Tundish for low carbon high sulfur free cutting steel 1215

By using high-density prefabricated parts and slag-blocking prefabricated parts in the steel-receiving part of the tundish, the problem of erosion of the working layer of the tundish in the production of low-carbon, high-sulfur free-cutting steel 1215 is solved, the service life is extended and the casting quality is improved. billet quality and caster stability.

CN114749648BActive Publication Date: 2024-10-18SGIS SONGSHAN CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202210491752.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-07
Publication Date
2024-10-18
Estimated Expiration
2042-05-07

AI Technical Summary

Technical Problem

When producing low-carbon, high-sulfur free-cutting steel 1215, the working layer of the tundish is severely eroded by molten steel and ladle slag, resulting in a short service life and affecting the safety of the continuous casting machine and the quality control of the cast slab.

Method used

In the steel-receiving part of the tundish, a first prefabricated part with a higher volume density is installed to replace the working layer to increase density, reduce gaps and porosity, and improve corrosion resistance, and a second prefabricated part is set in the steel-receiving part to block slag. and changing the flow of steel.

Benefits of technology

It effectively extends the service life of the tundish, improves corrosion resistance, avoids contamination of molten steel and plug rod adhesion, improves the stability of mold liquid level control, and can support the safety and stable production of continuous casting machines and the quality of cast slabs. control.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114749648B_ABST
    Figure CN114749648B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of steel smelting, and in particular to a tundish for low-carbon high-sulfur free-cutting steel 1215, comprising: a working area and a steel receiving part arranged in the working area; the working area comprises a first insulation layer, a first permanent layer and a working layer stacked in sequence from the outside to the inside; the steel receiving part comprises a second insulation layer, a second permanent layer and a first prefabricated part stacked in sequence from the outside to the inside, the second insulation layer is connected to the first insulation layer, the first permanent layer is connected to the second permanent layer, and the working layer is connected to the first prefabricated part, wherein the volume density of the first prefabricated part is greater than the volume density of the working layer. The tundish of the present invention can extend the service life of the tundish when producing low-carbon high-sulfur free-cutting steel 1215, and improve the risk issues of safe and stable production of continuous casting machines and quality control of ingots.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel smelting, and in particular to a tundish for low-carbon high-sulfur free-cutting steel 1215. Background Art

[0002] The tundish is a refractory container used in steelmaking. It is one of the key equipment in the continuous casting process. It plays a very important role in the smooth operation of continuous casting and ensuring the quality of molten steel. The tundish has the functions of stabilizing flow, diverting flow, reducing pressure, protecting molten steel, and removing molten steel inclusions. Usually, the refractory lining of the tundish mainly includes an insulating layer, a permanent layer, and a working layer. Among them, the working layer will contact the molten steel and is the key part of the lining of the tundish. The working layer generally uses magnesium dry material or coating material. During the use of the tundish, the working layer is always eroded by molten steel and ladle slag. The speed of erosion of the working layer directly affects the service life of the tundish.

[0003] Related technologies When producing low-carbon, high-sulfur free-cutting steel 1215, the free oxygen in the molten steel is as high as 50ppm or more, the basicity of the ladle slag is low, and the Tfe and MnO in the slag are high, which seriously erodes the working layer. When the tundish is continuously cast, the working layer is severely eroded, which has a serious adverse effect on the service life of the tundish, and brings great risks to the safe and stable production of the continuous casting machine and the quality control of the ingot. Summary of the invention

[0004] The present invention provides a tundish for low-carbon high-sulfur free-cutting steel 1215, which can extend the service life of the tundish when producing low-carbon high-sulfur free-cutting steel 1215, and improve the risk issues of safe and stable production of a continuous casting machine and quality control of ingots.

[0005] The embodiments of the present invention can be implemented as follows:

[0006] The present invention provides a tundish for low-carbon high-sulfur free-cutting steel 1215, comprising: a working area and a steel receiving part arranged in the working area;

[0007] The working area includes a first heat-insulating layer, a first permanent layer and a working layer which are stacked in sequence from outside to inside;

[0008] The steel-bearing part includes a second insulation layer, a second permanent layer and a first prefabricated part which are stacked in sequence from the outside to the inside, the second insulation layer is connected to the first insulation layer, the first permanent layer is connected to the second permanent layer, and the working layer is connected to the first prefabricated part, wherein the volume density of the first prefabricated part is greater than the volume density of the working layer.

