A method for observing flat-top dots on flexible resin plates
By using matting agent to treat flexible resin plate samples under a three-dimensional microscope to eliminate reflections, the problem of "false dots" when observing flat-top dots on flexible resin plates has been solved, and clear observation of dot morphology and accurate data statistics have been achieved.
Patent Information
- Application Number
- CN202011574537.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-12-28
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2040-12-28
AI Technical Summary
When observing flat-top dots on flexible resin plates, commonly used microscopes are prone to reflections, leading to the appearance of "false dots" and affecting the observation effect and data accuracy. Existing methods are difficult to completely eliminate reflections.
Use a three-dimensional microscope combined with matting agent treatment, select coaxial epi-illumination mode, and use a mixture of organic or inorganic matting agent and solvent to matt the flexible resin plate sample to eliminate reflections. The microscope is set to a 500x objective lens and the reflection removal function is turned on.
It effectively eliminates the reflection of the flexographic plate base, and the dots have a clear appearance under the microscope. It can accurately count the three-dimensional data of the dots and evaluate the restoration performance of the dots.
Smart Images

Figure 201227190045 
Figure 201227190050 
Figure 201227190055
Abstract
Description
Technical Field
[0001] The invention relates to flat-top dots of a flexible resin plate, and in particular to an observation method for the flat-top dots of a flexible resin plate. Background Art
[0002] As a special type of relief printing, flexographic printing is defined in the printing technology standard terminology GB / T 9851.3-2008 as a printing method that uses an elastic relief plate to transfer ink to the surface of the substrate. At present, flexographic printing has been widely used in packaging and decoration, commercial and newspaper printing at home and abroad. With the call and popularization of "green printing" by national policies, flexographic printing has shown a rapid upward trend in my country, attracting more and more companies to join the flexographic printing industry. As a sunrise industry in the printing industry, flexographic printing has distinct advantages compared with other printing methods, such as: green and environmental protection, a wide range of substrates (such as paper, plastic film, self-adhesive paper, cellophane, corrugated paper, aluminum foil, textiles, etc., and there is almost no requirement for whether the surface of the substrate is flat.), the ink layer thickness is thinner than gravure printing, thicker than offset printing, and the quality of printed products is more stable than other printing methods such as offset printing, high efficiency, and fast speed. Therefore, flexographic printing has a greater advantage in the fierce competition in the printing market.
[0003] Although flexographic printing has many advantages mentioned above and uses light pressure printing, it still has some disadvantages that are difficult to overcome: because the flexographic printing plate itself is soft, elastic and easy to deform, it is easy to produce dot enlargement during the printing process, which leads to changes in color levels and reproduction effects. Dots below 5% are usually lost during the printing process. The reproducibility of 10%~15% dots is very poor. The dots in the dark tone level sometimes turn into solid, which makes it very difficult to stabilize the solid quality of the printed product. The image changes seriously due to the difference in color levels. The entire printed product has unclear levels. It is difficult to reproduce the subtle changes in the color levels of the image, which makes the three-dimensional sense of the printed product weak.
[0004] In order to solve the above-mentioned problems such as dot deformation, dot enlargement, small dot loss and layer merging caused by printing pressure, laser engraving flat-top dot technology came into being.
[0005] Flat-top dot laser engraving technology produces dots that are "flat-topped", see Figure 2 , the top of the dot is relative to the dot diagram of traditional laser plate making Figure 1It is flat, with a steeply inclined shoulder, and the part above the shoulder is perpendicular to the printing plate surface. Since the top of the "flat-top dot" is flat, it has many stress points, and the printing pressure is shared by multiple stress points. Therefore, the force on the top of the "flat-top dot" is uniform and stable. Because the shoulder of the "flat-top dot" is steeply inclined and the shoulder extension length is greater than that of the round-top dot, the bottom of the "flat-top dot" can share more pressure during the flexographic printing process, so that most of the deformation of the dot is concentrated at the bottom of the dot rather than the top. Therefore, under the same printing pressure, the dot expansion produced by the "flat-top dot" is smaller than that of the traditional dot, which greatly improves the quality of flexographic printing.
