A polymer UV absorber for outdoor non-woven fabrics and preparation method thereof
Through the preparation of polymer UV absorbers, the combination of nano-scale titanium dioxide particles and acrylate monomers is used to solve the problem of photoaging of non-woven materials under sunlight, improve their ultraviolet and aging resistance, and extend their use life.
Patent Information
- Application Number
- CN202210248661.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-14
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-03-14
AI Technical Summary
Polymer materials are prone to photoaging under sunlight, resulting in a shortening of service life. The existing UV absorber has insufficient fixation fastness on non-woven fabrics, resulting in insufficient UV resistance time.
The polymer UV absorber consisting of nano-grade titanium dioxide particles, benzophenone light stabilizer, coupling agent, solvent, emulsifier and acrylate monomers are formed through physical modification and free radical polymerization. UV absorber improves bonding with non-woven fabrics.
It improves the UV irradiation resistance and aging resistance of non-woven fabrics, avoids the precipitation problem of small molecule UV absorbers, and extends the service life of the material.
Smart Images

Figure BDA0003545936210000091
Abstract
Description
Technical Field
[0001] The invention relates to the field of polymer materials, in particular to a polymer UV absorber for outdoor non-woven fabrics and a preparation method thereof. Background Art
[0002] Due to their own structure, polymer materials will experience photoaging phenomena such as deterioration of appearance and physical and mechanical performance when exposed to sunlight or strong fluorescence, such as discoloration, loss of gloss, silver streaks, corrosion, cracking, and decreased tensile strength, impact strength, elongation and electrical properties. Although there are significant differences in the photoaging rates of polymers with different structures, all polymer materials that have not been stabilized will experience photoaging when exposed to sunlight, regardless of the presence of oxygen. The ultimate result of photoaging of polymer materials is a shortened service life. For example, if polypropylene products are not stabilized, their outdoor service life is only a few months. This greatly affects the economy and environmental protection of outdoor use of polymer materials and limits their scope of application.
[0003] Outdoor non-woven fabrics are usually made of polymer materials through melt-blowing or other spinning processes. However, outdoor non-woven fabrics are exposed to ultraviolet rays for a long time and have a short aging resistance time. The current mainstream UV absorbers such as UV234, UV944, and UV770 are added to the finishing liquid and fixed on the surface of the non-woven fabric through post-finishing. However, due to their low degree of polymerization, there will be problems with insufficient fixation fastness. If these UV absorbers are directly added to polymer spinning, there will also be a risk of precipitation, resulting in insufficient UV resistance time. Summary of the invention
[0004] In order to overcome the shortcomings of the low polymerization degree and small molecular weight of UV absorbers in the prior art, the present invention provides a polymer UV absorber for outdoor non-woven fabrics and a preparation method thereof. The inventors of the present application have experimentally demonstrated that the polymer UV absorber for outdoor non-woven fabrics described in the present invention can effectively improve the precipitation problem of the ultraviolet UV absorber, improve the binding property of the ultraviolet UV absorber with the surface of the non-woven fabric, and further improve the long-term ultraviolet radiation resistance and aging resistance of the non-woven fabric material.
[0005] To achieve the above-mentioned purpose, the present invention provides the following technical solution: a polymer UV absorber for outdoor non-woven fabrics, wherein the raw materials for preparing the polymer UV absorber include the following components in parts by weight:
[0006] 10-25 parts of nano-sized titanium dioxide particles;
[0007] 5-8 parts of benzophenone light stabilizer;
[0008] Coupling agent 0.2-1 part;
[0009] 70-90 parts of solvent;
[0010] 10-15 parts of emulsifier;
[0011] 2 to 5 parts of initiator;
[0012] And 10 to 15 parts of acrylic acid ester monomer.
[0013] As a preferred technical solution of the present invention, the coupling agent contains at least one group selected from the group consisting of vinyl, allyl, acryloyloxy or methacryloyloxy.
[0014] As a preferred technical solution of the present invention, the coupling agent is selected from one or more of a silane coupling agent, a titanate coupling agent or an aluminate coupling agent.
[0015] As a preferred technical solution of the present invention, the coupling agent is selected from one or more of vinyl triethoxy silane or acryloxypropyl trimethoxy silane.
[0016] As a preferred technical solution of the present invention, the solvent is a mixture of ethanol and deionized water.
[0017] As a preferred technical solution of the present invention, the ethanol and deionized water are mixed in a volume ratio of 0.9-0.95:0.05-0.1.
[0018] As a preferred technical solution of the present invention, the emulsifier is one or more of dodecyl ammonium chloride, sodium dodecyl sulfate or sodium dodecylbenzene sulfonate.