[0009] In an optional embodiment, the steel receiving part also includes a second prefabricated part, which is spaced apart from and relatively distributed to the first prefabricated part, and a steel receiving area is formed between the first prefabricated part and the second prefabricated part; the volume density of the second prefabricated part is greater than the volume density of the working layer.

[0010] In an optional embodiment, in terms of percentage, the total content of Al2O3 and MgO in the raw materials for preparing at least one of the first preform and the second preform is greater than or equal to 80%, and the content of SiO2 is less than or equal to 5.0%;

[0011] The total content of Al2O3 and MgO in the raw materials for preparing the working layer is greater than or equal to 55%, and the content of SiO2 is less than or equal to 20.0%.

[0012] In an optional embodiment, the volume density of at least one of the first preform and the second preform under the condition of 200°C×3h is: ≥2.85g / cm 3 , at 1500℃×3h: 2.65±0.20g / cm 3 ;

[0013] The volume density of the working layer at 200℃×3h is: ≥2.05g / cm 3 , at 1500℃×3h: 1.85±0.20g / cm 3 .

[0014] In an optional embodiment, the second prefabricated member includes a fourth prefabricated panel, a fifth prefabricated panel and a sixth prefabricated panel connected in sequence at an angle, and the angle between the fourth prefabricated panel and the fifth prefabricated panel, and the angle between the fifth prefabricated panel and the sixth prefabricated panel are greater than 90°.

[0015] In an optional embodiment, the included angle between the fourth prefabricated board and the fifth prefabricated board, and the included angle between the fifth prefabricated board and the sixth prefabricated board are 136°.

[0016] In an optional embodiment, the fourth precast plate and the sixth precast plate are each provided with two molten steel circulation holes.

[0017] In an optional embodiment, one of the molten steel circulation holes opened in the fourth prefabricated plate is 100 mm away from the bottom of the second prefabricated part, and the other molten steel circulation hole opened in the fourth prefabricated plate is located 50 mm below the 1 / 2 height of the second prefabricated part.

[0018] In an optional embodiment, the diameter of the molten steel circulation hole is 100 mm.

[0019] In an optional embodiment, the first prefabricated member includes a first prefabricated panel, a second prefabricated panel and a third prefabricated panel connected in sequence at an angle, and the angle between the first prefabricated panel and the second prefabricated panel, and the angle between the second prefabricated panel and the third prefabricated panel are greater than 90°.

[0020] The beneficial effects of the embodiments of the present invention include:

[0021] The low-carbon high-sulfur free-cutting steel 1215 provided in the embodiment of the present invention uses a first preform with a larger volume density in the inner layer of the steel receiving part of the tundish to replace the working layer provided in the steel receiving part. The larger volume density of the first preform can increase its density, reduce the gaps in the first preform, and reduce the porosity, so that the corrosion resistance of the first preform is enhanced. Furthermore, when the low-carbon high-sulfur free-cutting steel 1215 is used, the erosion of the first preform by molten steel and ladle slag can be effectively slowed down, so as to extend the service life of the first preform, thereby extending the service life of the tundish, which is beneficial to improving the risk of safe and stable production of the continuous casting machine and quality control of the castings. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0023] Figure 1 This is a schematic diagram of the structure of a tundish for low-carbon, high-sulfur free-cutting steel 1215 in an embodiment of the present invention;

[0024] Figure 2 is a schematic structural diagram of a first prefabricated component in an embodiment of the present invention;

[0025] Figure 3 Schematic diagram of the structure of the second prefabricated component in an embodiment of the present invention.

[0026] Icons: 010- tundish; 100- working area; 101- stopper hole; 110- first insulation layer; 120- first permanent layer; 130- working layer; 200- steel-bearing part; 210- second insulation layer; 220- second permanent layer; 230- first prefabricated part; 231- first prefabricated plate; 232- second prefabricated plate; 233- third prefabricated plate; 240- second prefabricated part; 241- fourth prefabricated plate; 242- fifth prefabricated plate; 243- sixth prefabricated plate; 244- molten steel circulation hole. DETAILED DESCRIPTION

[0027] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.

[0028] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.