[0006] Make as Figure 2 There are several types of flat-top dots in domestic and foreign platemaking technologies: (1) Flint's NExT technology that integrates UVA-LED light source into traditional exposure machine; (2) Esko's Inline UV technology; (3) Kohler's high-quality LED light source KMF-LED flat-top dot technology; (4) DuPont's Digicorr / Digi Flow technology for platemaking with pure nitrogen; (5) Kodak's Flexcel NX technology for covering oxygen-insulating film; (6) MacDermid LUX technology. And Chinese patent CN 107521214 discloses a method of using liquid oxygen-insulating medium to block the contact between oxygen and exposed resin after ablation, and then subjecting the flexographic plate to UV main exposure to produce flat-top dots on the flexographic plate, so as to achieve the purpose of producing flat-top dots.
[0007] In view of the complex and diverse production technology of flat-top dots and their impact on the printing process and printed product quality, studying the dot morphology characteristics of "flat-top dots" is of great significance to the research and production of flexographic plates and to solving the dot enlargement phenomenon in the printing process.
[0008] The most common method for observing the appearance of flat-top dots is a microscope, such as a super-depth 3D microscope (KEYENCE digital microscope system). However, there is a great disadvantage in using this microscope to observe flat-top dots, that is, the flexible substrate will reflect light, resulting in reflective "fake dots" between the observed dots, such as Figure 3 , Figure 5 , Figure 7 As shown in the figure, the various shapes of columns between the normal dots are "false dots" caused by reflection, which is not only unsightly, but also affects the accurate calculation of normal dots. Moreover, it is difficult to completely eliminate the reflection of such dots by adjusting the incident light brightness (adjustable between 50-250), choosing different lighting methods (such as coaxial falling light, coaxial side light, coaxial ring light), and using the function of removing the reflection of the object in improving the visual effect.
[0009] As we all know, when a beam of light shines on a smooth surface, the light has the strongest reflective ability, while when the light shines on a rough surface, the light will be diffusely reflected or scattered in all directions, and the reflection is the weakest. Therefore, the extinction method is used to make the originally flat and smooth surface uneven, so as to achieve the purpose of extinction. When the gloss measured by the gloss meter is between 10-30, it is called matte, and less than 10 is dull. There are three main ways to reduce the gloss of the coating: one is to add inorganic granular matting agent; the second is to use spherical polymers with extinction properties; the third is to sandblast, etch, heat process or solvent corrosion on the smooth surface to obtain a certain rough surface, but this method will destroy the original morphology of the flat-top dots and is not easy to use.
[0010] At present, the commonly used matting agents are organic matting agents and inorganic matting agents. Organic matting agents include (1) metal soaps, such as aluminum stearate, calcium, zinc, etc.; (2) matting resins, which can avoid the problems of dust and reduced mechanical properties caused by the use of other matting agents. For example, triethoxypropylene silane silica, polyurea-formaldehyde resin, acrylic resin, poly(methyl methacrylate) / polystyrene microparticles, polyurethane spherical particles, etc. Inorganic matting agents are commonly used diatomaceous earth, talc, light calcium carbonate, kaolin, synthetic silica, etc. Summary of the invention
[0011] In order to solve the above problems, the present invention provides a method for observing flat-top dots of a flexible resin plate, which uses a three-dimensional microscope for observation and performs matting on the flat-top dots, so that relatively clear flat-top dots can be observed.
[0012] The object of the present invention is achieved in the following way: a method for observing flat-top dots of a flexible resin plate, using a matting agent to perform matting treatment on a flexible resin plate sample to be tested, and then using a three-dimensional microscope to observe the flat-top dots of the flexible resin plate sample and statistically calculate three-dimensional data, the lighting method selects coaxial incident light, a light source brightness of 120, a 500-fold objective lens, and turns on the de-reflection function.
[0013] The length of the flexible resin plate sample to be tested is 1 cm and the width is 1 cm.
