A natural block ore thermal cracking test evaluation device and method under simulated blast furnace conditions

By simulating the dynamic testing method under blast furnace conditions and using high-temperature furnace and reaction furnace tube systems, the problem of static detection methods in the existing technology ignoring small cracks inside the lump ore is solved, and a more accurate assessment of the thermal cracking index of the lump ore is achieved. Reflects its ability to form powder in the blast furnace.

CN114689650BActive Publication Date: 2024-10-11UNIV OF SCI & TECH BEIJING
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210197585.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-01
Publication Date
2024-10-11
Estimated Expiration
2042-03-01

AI Technical Summary

Technical Problem

The existing technology mainly uses static methods when detecting the thermal cracking index of natural lump ore, ignoring the potential impact of fine cracks inside the lump ore on the movement of materials in the blast furnace, and cannot fully reflect the powder formation of lump ore in the blast furnace.

Method used

A thermal cracking test and evaluation device for natural lump ores under simulated blast furnace conditions was designed, including a heating system, a reaction system, a control system and a gas supply system. The blast furnace environment was simulated through dynamic testing methods, and the high-temperature furnace and reaction furnace tubes were used to rotate and Gas control, measuring the bursting of lumps of minerals as they are rotated and squeezed at high temperatures.

Benefits of technology

Through the dynamic testing method, it can objectively reflect the explosion of lump ore in the upper part of the blast furnace, provide a more accurate thermal burst index, and reflect the powder forming ability and internal cracks of lump ore in the blast furnace.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114689650B_ABST
    Figure CN114689650B_ABST
Patent Text Reader

Abstract

The present invention provides a device and method for testing and evaluating the thermal cracking of natural lump ore under simulated blast furnace conditions, and belongs to the technical field of ironmaking. The device includes a heating system, a reaction system, a control system and a gas supply system. The heating system provides heat, including resistance wire heating, and contains refractory bricks, insulation cotton, water cooling, etc. The control system controls the movement of the high-temperature furnace and the rotation of the reaction tube. The reaction system includes a reaction furnace tube, materials, water cooling, etc., and the gas supply system mainly supplies N2 and CO. The dried lump ore is placed in the reaction furnace tube, heated at a certain speed, and the reaction furnace tube rotates. After a certain reaction time, the reaction furnace tube is separated from the high-temperature furnace body, and screened after cooling to calculate the dynamic lump ore thermal cracking index. The present invention dynamically tests the bursting degree of the lump ore, presents the fragmentation caused by the internal cracks of the lump ore after the thermal cracking due to rolling, extrusion and friction in the blast furnace, and can objectively reflect the bursting of the upper powder ore in the lump ore in the blast furnace.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ironmaking, and in particular to a device and method for testing and evaluating thermal cracking of natural lump ore under simulated blast furnace conditions. Background Art

[0002] With the rapid development of my country's steel industry, iron-making workers have a deeper understanding of blast furnace production technology, and the level of blast furnace iron-making has made great progress. One of the manifestations of progress is that the proportion of natural lump ore in the charge structure has continued to increase. A large number of production practices have shown that natural lump ore has both advantages and disadvantages for blast furnace smelting. The advantages are as follows: 1) Some types of lump ore can improve the grade of entering the furnace and save the cost of agglomeration. 2) Lump ore has a greater price advantage than pellets. 3) Natural lump ore does not have pollutants in the production process of iron ore powder agglomeration. 4) Some types of lump ore have high reducibility, good indirect reduction in the furnace, and high utilization rate of furnace top gas, which is conducive to reducing the coke ratio. After using lump ore, many companies have significantly reduced costs and increased efficiency. The thermal cracking index of lump ore is one of the important criteria for judging whether natural lump ore can be put into the furnace. Its main function is to qualitatively predict the degree of powder formation of lump ore in the middle and upper parts of the blast furnace. At present, the main test method for detecting the thermal cracking standard of lump ore is the national standard GB / T 10322.6-2004 "Test method for thermal cracking index of iron ore".