[0030] In the description of the present invention, it should be noted that if the terms "inside" or "outside" appear to indicate an orientation or position relationship, it is based on the orientation or position relationship shown in the accompanying drawings, or is the orientation or position relationship in which the product of the invention is usually placed when in use. This is only for the convenience of describing the present invention and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation. Therefore, it cannot be understood as a limitation on the present invention.

[0031] In addition, the terms “first”, “second”, etc., if used, are merely used to distinguish between the descriptions and should not be understood as indicating or implying relative importance.

[0032] It should be noted that, in the absence of conflict, the features in the embodiments of the present invention may be combined with each other.

[0033] Please refer to Figure 1 The present embodiment provides a tundish for low-carbon high-sulfur free-cutting steel 1215 (hereinafter referred to as tundish 010), which includes: a working area 100 and a steel receiving part 200 arranged in the working area 100; the working area 100 includes a first insulation layer 110, a first permanent layer 120 and a working layer 130 stacked in sequence from the outside to the inside; the steel receiving part 200 includes a second insulation layer 210, a second permanent layer 220 and a first prefabricated part 230 stacked in sequence from the outside to the inside, the second insulation layer 210 is connected to the first insulation layer 110, the first permanent layer 120 is connected to the second permanent layer 220, and the working layer 130 is connected to the first prefabricated part 230, wherein the volume density of the first prefabricated part 230 is greater than the volume density of the working layer 130.

[0034] A first preform 230 with a larger volume density is arranged in the inner layer of the steel receiving part 200 instead of arranging a working layer 130 in the steel receiving part 200. The larger volume density of the first preform 230 can increase its density, reduce the gaps in the first preform 230, and reduce the porosity, so that the corrosion resistance of the first preform 230 is enhanced, and then when low-carbon and high-sulfur free-cutting steel 1215 is used, the erosion of the first preform 230 by molten steel and ladle slag can be effectively slowed down, so as to extend the service life of the first preform 230, thereby extending the service life of the ladle 010, which is beneficial to improving the risk of safety, stable production and quality control of the casting for the continuous casting machine.

[0035] It should be noted that in the related art, the steel receiving part is provided with a working layer identical to the working area. In order to improve the problem that the working layer of the steel receiving part is easily corroded, the method of increasing the MgO content of the slag line of the working layer of the steel receiving part and increasing the thickness of the working layer of the steel receiving part is adopted. However, the above method does not significantly improve the effect. When producing low-carbon, high-sulfur free-cutting steel 1215, the number of continuous casting furnaces can be increased from 8 furnaces (using time 6h) to 10 furnaces, which cannot meet the continuous production of 16 furnaces (using time 12h). Moreover, the working layer is severely corroded during the later casting, and the corroded refractory will be drawn into the molten steel, causing the molten steel to be contaminated; the ladle slag is distributed throughout the tundish, which easily causes the stopper rod to stick to the ladle slag, affecting the stability of the crystallizer liquid level control. The tundish 010 provided in this embodiment can effectively improve the corrosion resistance by arranging a first preform 230 with a larger volume density in the steel receiving part 200 to replace the working layer 130. It can not only realize continuous casting of 16 furnaces (using time 12 hours), but also avoid the corrosion of refractory materials from being drawn into the molten steel, causing the molten steel to be contaminated, and it is not easy to cause the stopper rod to stick to the ladle slag, thereby improving the impact on the stability of the crystallizer liquid level control.

[0036] Furthermore, by replacing the working layer 130 with the first preform 230 having a larger volume density, rather than setting the working layer 130 in the steel receiving part 200 and then adding the first preform 230 on the inner side of the working layer 130, the space occupied by the first preform 230 in the steel receiving part 200 can be reduced, the volume of the steel receiving part 200 can be increased, and inclusions can be helped to float up; and directly replacing the working layer 130 of the steel receiving part 200 with the first preform 230 can ensure the assembly stability of the first preform 230 and reduce the possibility of the first preform 230 being separated from its assembly position.

[0037] It should also be noted that the working area 100 is provided with a stopper rod hole 101 for arranging a stopper rod.

[0038] Please refer to Figure 2The first prefabricated member 230 includes a first prefabricated panel 231, a second prefabricated panel 232 and a third prefabricated panel 233 which are connected in sequence at an angle, and the angle between the first prefabricated panel 231 and the second prefabricated panel 232, and the angle between the second prefabricated panel 232 and the third prefabricated panel 233 are greater than 90°, for example: 91°, 95°, 120°, 140°, etc.

