A salt-resistant polyamide composition and its preparation method and application
Through the synergistic effect of polyfatty amide, polyaromatic amide and compatibilizer, combined with glass fiber and ethylene-vinyl alcohol copolymer, the salt resistance of the polyamide composition is improved, and the salt resistance of the polyamide composition in the existing technology is solved. The problem of insufficient retention of mechanical properties in a fog environment has been solved, and the high performance of polyamide plastic products in a calcium chloride salt environment has been achieved.
Patent Information
- Application Number
- CN202210327045.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-30
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-03-30
AI Technical Summary
Existing polyamide compositions that are resistant to chloride salt stress corrosion cracking do not maintain high mechanical properties in salt spray environments, and cannot effectively improve the salt resistance of polyamide automotive parts to calcium chloride snow melting agents.
The synergistic effect of components such as polyaliphatic amide, polyaromatic amide and compatibilizer is used to improve the salt resistance of the polyamide composition through radiation cross-linking technology, glass fiber is added to enhance the mechanical properties, and ethylene-vinyl alcohol copolymer is used as the phase. Capacitant to improve system compatibility and resistance to chloride salt corrosion.
Significantly improves the retention rate of the tensile strength, flexural strength and notched impact properties of the polyamide composition under salt spray, ensuring the stable performance of polyamide plastic products in calcium chloride salt environments and meeting the needs of applications such as automotive cooling systems .
Smart Images

Figure BDA0003573944080000041 
Figure BDA0003573944080000051 
Figure BDA0003573944080000081
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of polymer materials, and more specifically to a salt-resistant polyamide composition, a preparation method thereof and an application thereof. Background Art
[0002] In addition to having to meet the service life requirements under high-temperature working conditions, nylon composite materials around automobile engines also face another more stringent use environment, which is the deicing agent that may be exposed in winter. Deicing agent is a chemical substance that melts snow on the road by lowering the melting point of ice and snow. The most common one is calcium chloride industrial salt. In addition to being corrosive to metal materials, it is also highly corrosive to nylon materials. It can reduce the hydrogen bonding strength between nylon molecules, greatly reduce the mechanical properties of the material, and cause corrosion cracking.
[0003] The prior art discloses a polyamide composition resistant to chloride salt stress corrosion cracking, which is made of the following raw materials in weight percentage: 45-90% polyamide resin; 5-50% glass fiber; 0.1-2% radiation stabilizer; 0.5-5% crosslinking agent; 0.1-15% antioxidant; 0.1-5% auxiliary agent. The present invention further improves the ability of polyamide, especially short-chain polyamide, to resist salt stress corrosion cracking through radiation crosslinking technology, so as to achieve cracking protection when polyamide automotive parts come into contact with chloride salt deicing agents. The polyamide composition mainly improves the salt stress corrosion cracking problem of polyamide nylon by adding radiation stabilizer and radiation crosslinking, but the improvement effect is not significant, and the retention rate of tensile strength, flexural strength and notched impact performance of the polyamide composition in a salt spray environment cannot be stably improved. Summary of the invention
[0004] The purpose of the present invention is to overcome the defects and shortcomings of the existing salt-resistant polyamide composition, such as poor salt resistance and low mechanical property retention rate, and to provide a salt-resistant polyamide composition. The salt resistance of the polyamide composition is significantly improved through the synergistic effect of components such as polyfatty amide, polyaromatic amide and a compatibilizer, and the performance retention rate of tensile strength, flexural strength and notched impact strength of the polyamide composition under salt spray is provided.
[0005] Another object of the present invention is to provide a method for preparing the salt-resistant polyamide composition.
[0006] Another object of the present invention is to provide an application of a salt-resistant polyamide composition in the preparation of salt-resistant polyamide plastic products.
[0007] Another object of the present invention is to provide a vehicle cooling system.
[0008] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0009] A salt-resistant polyamide composition comprises the following components in parts by weight:
[0010] 30-55 parts of polyfatty amide; 10-35 parts of polyaromatic amide; 10-50 parts of glass fiber; 1-6 parts of compatibilizer; 0-2 parts of other additives.
[0011] Among them, it should be noted that:
[0012] The polyaromatic amide of the present invention has a benzene ring structure, has a low water absorption rate, and has a better resistance to calcium chloride solution. The compatibilizer can better improve the combination between glass fiber and polyfatty amide, and further enhance the effect of resisting the corrosion of calcium chloride solution. The glass fiber mainly plays a reinforcing role and can synergistically improve the mechanical properties of the polyamide composition under salt-resistant conditions.