[0003] In addition, there are also existing technologies on the thermal cracking index of natural lump ore of iron ore, such as the method for rapid measurement of the thermal cracking index of lump ore disclosed in the prior art. It is mainly aimed at the characteristics of the frequent heating and cooling of the standard thermal cracking test equipment, which takes a long time. The furnace body is equipped with 5 evenly distributed furnace slots, which can put 10 equally divided lump ore samples into the furnace twice at a time, shortening the measurement time, but it belongs to the static method of thermal cracking index. A method for detecting the thermal cracking index of lump ore disclosed in the prior art is to dry the sample with a screen size of 20-25 mm for 12 hours, keep the sample with a size of 20-25 mm and continue to dry it for 12 hours, heat the graphite crucible to 700°C, keep the constant temperature for 20 minutes, put in the test sample, take it out after at least 30 minutes, and calculate the DI. -6.3 This method is almost consistent with the national standard hot cracking index static method.

[0004] It can be seen that the current methods for detecting the bursting of lump ore only consider static bursting. The bursting mechanism is that when heated to a certain temperature, the crystal water and carbonate inside the lump ore decompose, generate internal stress, and burst it along the texture direction. It is ignored that there are still a large number of cracks inside the lump ore. These cracks will be potential factors for the generation of cracks in the lump ore during the subsequent material movement process. These cracks are inside, and the cracks are extremely small. They cannot be observed by the naked eye and cannot be directly measured, but they can be qualitatively tested by simulating the extrusion friction in the blast furnace. Based on this, the present invention designs a test method and equipment for the powder generation ability of such lump ore. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a device and method for testing and evaluating thermal cracking of natural lump ore under simulated blast furnace conditions.

[0006] The device includes a heating system, a reaction system, a control system and a gas supply system.

[0007] The heating system is a high temperature furnace, including a resistance wire, a furnace body, and a temperature measuring thermocouple; the reaction system includes a reaction furnace tube, a furnace tube screen, a bearing seat, a furnace tube rotating mechanism, a temperature measuring thermocouple, and a sliding assembly; the control system includes a pressure gauge, a gas circuit control area, a furnace tube rotation control area, a furnace body movement control area, and a temperature control system; and the gas supply system includes an air outlet and an air inlet;

[0008] The high-temperature furnace body is hollow and can accommodate a reaction furnace tube. The high-temperature furnace body has a built-in resistance wire, refractory bricks are arranged on the inner wall of the furnace body, a furnace temperature thermocouple is arranged on the inner wall of the high-temperature furnace body, a temperature measuring thermocouple is arranged in the high-temperature furnace body, and the high-temperature furnace body is placed on a sliding assembly; the reaction furnace tube can rotate with the furnace tube rotating mechanism, the reaction furnace tube is introduced into the reaction furnace tube through the air inlet, and the gas is discharged through the air outlet, and a pressure gauge is installed at the air outlet; a furnace tube screen is arranged at the opening of the reaction furnace tube; the overall device controls the gas supply system through the gas path control area, controls the furnace tube rotating mechanism through the furnace tube rotation control area, controls the high-temperature furnace body through the furnace body movement control area, and controls the temperature inside the high-temperature furnace through the temperature control system.

[0009] The opening of the reaction furnace tube is sealed by a sealing flange.

[0010] A hole is opened on the sealing flange to connect the rotating tube, which is placed on the bearing seat. The rotating tube drives the reaction furnace tube to rotate along with the furnace tube rotating mechanism. An air inlet and an air outlet are arranged on the rotating tube, and a pressure gauge is installed at the air outlet.