[0039] Please refer to Figure 1 and Figure 2 Furthermore, the second insulation layer 210, the second permanent layer 220 and the first prefabricated part 230 of the steel receiving part 200 are stacked in sequence and closely fitted, that is, the shapes of the second insulation layer 210 and the second permanent layer 220 are adapted to the first prefabricated part 230. In this way, the steel receiving part 200 has an angle greater than 90°, which can reduce the flow rate of molten steel at the corner, facilitate the production operation of the large ladle long nozzle, and reduce the erosion of the refractory by the steel flow in the steel receiving area.

[0040] In order to protect the second permanent layer 220 of the steel receiving part 200 from corrosion, the height and angle of the first prefabricated part 230 are consistent with the height and angle of the inner cavity of the steel receiving part 200 , and the first prefabricated part 230 fits tightly with the second permanent layer 220 .

[0041] The working area 100 of this embodiment is roughly rectangular, and the first insulation layer 110, the first permanent layer 120 and the working layer 130 are all rectangular frame structures with openings. The two ends of the second insulation layer 210 are respectively connected to the two sides of the opening of the first insulation layer 110, the two ends of the second permanent layer 220 are respectively connected to the two sides of the opening of the first permanent layer 120, and the two ends of the first prefabricated part 230 are respectively connected to the two sides of the opening of the working layer 130, that is, the end of the first prefabricated plate 231 away from the second prefabricated plate 232 and the end of the third prefabricated plate 233 away from the second prefabricated plate 232 are respectively connected to the two sides of the opening of the working layer 130.

[0042] Please refer to Figure 1 In this embodiment, the steel receiving part 200 further includes a second preform 240, which is spaced apart from and relatively distributed with the first preform 230, and a steel receiving area is formed between the first preform 230 and the second preform 240; the volume density of the second preform 240 is greater than the volume density of the working layer 130. The second preform 240 can be used as a slag blocking preform, which can play a role of slag blocking, that is, effectively preventing the ladle slag from flowing into the working area 100 of the tundish 010, preventing the ladle slag from corroding the working layer 130 of the working area 100, and preventing the stopper rod set in the stopper rod hole 101 from being bonded.

[0043] In order to ensure the installation stability of the second preform 240 and effectively prevent the ladle slag from crossing the second preform 240 and entering the working area 100, the height of the second preform 240 is consistent with the height of the inner cavity of the steel receiving part 200, that is, the height of the second preform 240, the first preform 230 and the steel receiving area are consistent.

[0044] Optionally, the upper edge of the second preform 240 contacts the cover of the tundish 010, so that the cover of the tundish 010 can press the second preform 240, so as to ensure the assembly stability of the second preform 240 by using the cover of the tundish 010, that is, the second preform 240 is fixed by using the cover of the tundish 010, which can prevent the second preform 240 from being tilted due to the static pressure of the molten steel when pouring begins, thereby ensuring stable and reliable operation.

[0045] Please refer to Figure 3 The second prefabricated member 240 includes a fourth prefabricated plate 241, a fifth prefabricated plate 242 and a sixth prefabricated plate 243 which are connected in sequence at an angle, and the angle between the fourth prefabricated plate 241 and the fifth prefabricated plate 242, and the angle between the fifth prefabricated plate 242 and the sixth prefabricated plate 243 are greater than 90°, for example: 91°, 95°, 120°, 140°, etc. Such an arrangement can reduce the erosion of the second prefabricated member 240 by the molten steel.

[0046] It should be noted that the first prefabricated member 230 and the second prefabricated member 240 may be roughly arranged in a trapezoidal shape, so that the steel receiving area therebetween is roughly in a hexagonal shape.

[0047] It is also necessary to note that please refer to Figure 1-Figure 3 The fifth precast plate 242 is opposite to the second precast plate 232 and is spaced apart from each other. One end of the first precast plate 231 away from the second precast plate 232 is connected at an angle to one end of the fourth precast plate 241 away from the fifth precast plate 242. One end of the third precast plate 233 away from the second precast plate 232 is connected at an angle to one end of the sixth precast plate 243 away from the fifth precast plate 242, so that the cavity in the steel receiving area is roughly hexagonal.