[0013] In a specific embodiment, in order to further improve the salt resistance of the polyamide composition and improve the retention rate of the tensile strength, flexural strength and notched impact properties of the material under salt spray conditions, it is further preferred that the following components are included in parts by weight:
[0014] 35-40 parts of polyfatty amide; 15-30 parts of polyaromatic amide; 25-35 parts of glass fiber; 3-5 parts of compatibilizer; 0.5-1 part of other additives.
[0015] In a specific embodiment, preferably, the relative viscosity of the polyaromatic amide of the present invention is 2.4 to 2.6.
[0016] Among them, it should be noted that:
[0017] The relative viscosity of polyaromatic amide can be tested by the following method: testing according to ISO 307-2007 standard, using 96% concentrated sulfuric acid.
[0018] More preferably, the polyaromatic amide is poly(hexamethylene isophthalamide).
[0019] The poly(hexamethylene isophthalamide) and poly(fatty acid amide) have synergistic effects, and the processing technology is more coordinated with the poly(fatty acid amide), so a better compound processing effect can be achieved with the poly(fatty acid amide), which is more conducive to the processing and production of the salt-resistant polyamide composition.
[0020] In a specific embodiment, the compatibilizer of the present invention is preferably an ethylene-vinyl alcohol copolymer.
[0021] Ethylene-vinyl alcohol copolymer contains many hydroxyl groups in its molecular chain, which has high polarity and strong binding force with nylon resin and glass fiber, playing a bridging role and enhancing the compatibility of the system. At the same time, because the presence of hydroxyl groups can inhibit the destruction of amide bonds by chloride salts, the salt resistance of the polyamide composition can be further improved.
[0022] Ethylene-vinyl alcohol copolymer is beneficial to further improve the system compatibility of the polyamide composition and is more beneficial to improve the salt-resistant mechanical properties.
[0023] Preferably, the viscosity of the polyfatty acid amide is 120-150 mL / g.
[0024] Among them, it should be noted that:
[0025] The viscosity number of polyfatty acid amide can be tested by the following method: testing according to ISO 307-2007 standard, using 96% concentrated sulfuric acid.
[0026] In a specific embodiment, the polyfatty acid amide of the present invention can be one or more of PA6, PA66, PA610 and PA612.
[0027] Preferably, the polyfatty acid amide is PA610 and / or PA612.
[0028] PA610 and PA612 have lower water absorption than other polyacrylic acid amides, which is more conducive to improving salt resistance.
[0029] In a specific embodiment, in order to further improve the processing performance and meet the actual application performance requirements of the polyamide composition, other additives of the polyamide composition of the present invention may include antioxidants and lubricants.
[0030] In a specific embodiment, the antioxidant of the present invention may include one or more of hindered phenol antioxidants (1010, 1098) and phosphate antioxidants (168, PEP-36, etc.).
[0031] In a specific embodiment, the lubricant of the present invention can be one or more of amides, esters, and polyethylene waxes.
[0032] The present invention also specifically protects a method for preparing a salt-resistant polyamide composition, comprising the following steps:
[0033] After the components are uniformly mixed, they are added into a twin-screw extruder for melt mixing and extrusion granulation to obtain a salt-resistant polyamide composition.
[0034] The salt-resistant polyamide composition of the present invention has excellent salt resistance. Under the DBL5416-2010 standard test, it can still maintain a good mechanical property retention rate in an alcohol solution of a 35% concentration of CaCl2 solution, and can better maintain the tensile strength, bending strength and notched impact properties of the material, meeting the performance requirements of salt-resistant polyamide plastic products. Therefore, the use of the salt-resistant polyamide composition in the preparation of salt-resistant polyamide plastic products is also within the protection scope of the present invention.
[0035] The present invention also specifically protects an automobile cooling system, wherein a heat dissipation water chamber of the automobile cooling system is prepared from the salt-resistant polyamide composition.
[0036] The automobile cooling system needs to withstand corrosion from calcium chloride industrial salt and the like, especially components such as the heat dissipation water chamber therein. The automobile cooling system components prepared using the salt-resistant polyamide composition of the present invention have good salt resistance and can maintain good mechanical properties in a salt spray environment, thus fully meeting the use requirements of the automobile cooling system.