[0011] The test method of the device comprises the following steps:

[0012] S1: Take a 20-25mm natural lump ore sample and dry it as the reaction material;

[0013] S2: Place the reaction materials in the reaction furnace tube, install the furnace tube screen, add the sealing flange, and place the reaction furnace tube on the bearing seat;

[0014] S3: Raising the temperature inside the high-temperature furnace to the reaction temperature through the temperature control system;

[0015] S4: Control the gas to enter the reaction furnace tube through the gas path control area;

[0016] S5: Control the sliding assembly through the furnace body movement control area to place the reaction furnace tube in the high-temperature furnace body;

[0017] S6: After the high temperature furnace body is stable, the furnace tube rotation mechanism is controlled by the furnace tube rotation control area to drive the reaction furnace tube to rotate;

[0018] S7: After a period of reaction, the gas input is stopped through the gas path control area, the reaction furnace tube rotation is stopped through the furnace tube rotation control area, and the high temperature furnace body is reset through the furnace body movement control area;

[0019] S8: After the reaction furnace tube is cooled to room temperature, the reaction material is taken out, sieved, and weighed;

[0020] S9: Calculate the dynamic thermal cracking reaction parameters of the lump ore according to the screening results in S8.

[0021] Among them, the drying temperature in S1 is 105℃±1℃, and the drying time is not less than 4 hours.

[0022] The reaction temperature in S3 is 700°C-1100°C.

[0023] The gases in S4 are N2 and CO, the N2 flow rate is 10.5L / min, the CO flow rate is 4.5L / min, and the total is 15L / min.

[0024] The speed of the reaction furnace tube in S6 is 5-30r / min.

[0025] S7 reaction time is 30-60min.

[0026] In S9, the proportion of particles <6.3 mm is used as the thermal cracking index of the lump ore.

[0027] The beneficial effects of the above technical solution of the present invention are as follows:

[0028] In the above scheme, the bursting degree of the lump ore is tested by a dynamic test method, showing the internal cracks of the lump ore after thermal cracking due to rolling, extrusion and friction in the blast furnace. The lump ore thermal cracking test results of the present invention can objectively reflect the bursting of the upper powder ore in the lump ore in the blast furnace. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a schematic structural diagram of a natural block ore thermal cracking test and evaluation device under simulated blast furnace conditions of the present invention;

[0030] Figure 2 This is a heating curve of a high temperature furnace in an embodiment of the present invention;

[0031] Figure 3 This is the test result in the embodiment of the present invention.

[0032] Among them: 1-temperature measuring thermocouple, 2-high temperature furnace body, 3-furnace temperature thermocouple, 4-reaction furnace tube, 5-gas outlet, 6-pressure gauge, 7-gas inlet, 8-furnace tube rotating mechanism, 9-gas path control area, 10-furnace tube rotation control area, 11-furnace body movement control area, 12-bearing seat, 13-furnace tube screen, 14-sliding assembly, 15-temperature control system, 16-reaction material. DETAILED DESCRIPTION

[0033] In order to make the technical problems, technical solutions and advantages to be solved by the present invention more clear, a detailed description will be given below with reference to the accompanying drawings and specific embodiments.

[0034] The invention provides a device and method for testing and evaluating thermal cracking of natural lump ore under simulated blast furnace conditions.

[0035] like Figure 1 As shown, the device includes a heating system, a reaction system, a control system and a gas supply system.

[0036] The heating system is a high temperature furnace, including a resistance wire, a high temperature furnace body 2, and a furnace temperature thermocouple 3; the reaction system includes a reaction furnace tube 4, a furnace tube screen 13, a bearing seat 12, a furnace tube rotating mechanism 8, a temperature measuring thermocouple 1, and a sliding assembly 14; the control system includes a pressure gauge 6, a gas circuit control area 9, a furnace tube rotation control area 10, a furnace body movement control area 11, and a temperature control system 15; and the gas supply system includes an air outlet 5 and an air inlet 7;