[0048] Please continue to refer to Figure 3 The fourth precast plate 241 and the sixth precast plate 243 are both provided with two molten steel circulation holes 244, so that the molten steel can enter the working area 100 from the steel receiving area through the molten steel circulation holes 244; moreover, the molten steel circulation holes 244 are both provided on the fourth precast plate 241 and the sixth precast plate 243, so that both sides of the second precast part 240 have molten steel circulation holes 244. Such a setting can also change the molten steel flow field, avoid the molten steel from directly impacting the stopper rod set in the stopper rod hole 101, and improve the stability of the stopper rod.

[0049] In order to ensure a good slag blocking effect of the second preform 240 , the molten steel flow hole 244 can be arranged below the height center line of the second preform 240 , that is, the molten steel flow hole 244 can be arranged below 1 / 2 of the height of the second preform 240 .

[0050] The molten steel flow holes 244 of the fourth precast plate 241 and the sixth precast plate 243 can be symmetrically distributed; the following only describes the position of the molten steel flow holes 244 of the fourth precast plate 241. One of the molten steel flow holes 244 opened in the fourth precast plate 241 is 100mm away from the bottom of the second precast part 240, and the other molten steel flow hole 244 opened in the fourth precast plate 241 is located 50mm below the 1 / 2 height of the second precast part 240. During the ladle transfer process, the liquid level of the molten steel in the tundish 010 will drop by 1 / 3 to 1 / 2. Setting the molten steel flow hole 244 at the above position can ensure that the position of the slag is not lower than the molten steel flow hole 244 during the transfer, so as to facilitate the molten steel to be below the height center line of the second precast part 240 to achieve a good slag blocking effect.

[0051] It should be noted that one of the molten steel circulation holes 244 is opened at a position 100 mm away from the bottom of the fourth precast plate 241, which can ensure that the molten steel will not be accumulated in the steel receiving area, that is, to avoid a large amount of molten steel being accumulated in the steel receiving area when the casting is stopped. The other molten steel circulation hole 244 is set at 50 mm below the 1 / 2 height of the fourth precast plate 241. When the liquid level of the molten steel in the middle ladle 010 drops during the ladle transfer casting process, it can effectively ensure that the position of the slag is not lower than the molten steel circulation hole 244, thereby effectively blocking the slag.

[0052] In order to reduce the effect of the static pressure of the molten steel, the aperture of the molten steel circulation hole 244 can be increased as much as possible; at the same time, it is also necessary to consider the influence of the diameter of the molten steel circulation hole 244 on the strength of the second preform 240; in a preferred embodiment, the aperture of the molten steel circulation hole 244 is 100 mm.

[0053] Optionally, in some embodiments, the center of the molten steel flow hole 244 should avoid directly corresponding to the stopper rod set in the stopper rod hole 101, and the bending angle of the second prefabricated member 240 can be 136°, that is, the angle between the fourth prefabricated plate 241 and the fifth prefabricated plate 242, and the angle between the fifth prefabricated plate 242 and the sixth prefabricated plate 243 can be 136°.

[0054] Optionally, in order to reduce turbulence in the steel receiving area, the cavity in the steel receiving area can be set as large as possible; therefore, in some embodiments, please refer to Figure 1, the second preform 240 can be extended to the side away from the first preform 230. Specifically, the lengths of the fourth preform 241 and the sixth preform 243 can be extended as much as possible; however, it is necessary to ensure that the distance between the fifth preform 242 of the second preform 240 and the stopper rod arranged in the stopper rod hole 101 is greater than or equal to the distance between the stopper rod and the working layer 130 opposite to the fifth preform 242.

[0055] Optionally, the thickness of the first preform 230 and the second preform 240 can be maintained consistent with the thickness of the working layer 130 at 60 mm due to the influence of the mold.

[0056] In order to ensure that the volume density of the first preform 230 is greater than the volume density of the working layer 130; the first preform 230 is a special magnesium preform formed by integral casting, and the working layer 130 is a magnesium dry material or coating material. The physical and chemical indicators of the special magnesium preform are shown in Table 1, and the physical and chemical indicators of the magnesium dry material or coating material are shown in Table 2.

[0057] Table 1 Physical and chemical indicators of special magnesium prefabricated parts

[0058]

[0059] Table 2 Magnesium dry material or coating material

[0060]

[0061] According to the inventor's research and analysis, the steel slag of low-carbon, high-sulfur free-cutting steel 1215 contains SiO215-25%, FeO2-8%, and MnO 6-20%, which is much higher than the steel slag of other types of steel containing SiO25-10%, FeO 0-2%, and MnO 0-4%. As the MnO / FeO ratio of the slag increases, the reaction between [O] in the slag and C / Al in the refractory material is accelerated, thereby significantly accelerating the erosion rate of the refractory material.