[0019] As a preferred technical solution of the present invention, the benzophenone light stabilizer is selected from one or more of 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-n-octyloxybenzophenone, 2-hydroxy-4-dodecyloxybenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxy-2'-carboxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone or 2-hydroxy-4-methoxy-5-sulfonic acidbenzophenone.
[0020] The invention also provides a method for preparing the polymer UV absorber for outdoor non-woven fabrics.
[0021] The method for preparing the polymer UV absorber of the present invention comprises the following preparation steps:
[0022] S1: First, physically modify the nano-sized titanium dioxide particles:
[0023] (1) Place nano-sized titanium dioxide particles, a coupling agent, and a benzophenone-based light stabilizer in a reaction tank containing a solvent, heat to 50 to 80° C., and stir for 1 to 3 hours;
[0024] (2) cooling, drying, and crushing to obtain modified nano-sized titanium dioxide particles;
[0025] S2: Mixing the modified nano-sized titanium dioxide particles, the emulsifier and the deionized water and stirring for 40 to 50 minutes, and then placing them in an ultrasonic environment and dispersing them for 15 to 30 minutes;
[0026] S3: placing the solution after step S2 in a reaction tank, protecting it with nitrogen, heating it to 60-70°C, adding a reaction initiator thereto, mixing it for 0.3-0.5h, adding an acrylate monomer, reacting it for 2-3h, cooling it to room temperature and discharging it, filtering it, and drying it to obtain the polymer UV absorber of the present invention.
[0027] As a preferred technical solution of the present invention, the acrylic acid ester monomer includes one or more of methyl acrylate, ethyl acrylate, methyl 2-methacrylate or ethyl 2-methacrylate.
[0028] As a preferred technical solution of the present invention, in the step S2, the modified nano-sized titanium dioxide particles, the emulsifier and 10-15 parts by weight of deionized water are mixed.
[0029] As a preferred technical solution of the present invention, in the step S3, the acrylic acid ester monomer is added into the reaction tank in 3 to 5 times, with a time interval of 0.5 to 1 hour each time.
[0030] Compared with the prior art, the present invention can achieve the following beneficial effects:
[0031] 1. The polymer UV absorber for outdoor non-woven fabrics of the present invention is prepared by surface-modifying titanium dioxide particles with a silane coupling agent, and at the same time, part of the silane coupling agent reacts with a benzophenone light stabilizer to form surface-modified nano titanium dioxide; and then, by free radical polymerization, a polyacrylate structure is further connected to the surface of the modified titanium dioxide to obtain the polymer UV absorber for outdoor non-woven fabrics of the present invention. Compared with the existing UV absorbers, the polymer UV absorber has a larger molecular weight and a higher degree of polymerization. The polymer chain segments can be more tightly combined with the non-woven fabric fibers through physical intertwining or intermolecular forces, and the precipitation problem of the existing small molecule UV absorbers is avoided.
[0032] 2. The preparation method of the present invention prolongs the reaction time by adding acrylic acid ester monomers in batches, so that the internal chemical reaction can react sufficiently to obtain a pure product. DETAILED DESCRIPTION
[0033] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below in conjunction with specific embodiments, but the following embodiments are only preferred embodiments of the present invention, not all. Based on the embodiments in the implementation mode, other embodiments obtained by those skilled in the art without creative work all belong to the protection scope of the present invention. The experimental methods in the following embodiments, unless otherwise specified, are conventional methods, and the materials, reagents, etc. used in the following embodiments, unless otherwise specified, can all be obtained from commercial channels.
[0034] The method of the present invention is further described below by way of examples:
[0035] Example 1
[0036] A polymer UV absorber for outdoor non-woven fabrics comprises the following raw materials in parts by weight: 10 parts of nano-sized titanium dioxide particles, 5 parts of 2,4-dihydroxybenzophenone, 0.2 parts of vinyl triethoxysilane, 70 parts of solvent (the volume ratio of ethanol to deionized water is 0.93:0.07), 10 parts of dodecyl ammonium chloride, 10 parts of ethyl acrylate, and 2 parts of ammonium persulfate (initiator).
