065] Embodiment 4:
[0066] 1) The main phase components are prepared according to the designed main phase components. In terms of mass percentage, the main phase alloy I without heavy rare earth is composed of (Pr 0.2 Nd 0.8 ) 31.0 Fe bal Co 0.3 Zr 0.2 Ga 0.5 Al 0.1 Cu 0.2 B 0.95 The main phase alloy II with heavy rare earth addition has a composition of [(Pr 0.2 Nd 0.8 ) 0.4 Tb 0.6 ] 31.0 Fe bal Co 0.3 Zr 0.2 Ga 0.5 Al 0.1 Cu 0.2 B 0.95 , at vacuum degree ≤10 -2 The main phase alloy I and the main phase alloy II were melted in a vacuum medium frequency induction furnace at 1000 Pa, and the main phase alloy flakes with a thickness of 0.30 mm were obtained by rapid solidification casting technology. The main phase alloy I and the main phase alloy II powders with an average particle size of 3.1 μm were prepared by hydrogen crushing and air flow grinding.
[0067] 2) Under argon protection, the main phase alloy I and the main phase alloy II powders with different compositions were uniformly mixed in a mass ratio of 5:1 to obtain a main phase alloy having a composition of (Pr 0.2 Nd 0.8 ) 27.9 Tb 3.1 Fe bal Co 0.3 Zr 0.2 Ga 0.5 Al 0.1 Cu 0.2 B 0.95 A mixed main phase powder;
[0068] 3) Orienting and pressing the obtained mixed main phase powder in a magnetic field of 2.0 T to obtain a green body;
[0069] 4) After vacuum packaging, the obtained green body is subjected to cold isostatic pressing at 200 MPa, and then sintered in a high vacuum positive pressure sintering furnace at a sintering temperature of 1070°C and a sintering time of 3.5 hours to obtain a sintered magnet;
[0070] 5) performing surface pretreatment on the magnet obtained in step 4) so that the surface roughness of the magnet Ra is less than or equal to 0.1 μm and the surface is free of oil stains;
[0071] 6) In terms of mass percentage, the target material composition is Dy 10 Tb 60 Ce5Al5Cu5Fe 15 , the target material is activated by first evacuating the vacuum to 1×10 -3 Pa, and then high-purity argon gas was introduced to adjust the vacuum degree to 2×10 -2 Pa, adjust the target power to 100W, bias voltage to 100V, and working time to 8min; then turn on the DC power supply and bombard the target surface for 10min to remove the oxide layer on the target surface;
[0072] 7) performing magnetron sputtering on the surface of the magnet after the treatment in step 5) to deposit a heavy rare earth alloy film, introducing high-purity argon gas with a gas flow rate of 35 sccm, a sputtering power of 120 W, and a sputtering time of 4 h, and controlling the thickness of the deposited rare earth alloy film to be ~20 μm;
[0073] 8) Subsequently, a grain boundary diffusion treatment at 880°C was carried out in a high vacuum annealing furnace for 12 hours, and a low-temperature tempering heat treatment at 480°C was carried out for 5 hours to obtain a high-performance rare earth permanent magnet material with a composite hard magnetic shell structure.
[0074] The EPMA element surface distribution results show that there is a composite hard magnetic shell structure in the main phase grain epitaxial layer of the magnet, namely the Tb-rich hard magnetic shell introduced by the multi-main phase technology, and the outermost Dy / Tb-rich hard magnetic shell introduced by the grain boundary diffusion technology; the test results of the AMT-4 permanent magnet characteristic measuring instrument show that the magnetic properties of the magnet are B r =13.1kG, H cj =38.2kOe, (BH) max =41.2MGOe.
[0075] Comparative Example 4:
[0076] The difference from Example 4 is that the magnet is not subjected to magnetron sputtering. The EPMA element surface distribution results show that there is only a single-layer Tb-rich hard magnetic shell structure in the epitaxial layer of the main phase grain of the magnet; the test results of the AMT-4 permanent magnet property measuring instrument show that the magnetic properties of the magnet are B r =13.2kG, H cj =27.2kOe, (BH) max =42.3MGOe.