[0014] The specific method of performing matte treatment on the flexible resin plate sample to be tested is to immerse the flexible resin plate sample to be tested in matte liquid for 2-5 minutes, preferably 3 minutes, take it out and dry it.
[0015] Paste the dried flexographic plate sample on a 3.5cm*15cm glass plate to ensure that the dots are on the same plane. You can use double-sided tape to paste.
[0016] The matting liquid used is: a matting agent and a solvent for dissolving or dispersing the matting agent.
[0017] The solvent for dissolving or dispersing the matting agent is at least one of water, ethanol and isopropanol.
[0018] The matting agent is at least one of an organic matting agent or an inorganic matting agent.
[0019] The organic matting agent is a metal soap or a matting resin.
[0020] The metal soap is at least one of aluminum stearate, calcium stearate or zinc stearate; the matting resin is at least one of triethoxypropylene silane-modified silica, polyurea-formaldehyde resin, acrylic resin, poly(methyl methacrylate) / polystyrene microparticles, and polyurethane spherical particles; the inorganic matting agent is at least one of diatomaceous earth, talc, light calcium carbonate, kaolin, and silica, and has a diameter of less than 0.1 micron.
[0021] The solvent for dissolving or dispersing the matting agent is a mixture of water and ethanol or a mixture of water and isopropanol, wherein the weight proportion of water is between 10-90%; and the matting agent accounts for 20-80% of the weight of the matting liquid.
[0022] In the mixture of water and ethanol or the mixture of water and isopropanol, the weight proportion of water is 50%, and the matting agent accounts for 50% of the weight of the matting liquid.
[0023] Compared with the prior art, the method provided by the present invention can observe the flat-top dots of the flexible resin plate and calculate the three-dimensional data of different dots, calculate the dot diameter and dot height, so as to evaluate the dot reproduction performance of the flexible resin plate. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is the dot map of traditional laser plate making.
[0025] Figure 2 It is a flat-top dot pattern for standard plate making.
[0026] Figure 3 :3D microscope picture of 3# flat-top dots without matting agent.
[0027] Figure 4 : Three-dimensional microscope picture of 3# flat-top dots after using matting agent.
[0028] Figure 5 :3D microscope picture of 4# flat-top dots without matting agent.
[0029] Figure 6 :Three-dimensional microscope picture of 4# flat-top dots after using matting agent.
[0030] Figure 7 : 3D microscope picture of 5# flat top dots without matting agent.
[0031] Figure 8 :Three-dimensional microscope picture of 5# flat-top dots after using matting agent. DETAILED DESCRIPTION
[0032] A method for observing flat-top dots of a flexible resin plate, comprising: performing matting treatment on a flexible resin plate sample to be tested with a matting agent, and then using a three-dimensional microscope to observe the flat-top dots of the flexible resin plate sample and calculate three-dimensional data, wherein the illumination mode is coaxial incident light, the light source brightness is 120, the objective lens is 500 times, and the de-reflection function is turned on.
[0033] The length of the flexible resin plate sample to be tested is 1 cm and the width is 1 cm.
[0034] The specific method of performing matte treatment on the flexible resin plate sample to be tested is to immerse the flexible resin plate sample to be tested in matte liquid for 2-5 minutes, preferably 3 minutes, take it out and dry it.
[0035] Paste the dried flexographic plate sample on a 3.5cm*15cm glass plate to ensure that the dots are on the same plane. You can use double-sided tape to paste.
[0036] The matting liquid used is: a matting agent and a solvent for dissolving or dispersing the matting agent.
[0037] The solvent for dissolving or dispersing the matting agent is at least one of water, ethanol and isopropanol.
[0038] The matting agent is at least one of an organic matting agent or an inorganic matting agent.
[0039] The organic matting agent is a metal soap or a matting resin.
[0040] The metal soap is at least one of aluminum stearate, calcium stearate or zinc stearate; the matting resin is at least one of triethoxypropylene silane-modified silica, polyurea-formaldehyde resin, acrylic resin, poly(methyl methacrylate) / polystyrene microparticles, and polyurethane spherical particles; the inorganic matting agent is at least one of diatomaceous earth, talc, light calcium carbonate, kaolin, and silica, and has a diameter of less than 0.1 micron.