[0037] The preparation method is as follows:
[0038] S1: First, physically modify the nano-sized titanium dioxide particles:
[0039] (1) placing nano-sized titanium dioxide particles, vinyl triethoxysilane, and 2,4-dihydroxybenzophenone in a reaction tank containing a solvent (a mixture of ethanol and deionized water in a volume ratio of 0.93:0.07), heating at 70° C. for 2 h, and uniformly stirring;
[0040] (2) cooling, drying, and crushing to obtain modified nano-sized titanium dioxide particles;
[0041] S2: The modified nano-sized titanium dioxide particles, dodecyl ammonium chloride and 10 parts by weight of deionized water were fully stirred for 4 minutes, and dispersed in an ultrasonic environment for 15 minutes;
[0042] S3: placing the solution after step S2 in a reaction tank, protecting it with nitrogen, heating it to 60°C, adding a reaction initiator thereto, reacting for 0.5h, then adding ethyl acrylate in 5 times, each time with an interval of 0.5h. After complete addition, reacting for 2.5h, cooling to room temperature and discharging the material, filtering and drying to obtain the polymer UV absorber for outdoor non-woven fabrics.
[0043] Example 2
[0044] A polymer UV absorber for outdoor non-woven fabrics comprises the following raw materials in parts by weight: 25 parts of nano-sized titanium dioxide particles, 8 parts of 2-hydroxy-4-dodecyloxybenzophenone, 1 part of acryloxypropyltrimethoxysilane, 90 parts of solvent (ethanol and deionized water are mixed at a ratio of 0.95:0.05), 10 parts of sodium dodecyl sulfate, 5 parts of ammonium persulfate (initiator), and 15 parts of 2-methyl methacrylate.
[0045] The preparation method is as follows:
[0046] S1: First, physically modify the nano-sized titanium dioxide particles:
[0047] (1) placing nano-sized titanium dioxide particles, acryloxypropyltrimethoxysilane, and 2,4-dihydroxybenzophenone in a reaction tank containing a solvent (a mixture of ethanol and deionized water in a volume ratio of 0.95:0.05), heating to 80° C. for 2 h, and uniformly stirring;
[0048] (2) cooling, drying, and crushing to obtain modified nano-sized titanium dioxide particles;
[0049] S2: fully stirring the modified nano-sized titanium dioxide particles, sodium dodecyl sulfate and 15 parts by weight of water for 4 minutes, and dispersing them under an ultrasonic environment for 15 minutes;
[0050] S3: placing the solution after step S2 in a reaction tank, protecting it with nitrogen, heating it to 60°C, adding a reaction initiator thereto, reacting for 0.5h, then adding ethyl acrylate in 4 times, each time with an interval of 0.5h. After complete addition, reacting for 2.5h, cooling to room temperature and discharging the material, filtering and drying to obtain the polymer UV absorber for outdoor non-woven fabrics.
[0051] Example 3
[0052] A high molecular UV absorber for outdoor non-woven fabrics comprises the following raw materials in parts by weight: 18 parts of nano-sized titanium dioxide particles, 6 parts of 2-hydroxy-4-methoxy-5-sulfonic acid benzophenone, 0.8 parts of acryloxypropyltrimethoxysilane, 80 parts of solvent (ethanol and deionized water are mixed at a ratio of 0.95:0.05), 13 parts of sodium dodecyl sulfate, parts of ammonium persulfate (initiator), and 13 parts of 2-methyl methacrylate.
[0053] The preparation method is as follows:
[0054] S1: First, physically modify the nano-sized titanium dioxide particles:
[0055] (1) placing nano-sized titanium dioxide particles, acryloxypropyltrimethoxysilane, and 2-hydroxy-4-methoxy-5-sulfonic acid benzophenone in a reaction tank containing a solvent (ethanol and deionized water mixed in a volume ratio of 0.95:0.05), heating to 80° C. for 2 h, and uniformly stirring;
[0056] (2) cooling, drying, and crushing to obtain modified nano-sized titanium dioxide particles;
[0057] S2: The modified nano-sized titanium dioxide particles, sodium dodecyl sulfate and 15 parts by weight of deionized water were fully stirred for 4 minutes, and dispersed in an ultrasonic environment for 15 minutes;
[0058] S3: placing the solution after step S2 in a reaction tank, protecting it with nitrogen, heating it to 60°C, adding a reaction initiator thereto, reacting for 0.5h, then adding 2-methyl methacrylate in 3 times, each time with an interval of 0.5h. After complete addition, reacting for 2.5h, cooling to room temperature and discharging the material, filtering and drying to obtain the polymer UV absorber for outdoor non-woven fabrics.
[0059] Comparative Example 1
[0060] Compared with Example 1, the polymerization of the acrylic ester monomers was not performed.
[0061] Comparative Example 2
[0062] Compared with Example 1, the acrylic acid ester monomers are directly added at one time for polymerization.
[0063] Comparative Example 3
[0064] The same amount of nano-titanium dioxide and 2-hydroxy-4-dodecyloxybenzophenone as in Example 1 were directly used without surface modification.