[0037] The high-temperature furnace body 2 is hollow and can accommodate a reaction furnace tube 4. The high-temperature furnace body 2 has a built-in resistance wire, and refractory bricks are arranged on the inner wall of the furnace body. A furnace temperature thermocouple 3 is arranged on the inner wall of the high-temperature furnace body 2. A temperature measuring thermocouple 1 is arranged in the high-temperature furnace body 2, and the high-temperature furnace body 2 is placed on a sliding assembly 14; the reaction furnace tube 4 can rotate with the furnace tube rotating mechanism 8, and the reaction gas is introduced into the reaction furnace tube 4 through the air inlet 7 and the gas is discharged through the air outlet 5. A pressure gauge 6 is installed at the air outlet 5; a furnace tube screen 13 is arranged at the opening of the reaction furnace tube 4; the overall device controls the gas supply system through the gas path control area 9, controls the furnace tube rotating mechanism 8 through the furnace tube rotation control area 10, controls the high-temperature furnace body 2 through the furnace body movement control area 11, controls the temperature inside the high-temperature furnace through the temperature control system 15, measures the temperature of the high-temperature furnace body with the furnace temperature thermocouple 3, and measures the temperature of the reaction material 16 with the temperature measuring thermocouple 1.

[0038] The opening of the reaction furnace tube 4 is sealed by a sealing flange.

[0039] A hole is opened on the sealing flange to connect the rotating tube, which is placed on the bearing seat 12. The rotating tube drives the reaction furnace tube 4 to rotate along with the furnace tube rotating mechanism 8. An air inlet 7 and an air outlet 5 are arranged on the rotating tube, and a pressure gauge 6 is installed at the air outlet 5.

[0040] The specific test process is explained below.

[0041] S1: Take 500 g ± 1 g of a natural lump ore sample with a particle size of 20-25 mm and dry it at 105° C. for 4 hours as the reaction material 16;

[0042] S2: placing the reaction material 16 in the reaction furnace tube 4, installing the furnace tube screen 13, and adding a sealing flange, and placing the reaction furnace tube 4 on the bearing seat 12;

[0043] S3: The temperature in the high temperature furnace body 2 is raised to 950°C ± 10°C by the temperature control system 15; wherein the temperature rise curve of the high temperature furnace is as follows: Figure 2 As shown;

[0044] S4: Control the gas to enter the reaction furnace tube 4 through the gas path control area 9;

[0045] S5: Control the sliding assembly 14 through the furnace body movement control area 11 to place the reaction furnace tube 4 in the high-temperature furnace body 2;

[0046] S6: After the high temperature furnace body 2 is stabilized, the furnace tube rotation control area 10 controls the furnace tube rotation mechanism 8 to drive the reaction furnace tube 4 to rotate;

[0047] S7: After the reaction has lasted for 30 minutes, the gas input is stopped through the gas path control area 9, the rotation of the reaction furnace tube 4 is stopped through the furnace tube rotation control area 10, and the high temperature furnace body 2 is reset through the furnace body movement control area 11;

[0048] S8: After the reaction furnace tube 4 is cooled to room temperature, the reaction material is taken out, its mass is measured, and it is sieved with 6.3 mm, 3.15 mm and 0.5 mm sieves;

[0049] S9: Based on the screening results in S8, the proportion of particles <6.3 mm is taken as the thermal burst index and expressed as DI.

[0050] Take natural block ore A and conduct the test according to the above steps. The results are as follows Figure 3 shown.