[0037] Compared with the prior art, the present invention has the following beneficial effects:
[0038] The polyamide composition of the present invention utilizes the synergistic effect of components such as polyfatty amide, polyaromatic amide and compatibilizer to significantly improve the salt resistance of the polyamide composition. After being immersed in an alcohol solution of calcium chloride salt, the retention rate of the tensile strength performance can reach more than 97%, the retention rate of the bending strength performance can reach more than 97%, and the retention rate of the notched impact performance can reach more than 90%. It has excellent salt resistance mechanical property retention rate and can fully meet the performance requirements of polyamide plastic parts used in salt spray environments such as automobile cooling systems. DETAILED DESCRIPTION
[0039] The present invention is further described below in conjunction with specific embodiments, but the embodiments do not limit the present invention in any form. Unless otherwise specified, the raw materials and reagents used in the embodiments of the present invention are conventionally purchased raw materials and reagents.
[0040] Wherein, the raw materials of the embodiments of the present invention and the comparative examples are described as follows:
[0041] Polyfatty amide:
[0042] PA612: viscosity number 125mL / g, brand A120, manufacturer Shandong Guangyin;
[0043] PA66: viscosity 145mL / g, brand EP-158, manufacturer Zhejiang Huafeng;
[0044] Polyarylamide:
[0045] Polyaromatic amide-1: poly(hexamethylene isophthalamide), relative viscosity 2.5, brand PA MXD6, manufacturer Shanghai Yinggu Chemical Co., Ltd.;
[0046] Polyaromatic amide-2: poly 6T / 66, relative viscosity 2.4, brand KFHP41B, manufacturer Zhuhai Wantong Special Engineering Plastics Co., Ltd.
[0047] Compatibilizer:
[0048] Compatibilizer-1: ethylene-vinyl alcohol copolymer, brand EV-3851F, manufacturer: SK, South Korea;
[0049] Compatibilizer-2: Acrylate copolymer, brand AC RESIN 2615, manufacturer DuPont, USA;
[0050] Glass fiber: commercially available, the parallel embodiments of the present invention and the comparative examples are of the same kind;
[0051] Antioxidant: Hindered phenol antioxidant, commercially available, the parallel examples and comparative examples of the present invention are of the same type;
[0052] Lubricant: amide lubricant, commercially available, the parallel examples and comparative examples of the present invention are of the same type.
[0053] Examples 1 to 6
[0054] A salt-resistant polyamide composition comprises the components described in Table 1 below, in parts by weight.
[0055] Table 1 Content of each component
[0056]
[0057]
[0058] Wherein, the preparation method of the salt-resistant polyamide composition of Examples 1 to 6 is as follows:
[0059] After the components are uniformly mixed, they are added into a twin-screw extruder at a temperature of 250±15° C. for melt mixing and extrusion granulation to obtain a salt-resistant polyamide composition.
[0060] Example 7
[0061] A salt-resistant polyamide composition, comprising the following components in parts by weight:
[0062] 40 parts of polyfatty amide; 20 parts of polyaromatic amide; 30 parts of glass fiber; 5 parts of compatibilizer, 0.4 parts of antioxidant, and 0.3 parts of lubricant.
[0063] Among them, the polyfatty amide is PA612, the polyaromatic amide is polyaromatic amide-2: PA6T / 66, and the compatibilizer is ethylene-vinyl alcohol copolymer.
[0064] The preparation method of the salt-resistant polyamide composition is as follows:
[0065] After the components are uniformly mixed, they are added into a twin-screw extruder for melt mixing and extrusion granulation to obtain a salt-resistant polyamide composition.
[0066] Example 8
[0067] A salt-resistant polyamide composition, comprising the following components in parts by weight:
[0068] 40 parts of polyfatty amide; 20 parts of polyaromatic amide; 30 parts of glass fiber; 5 parts of compatibilizer, 0.4 parts of antioxidant, and 0.3 parts of lubricant.
[0069] The polyfatty amide is PA66, the polyaromatic amide is polyaromatic amide-1 poly(hexamethylene isophthalamide), and the compatibilizer is ethylene-vinyl alcohol copolymer.
[0070] The preparation method of the salt-resistant polyamide composition is as follows:
[0071] After the components are uniformly mixed, they are added into a twin-screw extruder for melt mixing and extrusion granulation to obtain a salt-resistant polyamide composition.