[0065] Application of Examples 1-3 and Comparative Examples 1-3:
[0066] Commercially available masks were used as non-woven fabric substrates for testing (Anhui Leisheng Medical Supplies Technology Co., Ltd., polypropylene, spunbond, 30 g / m 2 ). Prepare 6 parts of polyvinyl alcohol solution with a concentration of 5wt%, add 1wt% of UV absorber prepared in Examples 1-3 and Comparative Examples 1-3 respectively, mix well and apply the solution to non-woven fabric substrates respectively, dry naturally and further dry under vacuum. Each dried sample is placed in an aging test chamber for UV aging test (temperature 25°C, irradiation intensity 75W / m 2, irradiation distance 50mm, irradiation time 12h). Each sample before and after the test was subjected to mechanical property test (breaking strength, breaking elongation) according to the standard "GB / T 24218.3-2010 Textile nonwoven fabric test method Part 3: Determination of breaking strength and breaking elongation (strip method)". The specific experimental data are shown in Table 1.
[0067] Table 1
[0068]
[0069] As shown in Table 1, the breaking strength and breaking elongation of the products of Examples 1-3 are significantly improved compared with those of Comparative Examples 1-3. After 12 hours of ultraviolet irradiation, the breaking strength is reduced by less than 2% and the breaking elongation is reduced by less than 5%, while the breaking strength of Comparative Examples 1-3 is 10%-40% and the breaking elongation is 13-40%. It can be seen that the polymer UV absorber for outdoor non-woven fabrics of the present invention is better combined with the non-woven fabrics by introducing the coupling agent selected by the present invention into the polyacrylate polymer chain segment, thereby improving the long-term ultraviolet irradiation resistance and aging resistance of the non-woven fabric material.
[0070] In the actual production process, similar effects can be obtained by adjusting within the specified metering range, which is suitable for different use environments.
[0071] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only preferred examples of the present invention and are not intended to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for preparing a polymer UV absorber for outdoor non-woven fabrics, characterized in that: The method comprises the following preparation steps: S1: First, physically modify the nano-sized titanium dioxide particles: (1) Place nano-sized titanium dioxide particles, coupling agent, and benzophenone light stabilizer in a reaction tank containing a solvent, heat to 50-80°C, and stir for 1-3 hours; (2) cooling, drying, and crushing to obtain modified nano-sized titanium dioxide particles; S2: Mix the modified nano-sized titanium dioxide particles, emulsifier and deionized water and stir for 40 to 50 minutes, then place in an ultrasonic environment and disperse for 15 to 30 minutes; S3: placing the solution after step S2 in a reaction tank, protecting it with nitrogen, heating it to 60-70° C., adding a reaction initiator thereto, mixing it for 0.3-0.5 h, adding an acrylic acid ester monomer, reacting it for 2-3 h, cooling it to room temperature, discharging it, filtering it, and drying it to obtain the polymer UV absorber; In the step S2, the modified nano-sized titanium dioxide particles, the emulsifier and 10-15 parts by weight of deionized water are mixed; In the step S3, the acrylic acid ester monomer is added into the reaction tank in 3 to 5 times, with a time interval of 0.5 to 1 hour each time; The weight proportions of the components are as follows: 10-25 parts of nano-sized titanium dioxide particles, 5-8 parts of benzophenone light stabilizer, 0.2-1 parts of coupling agent, 70-90 parts of solvent, 10-15 parts of emulsifier, 2-5 parts of initiator, and 10-15 parts of acrylate monomer; The solvent is a mixture of ethanol and deionized water; The ethanol and deionized water are mixed in a volume ratio of 0.9-0.95:0.05-0.1; The benzophenone light stabilizer is selected from one or more of 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-octyloxybenzophenone, 2-hydroxy-4-dodecyloxybenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxy-2'-carboxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone or 2-hydroxy-4-methoxy-5-sulfonic acidbenzophenone.
2. The method for preparing a polymer UV absorber according to claim 1, characterized in that: The coupling agent contains at least one group selected from the group consisting of vinyl, allyl, acryloxy, and methacryloyloxy.
3. The method for preparing a polymer UV absorber according to claim 1, characterized in that: The emulsifier is selected from one or more of dodecyl ammonium chloride, sodium dodecyl sulfate or sodium dodecylbenzene sulfonate.
4. The method for preparing a polymer UV absorber according to claim 1, characterized in that: The acrylic acid ester monomer includes one or more of methyl acrylate, ethyl acrylate, 2-methyl methacrylate or 2-ethyl methacrylate.