[0062] SiO2-MnO-FeO and A12O3 in the 1215 steel slag can easily form MnO-SiO2-A12O3 liquid oxide, which can easily corrode the refractory material; SiO2-MnO-FeO reacts with Al2O3+MgO to form MgAl2O4, MnAl2O4 spinel phase in solid state, which can adhere to the surface of the refractory material to prevent the steel slag from further corroding the refractory material. Therefore, the working layer 130 and the prefabricated parts select spinel Al2O3+MgO as the main component, instead of using the simple Al2O3-C as the main component commonly used in related technologies.

[0063] The inventors studied the erosion behavior of spinel refractories with different compressive strengths when in contact with high manganese slag; specifically, the fine rod rotation test (FRT) was used to analyze the erosion behavior of spinel refractory samples in 1550°C slag at a rotation speed of 150r / min. Before the fine rod rotation test, the refractory samples with high compressive strength had high bonding strength and low porosity between magnesia-alumina spinel aggregates, and binders could be observed between the aggregates; on the contrary, the samples with lower compressive strength had small pores between various fine-grained magnesia-alumina spinel aggregates and larger magnesia-alumina spinel aggregates, and no binders were observed between the aggregates. After the thin rod rotation test, SEM and EDS were used for analysis. In both groups of samples, at the slag-refractory interface, the refractory dissolved into the slag, resulting in a reduction in the sample radius, and the slag could be further observed to penetrate into the refractory; however, the chemical erosion of the binder and aggregate in the refractory sample with high compressive strength prevented the penetration of the slag, while the slag easily penetrated into the sample with lower compressive strength due to the presence of more pores in the sample with lower compressive strength, without reacting with the refractory. Therefore, the slag prevented the bonding between the aggregates and caused the strength of the refractory to decrease. Therefore, the refractory of the sample with lower compressive strength suddenly broke during the 30-60min thin rod rotation test. The two important differences observed in the sample microstructure, namely the porosity and the presence of a binder between the aggregates, are the reasons for the different corrosion degrees of different samples.

[0064] According to Table 1 and Table 2, it can be seen that the compressive strength and volume density of the special magnesium preform are very different from the magnesium dry material or coating material of the working layer 130. The volume density of the special magnesium preform is improved, the density is increased, the gap is reduced, and the porosity is reduced, which can prevent MnO-SiO2-A12O3 in the slag from penetrating the prefabricated interior, effectively improve the corrosion resistance of the special magnesium preform, that is, improve the corrosion resistance, and can effectively slow down the corrosion of the special magnesium preform by molten steel and ladle slag; in addition, the compressive strength of the special magnesium preform is greatly improved, and MnO-SiO2-A12O3 in the slag can also be prevented from penetrating the prefabricated interior, effectively improving the corrosion resistance of the special magnesium preform, thereby ensuring the working strength, and can prevent the special magnesium preform from collapsing during work, and at the same time, the anti-scouring erosion ability of the special magnesium preform is also improved.

[0065] It should be noted that the increase of SiO2 will reduce the strength of the preform. In order to ensure the strength of the special magnesium preform, the SiO2 content is controlled within 5%.

[0066] In this embodiment, the second preform 240 is also a special magnesium preform formed by integral casting, and its physical and chemical indicators are the same as those of the first preform 230, which will not be described in detail here.

[0067] The physical and chemical indicators of the first permanent layer 120 and the second permanent layer 220 of this embodiment are the same, see Table 3.