[0041] The solvent for dissolving or dispersing the matting agent is a mixture of water and ethanol or a mixture of water and isopropanol, wherein the weight proportion of water is between 10-90%; and the matting agent accounts for 20-80% of the weight of the matting liquid.
[0042] In the mixture of water and ethanol or the mixture of water and isopropanol, the weight proportion of water is 50%, and the matting agent accounts for 50% of the weight of the matting liquid.
[0043] The following will be combined with the accompanying drawings and specific embodiments to clearly and completely describe the technical solution of the present invention. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art in this field can make some non-essential improvements and adjustments based on the content of the present invention described below. In the present invention, unless otherwise clearly specified and limited, the technical terms used in this application should be the common meanings understood by the technical personnel of the present invention.
[0044] Example 1
[0045] 3#, 4#, 5# flexible resin plates have flat-top dots. Cut the cleaned 3#, 4#, 5# flexible resin plates into small pieces with a length and width of 1 cm respectively, without matting, directly paste them on the glass plate, put them on the stage of the 3D microscope, set the lighting mode to coaxial incident light, light source brightness 120, 500x objective lens, turn on the de-reflection function, observe the flat-top dots and take photos, the results are shown in Figure 3 , Figure 5 and Figure 7 From these three figures, it can be seen that the flexible substrate has serious reflectivity and "false dots" appear, which affects the observation of dots and the acquisition of accurate three-dimensional data.
[0046] Example 2
[0047] Cut the cleaned 3# flexible resin plate into small pieces with a length and width of 1 cm respectively, and prepare 10 mL of 50% aluminum stearate solution, the solvent is a mixed solution of water and isopropanol, and the weight ratio of water to isopropanol is 1:1. Put the 3# flexible plate flat-top dot sample into the above-mentioned matting liquid for 2 minutes, take it out and dry it, and then paste it on a glass plate with a length and width of 3.5 cm*15 cm. Set the lighting mode to coaxial incident light, light source brightness 120, 500x objective lens, turn on the de-reflection function, observe the flat-top dots and take photos. The results are shown in Figure 4 As can be seen from this figure, the reflection of the flexible base is basically eliminated, no "false dots" appear, and the dot morphology is very clear. The three-dimensional data is shown in the following table.
[0048] Table 1 Three-dimensional data of 3# flat-top dots on flexible version
[0049] Sampling point 1 Sampling point 2 Sampling point 3 Sampling point 4 Sampling point 5 Sampling point 6 Sampling point 7 Sampling point 8 Sampling point 9 average value Dot diameter / micron 23.88 23.77 24.54 23.14 25.00 24.77 24.9 24.91 24.82 24.41 Dot height / micron 97.66 96.75 98.12 95.98 96.14 97.5 97.5 98.15 97.42 97.25
[0050] Example 3
[0051] Cut the cleaned 4# flexible resin plate into small pieces with a length and width of 1 cm respectively, and prepare 10 mL of 20% aluminum stearate solution. The solvent is a mixed solution of water and isopropanol, and the weight ratio of water to isopropanol is 1:9. Put the 4# flexible plate flat-top dot sample into the above matting liquid for 2 minutes, take it out and dry it, and paste it on the glass plate. Set the lighting mode to coaxial incident light, light source brightness 120, 500x objective lens, turn on the de-reflection function, observe the flat-top dots and take photos. The results are shown in Figure 6 As can be seen from this figure, the reflection of the flexible base is basically eliminated, no "false dots" appear, and the dot morphology is very clear. The three-dimensional data is shown in the following table.