[0051] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A natural block ore thermal cracking test and evaluation device under simulated blast furnace conditions, characterized in that: Including heating system, reaction system, control system and gas supply system, The heating system is a high-temperature furnace, including a resistance wire, a high-temperature furnace body, and a furnace temperature thermocouple; the reaction system includes a reaction furnace tube, a furnace tube screen, a bearing seat, a furnace tube rotating mechanism, a temperature measuring thermocouple, and a sliding assembly; the control system includes a pressure gauge, a gas circuit control area, a furnace tube rotation control area, a furnace body movement control area, and a temperature control system; and the gas supply system includes an air outlet and an air inlet; The high-temperature furnace body is hollow and can accommodate a reaction furnace tube. The high-temperature furnace body has a built-in resistance wire, refractory bricks are arranged on the inner wall of the furnace body, a furnace temperature thermocouple is arranged on the inner wall of the high-temperature furnace body, a temperature measuring thermocouple is arranged in the high-temperature furnace body, and the high-temperature furnace body is placed on a sliding assembly; the reaction furnace tube can rotate with the furnace tube rotating mechanism, the reaction furnace tube is introduced into the reaction furnace tube through the air inlet, and the gas is discharged through the air outlet, and a pressure gauge is installed at the air outlet; a furnace tube screen is arranged at the opening of the reaction furnace tube; the overall device controls the gas supply system through the gas path control area, controls the furnace tube rotating mechanism through the furnace tube rotation control area, controls the high-temperature furnace body through the furnace body movement control area, and controls the temperature inside the high-temperature furnace through the temperature control system.

2. The natural block ore thermal cracking test and evaluation device under simulated blast furnace conditions according to claim 1, characterized in that: The opening of the reaction furnace tube is sealed by a sealing flange.

3. The natural block ore thermal cracking test and evaluation device under simulated blast furnace conditions according to claim 2, characterized in that: The sealing flange is provided with a hole to connect a rotating tube, the rotating tube is placed on a bearing seat, and the rotating tube drives the reaction furnace tube to rotate along with the furnace tube rotating mechanism; an air inlet and an air outlet are arranged on the rotating tube.

4. The test method of the natural block ore thermal cracking test and evaluation device under simulated blast furnace conditions according to claim 1, characterized in that: The steps include: S1: Take a 20-25mm natural lump ore sample and dry it as the reaction material; S2: Place the reaction materials in the reaction furnace tube, install the furnace tube screen, add the sealing flange, and place the reaction furnace tube on the bearing seat; S3: Raising the temperature inside the high-temperature furnace to the reaction temperature through the temperature control system; S4: Control the gas to enter the reaction furnace tube through the gas path control area; S5: Control the sliding assembly through the furnace body movement control area to place the reaction furnace tube in the high-temperature furnace body; S6: After the high temperature furnace body is stable, the furnace tube rotation mechanism is controlled by the furnace tube rotation control area to drive the reaction furnace tube to rotate; S7: After a period of reaction, the gas input is stopped through the gas path control area, the reaction furnace tube rotation is stopped through the furnace tube rotation control area, and the high temperature furnace body is reset through the furnace body movement control area; S8: After the reaction furnace tube is cooled to room temperature, the reaction material is taken out, sieved, and weighed; S9: Calculate the dynamic thermal cracking reaction parameters of the lump ore according to the screening results in S8.

5. The test method of the natural block ore thermal cracking test and evaluation device under simulated blast furnace conditions according to claim 4, characterized in that: The drying temperature in S1 is 105°C ± 1°C, and the drying time is not less than 4 hours.

6. The test method of the natural block ore thermal cracking test and evaluation device under simulated blast furnace conditions according to claim 4, characterized in that: The reaction temperature in S3 is 700°C-1100°C.

7. The test method of the natural block ore thermal cracking test and evaluation device under simulated blast furnace conditions according to claim 4, characterized in that: The gases in S4 are N2 and CO, the N2 flow rate is 10.5 L / min, the CO flow rate is 4.5 L / min, and the total is 15 L / min.

8. The test method of the natural block ore thermal cracking test and evaluation device under simulated blast furnace conditions according to claim 4, characterized in that: The rotation speed of the reaction furnace tube in S6 is 5-30r / min.

9. The test method of the natural block ore thermal cracking test and evaluation device under simulated blast furnace conditions according to claim 4, characterized in that: The S7 reaction time is 30-60 min.

10. The test method of the natural lump ore thermal cracking test and evaluation device under simulated blast furnace conditions according to claim 4, characterized in that: In the S9, the proportion of particles <6.3 mm is used as the thermal cracking index of the lump ore.