[0072] Example 9
[0073] A salt-resistant polyamide composition, comprising the following components in parts by weight:
[0074] 40 parts of polyfatty amide; 20 parts of polyaromatic amide; 30 parts of glass fiber; 5 parts of compatibilizer, 0.4 parts of antioxidant, and 0.3 parts of lubricant.
[0075] The polyfatty amide is PA612, the polyaromatic amide is polyaromatic amide-1: poly(hexamethylene isophthalamide), and the compatibilizer is compatibilizer 2: acrylate copolymer.
[0076] The preparation method of the salt-resistant polyamide composition is as follows:
[0077] After the components are uniformly mixed, they are added into a twin-screw extruder for melt mixing and extrusion granulation to obtain a salt-resistant polyamide composition.
[0078] Comparative Examples 1 to 4
[0079] A polyamide composition comprises the components described in Table 2 below, in parts by weight.
[0080] Table 2 Content of each component
[0081] Serial number Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 PA612 30 55 30 55 PAMXD6 40 8 35 10 Fiberglass 50 10 50 10 Compatibilizer-1 6 1 8 0.8 Antioxidants 0.4 0.4 0.4 0.4 Lubricants 0.3 0.3 0.3 0.3
[0082] Wherein, the preparation method of the polyamide composition of Comparative Examples 1 to 4 is as follows:
[0083] After the components are uniformly mixed, they are added into a twin-screw extruder at a processing temperature of 250±15° C. for melt mixing and extrusion granulation to obtain a polyamide composition.
[0084] Comparative Example 5
[0085] A polyamide composition, comprising the following components in parts by weight:
[0086] 40 parts of polyfatty amide; 30 parts of glass fiber; 5 parts of compatibilizer, 0.4 parts of antioxidant, and 0.3 parts of lubricant.
[0087] Wherein, the polyfatty amide is PA612, poly(hexamethylene isophthalamide), and the compatibilizer is ethylene-vinyl alcohol copolymer.
[0088] The preparation method of the polyamide composition is as follows:
[0089] After the components are uniformly mixed, they are added into a twin-screw extruder for melt mixing and extrusion granulation to obtain a polyamide composition.
[0090] Comparative Example 6
[0091] A polyamide composition, comprising the following components in parts by weight:
[0092] 40 parts of polyfatty amide, 20 parts of polyaromatic amide, 30 parts of glass fiber, 0.4 parts of antioxidant, and 0.3 parts of lubricant.
[0093] The polyfatty amide is PA612, and the polyaromatic amide is polyaromatic amide-1: poly(hexamethylene isophthalamide).
[0094] The preparation method of the polyamide composition is as follows:
[0095] After the components are uniformly mixed, they are added into a twin-screw extruder for melt mixing and extrusion granulation to obtain a polyamide composition.
[0096] Comparative Example 7
[0097] A polyamide composition, comprising the following components in parts by weight:
[0098] 40 parts of polyfatty amide, 30 parts of glass fiber, 0.4 parts of antioxidant, and 0.3 parts of lubricant.
[0099] Among them, the polyfatty amide is PA612.
[0100] The preparation method of the polyamide composition is as follows:
[0101] After the components are uniformly mixed, they are added into a twin-screw extruder for melt mixing and extrusion granulation to obtain a polyamide composition.
[0102] Results
[0103] The salt-resistant polyamide compositions prepared in the above embodiments and comparative examples were injection molded into ISO mechanical bars, including ISO527-2012, 1A tensile bars, ISO 178-2010 bending bars (80*10*4mm) and ISO179-2010 notched impact bars (80*10*4mm). The bars were treated with salt resistance, and the mechanical property retention rates before and after salt resistance were compared.
[0104] Salt resistance test method: According to the DBL5416:2010 standard test, first prepare a 35% concentration of CaCl2 solution, stir and mix 100mL of deionized water, 100mL of ethanol and 76.6g of CaCl2, and after cooling to room temperature, immerse the specimen in the solution for 30 minutes, take it out and rinse it with a large amount of deionized water; after drying, observe the surface state of the specimen and test the performance.
[0105] Among them, mechanical properties include tensile strength, flexural strength, and notched impact properties. The specific testing methods are as follows:
[0106] Tensile test is conducted in accordance with ISO 527:2012;
[0107] Bend test according to ISO 178:2010;
[0108] Notched impact test according to ISO 179:2010;
[0109] The specific test results are shown in Table 3 below.