[0052] Table 2 Three-dimensional data of 4# flat-top dots on flexible version
[0053] Sampling point 1 Sampling point 2 Sampling point 3 Sampling point 4 Sampling point 5 Sampling point 6 Sampling point 7 Sampling point 8 Sampling point 9 average value Dot diameter / micron 27.23 27.23 30.78 29.19 28.58 27.66 29.81 30.60 26.93 28.67 Dot height / micron 95.87 94.75 95.12 94.98 95.54 96.02 96.12 95.15 95.42 95.44
[0054] Example 4
[0055] Cut the cleaned 5# flexible resin plate into small pieces with a length and width of 1 cm respectively, and prepare 10 mL of 80% aluminum stearate solution. The solvent is a mixed solution of water and isopropanol, and the weight ratio of water to isopropanol is 9:1. Put the 5# flexible plate flat-top dot sample into the above matting liquid for 2 minutes, take it out and dry it, then stick it on the glass plate, set the lighting mode to coaxial incident light, light source brightness 120, 500x objective lens, turn on the de-reflection function, observe the flat-top dots and take photos, the results are shown in Figure 8 As can be seen from this figure, the reflection of the flexible base is basically eliminated, no "false dots" appear, and the dot morphology is very clear. The three-dimensional data is shown in the following table.
[0056] Table 3 Three-dimensional data of flexographic version 5# flat top dots
[0057] Sampling point 1 Sampling point 2 Sampling point 3 Sampling point 4 Sampling point 5 Sampling point 6 Sampling point 7 Sampling point 8 Sampling point 9 average value Dot diameter / micron 38.84 35.85 37.67 36.33 33.4 36.95 31.31 34.87 35.35 35.62 Dot height / micron 94.87 93.75 94.12 93.78 94.45 93.02 94.34 94.15 94.22 94.08
[0058] The embodiments of the present invention may also be the following embodiments:
[0059] Example 5
[0060] The cleaned 4# flexible resin plate was cut into small pieces with a length and width of 1 cm respectively, and 10 mL of poly(methyl methacrylate) / polystyrene microparticle suspension with a mass fraction of 50% was prepared. The solvent was a mixed solution of water and ethanol, and the weight ratio of water to ethanol was 1: 4. The 4# flexible plate flat-top dot sample was placed in the above-mentioned matting liquid for 3 minutes, taken out and dried, and then pasted on a glass plate. The lighting mode was set to coaxial incident light, light source brightness 100, 500x objective lens, and the de-reflection function was turned on. The flat-top dots were observed and photographed. The observation results showed that there were no "fake dots" and the dot morphology was very clear.
[0061] Example 6
[0062] The cleaned surface of the 5# flexible resin plate was cut into small pieces with a length and width of 1 cm respectively, and 10 mL of a 20% mass fraction of poly(methyl methacrylate) / polystyrene microparticle suspension was prepared. The solvent was a mixed solution of water and ethanol, and the weight ratio of water to ethanol was 1:1. The 5# flexible plate flat-top dot sample was placed in the above-mentioned matting liquid for 3 minutes, taken out and dried, and then pasted on a glass plate. The lighting mode was set to coaxial incident light, light source brightness 100, 500x objective lens, and the de-reflection function was turned on. The flat-top dots were observed and photographed. The observation results showed that there were no "fake dots" and the dot morphology was very clear.
[0063] Example 7
[0064] The cleaned surface of the 3# flexible resin plate was cut into small pieces with a length and width of 1 cm respectively, and 10 mL of poly(methyl methacrylate) / polystyrene microparticle suspension with a mass fraction of 80% was prepared. The solvent was a mixed solution of water and ethanol, and the weight ratio of water to ethanol was 9:1. The 3# flexible plate flat-top dot sample was placed in the above-mentioned matting liquid for 3 minutes, taken out and dried, and then pasted on the glass plate. The lighting mode was set to coaxial incident light, light source brightness 100, 500x objective lens, and the de-reflection function was turned on. The flat-top dots were observed and photographed. The observation results showed that there were no "fake dots" and the dot morphology was very clear.