Claims
1. A method for preparing a high-performance rare earth permanent magnetic material having a composite hard magnetic shell structure, characterized in that: Firstly, a multi-main-phase magnet having a heavy rare earth-rich hard magnetic shell is prepared by using a main-phase alloy I without heavy rare earth and one or more main-phase alloys II with heavy rare earth added; then, a heavy rare earth alloy film is deposited on the surface of the multi-main-phase magnet by magnetron sputtering, and a new hard magnetic shell with a higher heavy rare earth content is formed on the surface of the main-phase grains through grain boundary diffusion and low-temperature tempering heat treatment; Among them, the main phase alloy I without heavy rare earth has a composition of RE in mass percentage. x1 Q bal M y1 B z1 , RE is one or more of the other lanthanide rare earth elements except the heavy rare earth elements Dy and Tb, Q is one or more of the elements Fe, Co, and Ni, M is one or more of the elements Al, Cr, Cu, Ga, Mn, Mo, N, Nb, P, Pb, Si, Ta, Ti, V, and Zr, B is boron, and x1, y1, and z1 satisfy the following relationship: 27≤x1≤36, 0≤y1≤3, and 0.8≤z1≤1.2; Among them, the main phase alloy II with heavy rare earth added has the following composition by mass percentage: w HRE 1-w ) x2 Q bal M y2 B z2 , RE is one or more of the other lanthanide rare earth elements except the heavy rare earth elements Dy and Tb, HRE is one or two of the heavy rare earth elements Dy and Tb, Q is one or more of the elements Fe, Co, and Ni, M is one or more of the elements Al, Cr, Cu, Ga, Mn, Mo, N, Nb, P, Pb, Si, Ta, Ti, V, and Zr, B is boron, and x2, y2, z2, and w satisfy the following relationship: 0.2≤w≤0.8, 26≤x2≤35, 0≤y2≤3, and 0.85≤z2≤1.15; Among them, the heavy rare earth alloy film is composed of HRE in terms of mass percentage. a RE b Q bal N c , HRE is one or two of the heavy rare earth elements Dy and Tb, RE is one or more of the other lanthanide rare earth elements except the heavy rare earth elements Dy and Tb, Q is one or more of the elements Fe, Co, and Ni, N is one or more of the elements Al, Cu, Ga, Zn, Mn, and Mg, and a, b, and c satisfy the following relationship: 20≤a≤70, 2≤b≤15, and 0≤c≤10.
2. The method for preparing a high-performance rare earth permanent magnetic material having a composite hard magnetic shell structure according to claim 1, characterized in that: The specific steps include: 1) According to the composition of main phase alloy I without heavy rare earth and main phase alloy II with heavy rare earth, the ingredients are prepared respectively, and the vacuum degree is ≤10 -2 Different main phase alloys were melted in a vacuum medium frequency induction furnace at 10000 Pa, and main phase alloy flakes with a thickness of 0.2-0.6 mm were obtained by rapid solidification casting technology. Main phase alloy I and main phase alloy II powders with an average particle size of 2-4 μm were prepared by hydrogen crushing and air flow grinding. 2) Under nitrogen or argon protection, the main phase alloy I and the main phase alloy II powders with different compositions are uniformly mixed according to a proportion to obtain mixed main phase powders with different heavy rare earth addition amounts; 3) Orienting and pressing the obtained mixed main phase powder in a 1.5-2.0T magnetic field to obtain a green body; 4) After vacuum packaging the obtained green body, cold isostatic pressing is performed at 150-250 MPa, and then sintering is performed in a high vacuum positive pressure sintering furnace to obtain a sintered magnet; 5) Pre-treating the surface of the obtained sintered magnet to ensure that the surface roughness Ra of the magnet is less than or equal to 0.1 μm and the surface is free of oil stains; 6) Activate the target and evacuate to 1×10 -3 ~1×10 -4 Pa, and then high-purity argon gas was introduced to adjust the vacuum degree to 1.5×10 -2 ~1.0Pa, adjust the target power to 60~140W, the bias voltage to 70~130V, and the working time to 5~15min; then turn on the DC power supply, bombard the target surface for 5~15min to remove the oxide layer on the target surface; 7) performing magnetron sputtering on the surface of the magnet treated in step 5) to deposit a heavy rare earth alloy film, introducing high-purity argon gas, with a gas flow rate of 15 to 60 sccm, a sputtering power of 60 to 220 W, and a sputtering time of 0.5 to 6 hours, and controlling the thickness of the deposited heavy rare earth alloy film to be 1 to 30 μm; 8) The deposited magnet is subjected to grain boundary diffusion treatment and low temperature tempering heat treatment in a high vacuum annealing furnace to obtain a high performance rare earth permanent magnet material with a composite hard magnetic shell structure.
3. The method for preparing a high-performance rare earth permanent magnetic material having a composite hard magnetic shell structure according to claim 2, characterized in that: In step 8), the grain boundary diffusion treatment system is: grain boundary diffusion is carried out in the range of 650 to 1000° C. for 0.5 to 12 h, and the low temperature tempering heat treatment system is: heat treatment is carried out in the range of 420 to 650° C. for 2 to 5 h.
4. A high-performance rare earth permanent magnetic material with a composite hard magnetic shell structure, characterized in that: The method is prepared by the method described in any one of claims 1 to 3.
5. The high performance rare earth permanent magnetic material with a composite hard magnetic shell structure as claimed in claim 4, characterized in that: The final magnet main phase grain epitaxial layer has multiple layers of heavy rare earth-rich hard magnetic shells, including two or more low heavy rare earth content n1 main phase grain cores and high heavy rare earth content n2 main phase grain cores, as well as high heavy rare earth content n3 main phase grain hard magnetic shells, and the outermost layer of higher heavy rare earth content n4 main phase grain hard magnetic shells, where n1<n3<n2 and n1<n3<n4, thereby improving the coercive force of the magnet and maintaining the remanence of the magnet.
6. The high performance rare earth permanent magnetic material with a composite hard magnetic shell structure as claimed in claim 4, characterized in that: The final magnet has a continuous rare earth-rich grain boundary phase, which effectively isolates the short-range magnetic exchange between adjacent grains and improves the coercive force of the magnet.