[0110] Table 3 Test results
[0111]
[0112] Among them, the calculation formula of the relevant performance retention rate in Table 3 above is as follows:
[0113] Retention rate = strength after aging / strength before aging * 100%
[0114] And because polyamide will produce recrystallization and perfect crystallization during the salt resistance test, the related tensile strength properties, flexural strength properties and notched impact properties will be improved to a certain extent, and the tensile strength property retention rate, flexural strength property retention rate and notched impact property retention rate may be greater than 100%.
[0115] It can be seen from the data in Table 3 above that after the salt-resistant polyamide composition splines of the present invention are subjected to salt-resistant treatment, the appearance of the splines has no whitish cracking or only slight cracks, the surface state of the splines is good, and the mechanical test of the surface state of the splines after the salt-resistant treatment shows that the tensile strength performance retention rate is 97% and above, the bending strength performance retention rate is 97% and above, and the notched impact performance retention rate is 90% and above, and has good salt resistance.
[0116] The amount of polyaromatic amide added to the polyamide composition of Comparative Example 1 is too much. Obviously, the specimens have white appearance and cracks after salt resistance treatment, and the retention rate of mechanical properties is also significantly reduced.
[0117] The amount of polyaromatic amide added to the polyamide composition of Comparative Example 2 is too small. Obviously, the specimen has a whitish appearance and obvious cracks after salt resistance treatment, and the retention rate of mechanical properties decreases more significantly, which significantly reduces the salt resistance of the polyamide composition.
[0118] The amount of compatibilizer added to the polyamide composition of Comparative Example 3 is too much. Obviously, after the specimen is subjected to salt resistance treatment, the appearance is whitish and has obvious cracks, and the retention rate of mechanical properties is also significantly reduced, which significantly reduces the salt resistance of the polyamide composition.
[0119] The amount of compatibilizer added to the polyamide composition of Comparative Example 4 is too small. Obviously, after the specimen is subjected to salt resistance treatment, the appearance is whitish and cracked, and the retention rate of mechanical properties decreases more significantly, which significantly reduces the salt resistance of the polyamide composition.
[0120] The polyamide compositions of Comparative Examples 5-7 lack polyaromatic amide, compatibilizer and polyfatty amide respectively. After the specimens are subjected to salt resistance treatment, their corresponding appearance is whitish and has obvious cracks, and the retention rate of mechanical properties is significantly reduced, which significantly reduces the salt resistance of the polyamide composition.
[0121] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A salt-resistant polyamide composition, characterized in that: In parts by weight, it is composed of the following components: 35-40 parts of polyfatty amide; 15-30 parts of polyaromatic amide; 10-50 parts of glass fiber; 3-5 parts of compatibilizer; 0-2 parts of other additives; The polyfatty acid amide is PA612, and the viscosity of the polyfatty acid amide is 125-150 mL / g; The polyaromatic amide is PA MXD6, and the relative viscosity is 2.4 to 2.6; The compatibilizer is ethylene-vinyl alcohol copolymer; The other auxiliary agents are antioxidants and lubricants.
2. The salt-resistant polyamide composition according to claim 1, characterized in that: In parts by weight, it includes the following components: 35-40 parts of polyfatty amide; 15-30 parts of polyaromatic amide; 25-35 parts of glass fiber; 3-5 parts of compatibilizer; 0.5-1 part of other additives.
3. A method for preparing the salt-resistant polyamide composition according to any one of claims 1 to 2, characterized in that: The steps include: After the components are uniformly mixed, they are added into a twin-screw extruder for melt mixing and extrusion granulation to obtain a salt-resistant polyamide composition.
4. Use of the salt-resistant polyamide composition according to any one of claims 1 to 2 in the preparation of salt-resistant polyamide plastic products.
5. An automobile cooling system, characterized in that: The heat dissipation water chamber of the automobile cooling system is prepared from the salt-resistant polyamide composition according to any one of claims 1 to 2.
Citation Information
Patent Citations
Polyamide compositions with improved salt resistance and heat stability
CN102712810A
Low-moisture-absorption long-term heat-resistant aging-resistant polyamide composition and preparation method thereof
CN104592749A
High-surface glossiness and high-dimensional stability polyamide composite material and preparation method thereof
CN106751793A