[0065] Example 8
[0066] The cleaned 4# flexible resin plate was cut into small pieces with a length and width of 1 cm respectively, and 10 mL of 30% poly(methyl methacrylate) / polystyrene microparticle suspension was prepared. The solvent was a mixed solution of water and ethanol, and the weight ratio of water to ethanol was 1:9. The 4# flexible plate flat-top dot sample was placed in the above-mentioned matting liquid for 3 minutes, taken out and dried, and then pasted on a glass plate. The lighting mode was set to coaxial incident light, light source brightness 100, 500x objective lens, and the de-reflection function was turned on. The flat-top dots were observed and photographed. The observation results showed that there were no "fake dots" and the dot morphology was very clear.
[0067] Example 9
[0068] The cleaned surface of the 5# flexible resin plate was cut into small pieces with a length and width of 1 cm respectively, and 10 mL of 70% poly(methyl methacrylate) / polystyrene microparticle suspension was prepared. The solvent was a mixed solution of water and ethanol, and the weight ratio of water to ethanol was 2:3. The 5# flexible plate flat-top dot sample was placed in the above-mentioned matting liquid for 3 minutes, taken out and dried, and then pasted on the glass plate. The lighting mode was set to coaxial incident light, light source brightness 100, 500x objective lens, and the de-reflection function was turned on. The flat-top dots were observed and photographed. The observation results showed that there were no "fake dots" and the dot morphology was very clear.
[0069] Example 10
[0070] Cut the cleaned 3# flexible resin plate into small pieces with a length and width of 1 cm respectively, and prepare 10 mL of 40% silica suspension, the solvent is a mixed solution of water and isopropanol, and the weight ratio of water to isopropanol is 1:3. Put the 3# flexible plate flat-top dot sample into the above-mentioned matting liquid for 2 minutes, take it out and dry it, and paste it on the glass plate. Set the lighting mode to coaxial incident light, light source brightness 100, 500x objective lens, turn on the de-reflection function, observe the flat-top dots and take pictures. The observation results show that there are no "fake dots" and the dot morphology is very clear.
[0071] Embodiment 11
[0072] The cleaned surface of the 3# flexible resin plate was cut into small pieces with a length and width of 1 cm respectively, and 10 mL of a suspension of triethoxypropylene silane-modified silica with a mass fraction of 70% was prepared. The solvent was a mixed solution of water and ethanol, and the weight ratio of water to ethanol was 7:1. The 3# flexible plate flat-top dot sample was placed in the above-mentioned matting liquid for 3 minutes, taken out and dried, and then pasted on a glass plate. The lighting mode was set to coaxial incident light, light source brightness 100, 500x objective lens, and the de-reflection function was turned on. The flat-top dots were observed and photographed. The observation results showed that there were no "fake dots" and the dot morphology was very clear.
[0073] Example 12
[0074] The 4# flexible resin plate with clean surface was cut into small pieces with a length and width of 1 cm respectively, and 10 mL of a suspension of polyurea-formaldehyde resin with a mass fraction of 60% was prepared. The solvent was a mixed solution of water and ethanol, and the weight ratio of water to ethanol was 5:1. The 4# flexible plate flat-top dot sample was placed in the above-mentioned matting liquid for 3 minutes, taken out and dried, and then pasted on a glass plate. The lighting mode was set to coaxial incident light, light source brightness 100, 500x objective lens, and the de-reflection function was turned on. The flat-top dots were observed and photographed. The observation results showed that there were no "fake dots" and the dot morphology was very clear.
[0075] Embodiment 13
[0076] Cut the cleaned 5# flexible resin plate into small pieces with a length and width of 1 cm respectively, and prepare 10mL of a suspension of acrylic resin with a mass fraction of 40%. The solvent is a mixed solution of water and isopropanol, and the weight ratio of water to ethanol is 2:3. Put the 5# flexible plate flat-top dot sample into the above-mentioned matting liquid for 3 minutes, take it out and dry it, and paste it on the glass plate. Set the lighting mode to coaxial incident light, light source brightness 100, 500x objective lens, turn on the de-reflection function, observe the flat-top dots and take photos. The observation results show that there are no "fake dots" and the dot morphology is very clear.
[0077] Embodiment 14
[0078] The cleaned surface of the 3# flexible resin plate was cut into small pieces with a length and width of 1 cm respectively, and 10 mL of a suspension of polyurethane spherical particles with a mass fraction of 30% was prepared. The solvent was a mixed solution of water and isopropanol, and the weight ratio of water to ethanol was 1:3. The 3# flexible plate flat-top dot sample was placed in the above-mentioned matting liquid for 3 minutes, taken out and dried, and then pasted on a glass plate. The lighting mode was set to coaxial incident light, light source brightness 100, 500x objective lens, and the de-reflection function was turned on. The flat-top dots were observed and photographed. The observation results showed that there were no "fake dots" and the dot morphology was very clear.
[0079] Embodiment 15
[0080] Cut the cleaned 4# flexible resin plate into small pieces with a length and width of 1 cm respectively, and prepare 10 mL of diatomaceous earth suspension with a mass fraction of 35%. The solvent is a mixed solution of water, ethanol and isopropanol, and the weight ratio of water, ethanol and isopropanol is 4:4:1. Put the 4# flexible plate flat-top dot sample into the above-mentioned matting liquid for 3 minutes, take it out and dry it, and paste it on the glass plate. Set the lighting mode to coaxial incident light, light source brightness 100, 500x objective lens, turn on the de-reflection function, observe the flat-top dots and take pictures. The observation results show that there are no "fake dots" and the dot morphology is very clear.
[0081] Example 16
[0082] Cut the cleaned 5# flexible resin plate into small pieces with a length and width of 1 cm respectively, and prepare 10mL of talcum powder suspension with a mass fraction of 65%. The solvent is a mixed solution of water, ethanol and isopropanol, and the weight ratio of water, ethanol and isopropanol is 3:1:3. Put the 5# flexible plate flat-top dot sample into the above-mentioned matting liquid for 3 minutes, take it out and dry it, and paste it on the glass plate. Set the lighting mode to coaxial falling, light source brightness 100, 500x objective lens, turn on the de-reflection function, observe the flat-top dots and take pictures. The observation results show that there are no "fake dots" and the dot morphology is very clear.
[0083] Embodiment 17
[0084] Cut the cleaned 5# flexible resin plate into small pieces with a length and width of 1 cm respectively, and prepare 10 mL of suspension of light calcium carbonate with a mass fraction of 85%. The solvent is a mixed solution of water, ethanol and isopropanol, and the weight ratio of water, ethanol and isopropanol is 2:3:4. Put the 5# flexible plate flat-top dot sample into the above-mentioned matting liquid for 3 minutes, take it out and dry it, and paste it on the glass plate. Set the lighting mode to coaxial falling, light source brightness 100, 500x objective lens, turn on the de-reflection function, observe the flat-top dots and take pictures. The observation results show that there are no "fake dots" and the dot morphology is very clear.
[0085] Embodiment 18
[0086] The cleaned surface of the 3# flexible resin plate was cut into small pieces with a length and width of 1 cm respectively, and 10 mL of a suspension of kaolin with a mass fraction of 70% was prepared. The solvent was a mixed solution of water, ethanol and isopropanol, and the weight ratio of water, ethanol and isopropanol was 3:3:2. The 3# flexible plate flat-top dot sample was placed in the above-mentioned matting liquid for 3 minutes, taken out and dried, and then pasted on a glass plate. The lighting mode was set to coaxial incident light, light source brightness 100, 500x objective lens, and the de-reflection function was turned on. The flat-top dots were observed and photographed. The observation results showed that there were no "fake dots" and the dot morphology was very clear.
[0087] Embodiment 19
[0088] The cleaned surface of the 5# flexible resin plate was cut into small pieces with a length and width of 1 cm respectively, and 10 mL of calcium stearate solution with a mass fraction of 30% was prepared. The solvent was a mixed solution of water, ethanol and isopropanol, and the weight ratio of water, ethanol and isopropanol was 3:5:2. The 5# flexible plate flat-top dot sample was placed in the above-mentioned matting liquid for 3 minutes, taken out and dried, and then pasted on the glass plate. The lighting mode was set to coaxial incident light, light source brightness 100, 500x objective lens, and the de-reflection function was turned on. The flat-top dots were observed and photographed. The observation results showed that there were no "fake dots" and the dot morphology was very clear.
[0089] Embodiment 20
[0090] The cleaned 4# flexible resin plate was cut into small pieces with a length and width of 1 cm respectively, and 10 mL of 35% zinc stearate solution was prepared. The solvent was a mixed solution of water, ethanol and isopropanol, and the weight ratio of water, ethanol and isopropanol was 2:3:2. The 4# flexible plate flat-top dot sample was placed in the above matting liquid for 3 minutes, taken out and dried, and then pasted on the glass plate. The lighting mode was set to coaxial incident light, light source brightness 100, 500x objective lens, and the de-reflection function was turned on. The flat-top dots were observed and photographed. The observation results showed that there were no "fake dots" and the dot morphology was very clear.
[0091] The above is only to illustrate the typical implementation of the method of the present application, rather than all implementations. The protection scope of the present invention is not limited to this. In order to make the description concise, all possible combinations of the above-mentioned technical features are not described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification. When the combination of technical solutions is mutually contradictory or cannot be implemented, it should be considered that such a combination of technical solutions does not exist and is not within the protection scope required by the present invention. It should be pointed out that for those skilled in the art and any technician familiar with the technical field, without departing from the spirit of the overall concept of the invention and the principle of the present invention, the technical solution and its inventive concept of the present invention are equivalently replaced or changed, and several changes and improvements are made, which should also be regarded as the protection scope of the present invention.
Claims
1. A method for observing flat-top dots on flexible resin plates. Features: The flexible resin plate sample to be tested is subjected to matting treatment with a matting agent. The specific method for the matting treatment of the flexible resin plate sample to be tested is as follows: immersing the flexible resin plate sample to be tested in the matting liquid for 2-5 minutes, taking it out and drying it. The matting liquid used includes a matting agent and a solvent for dissolving or dispersing the matting agent. The solvent for dissolving or dispersing the matting agent is a mixed solution of water and ethanol, a mixed solution of water and isopropanol, or a mixed solution of water, ethanol and isopropanol. The matting agent is at least one of an organic matting agent or an inorganic matting agent, and the matting agent accounts for 20-80% of the weight of the matting liquid. The dried flexible resin plate sample is pasted on a glass plate to ensure that the dots are in the same plane, and then a three-dimensional microscope is used to observe the flat-top dots of the flexible resin plate sample and calculate the three-dimensional data. The illumination mode selects coaxial incident light, a light source brightness of 120, a 500-fold objective lens, and the de-reflection function is turned on.
2. The method for observing flat-top dots of a flexible resin plate according to claim 1, Features: The length of the flexible resin plate sample to be tested is 1 cm and the width is 1 cm.
3. The method for observing flat-top dots of a flexible resin plate according to claim 1, Features: Immerse the flexible resin plate sample to be tested in the matting liquid for 3 minutes; stick the dried flexible plate sample on a 3.5cm*15cm glass plate to ensure that the dots are on the same plane.
4. The method for observing flat-top dots of a flexible resin plate according to claim 1, Features: The organic matting agent is a metal soap or a matting resin.
5. The method for observing flat-top dots of a flexible resin plate according to claim 4, Features: The metal soap is at least one of aluminum stearate, calcium stearate or zinc stearate; the matting resin is at least one of triethoxypropylene silane-modified silica, polyurea-formaldehyde resin, acrylic resin, poly(methyl methacrylate) / polystyrene microparticles, and polyurethane spherical particles; the inorganic matting agent is at least one of diatomaceous earth, talc, light calcium carbonate, kaolin, and silica, and the diameter of each of them is less than 0.1 micron.
6. The method for observing flat-top dots of a flexible resin plate according to claim 1, Features: The solvent for dissolving or dispersing the matting agent is a mixture of water and ethanol or a mixture of water and isopropanol, wherein the weight proportion of water is between 10-90%.