[0068] Table 3 Physical and chemical indicators of the first permanent layer 120 and the second permanent layer 220

[0069]

[0070] The assembly process of the tundish 010 of the present embodiment includes: after the first permanent layer 120 and the second permanent layer 220 of the tundish 010 are tied together, when constructing the working layer 130 of the tundish 010, a first prefabricated plate 231 is placed on the steel receiving part 200 to replace the working layer 130 set on the steel receiving part 200, and then the working layer 130 of the working area 100 is constructed, and the gap between the first prefabricated part 230 and the working layer 130 of the working area 100 is filled with magnesium dry material, so that the working layer 130 and the first prefabricated part 230 are connected by the magnesium dry material filling. After the construction of the working layer 130 is completed, the second prefabricated part 240 is placed as required. When installing the second prefabricated part 240, magnesium dry surrounding materials are used to level the bottom. The second prefabricated part 240 is also filled with magnesium surrounding materials on both sides of the contact surface with the bottom and wall of the package, and the dry material is pounded densely with a small hammer. The surrounding material can be made into a right-angled triangle with a side length of 60mm to fix the second prefabricated part 240. This can also make the second prefabricated part 240 easier to disassemble when unpacking, and will not cause adverse effects on the first permanent layer 120 and the second permanent layer 220.

[0071] In summary, the tundish for low-carbon and high-sulfur free-cutting steel 1215 of the present invention can improve the problem that the steel-receiving part 200 is easily corroded, thereby helping to extend the service life of the tundish 010. The service life of the tundish 010 can be increased from an average of 8 furnaces to about 16-25 furnaces; moreover, the reduced corrosion of the steel-receiving area can prevent impurities from entering the molten steel, so as to improve the purity of the molten steel; in addition, the provision of the second preform 240 effectively blocks the diffusion of ladle slag to the working area 100, thereby preventing the stopper rod from sticking. At the same time, the reasonable design of the molten steel flow holes 244 on both sides of the second preform 240 changes the molten steel flow field, thereby preventing the molten steel from directly impacting the stopper rod, and greatly improving the control of the crystallizer liquid level fluctuation.

[0072] The above are only specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the protection scope of the claims.

Claims

1. A tundish for low-carbon, high-sulfur free-cutting steel 1215, characterized in that: include: A working area and a steel receiving portion arranged in the working area; the working area is provided with a stopper rod hole for arranging a stopper rod; The working area includes a first heat-insulating layer, a first permanent layer and a working layer which are stacked in sequence from outside to inside; The steel receiving part comprises a second heat insulating layer, a second permanent layer and a first prefabricated part which are sequentially stacked from outside to inside, the second heat insulating layer is connected to the first heat insulating layer, the first permanent layer is connected to the second permanent layer, and the working layer is connected to the first prefabricated part, wherein the volume density of the first prefabricated part is greater than the volume density of the working layer; The steel receiving part further includes a second prefabricated part, the second prefabricated part is spaced apart from and relatively distributed with the first prefabricated part, and a steel receiving area is formed between the first prefabricated part and the second prefabricated part; the volume density of the second prefabricated part is greater than the volume density of the working layer; The second prefabricated member comprises a fourth prefabricated plate, a fifth prefabricated plate and a sixth prefabricated plate which are sequentially connected at an angle, and the angle between the fourth prefabricated plate and the fifth prefabricated plate, and the angle between the fifth prefabricated plate and the sixth prefabricated plate are greater than 90°; The fourth prefabricated plate and the sixth prefabricated plate are both provided with two molten steel circulation holes, and the diameter of the molten steel circulation holes is 100 mm; One of the molten steel flow holes opened in the fourth prefabricated plate is 100 mm away from the bottom of the second prefabricated part, and the other molten steel flow hole opened in the fourth prefabricated plate is located 50 mm below the 1 / 2 height of the second prefabricated part; The distance between the fifth prefabricated plate and the stopper rod disposed in the stopper rod hole is greater than or equal to the distance between the stopper rod disposed in the stopper rod hole and the working layer at a position opposite to the fifth prefabricated plate; In percentage, the total content of Al2O3 and MgO in the raw materials for preparing at least one of the first preform and the second preform is greater than or equal to 80%, and the content of SiO2 is less than or equal to 5.0%; the total content of Al2O3 and MgO in the raw materials for preparing the working layer is greater than or equal to 55%, and the content of SiO2 is less than or equal to 20.0%; The volume density of at least one of the first preform and the second preform under the condition of 200°C×3h is: ≥2.85g / cm 3 , at 1500℃×3h: 2.65±0.20g / cm 3 ; The volume density of the working layer at 200°C × 3h is: ≥2.05g / cm 3 , at 1500℃×3h: 1.85±0.20g / cm 3 .

2. The tundish for low carbon high sulfur free cutting steel 1215 according to claim 1, characterized in that: The included angle between the fourth prefabricated plate and the fifth prefabricated plate, and the included angle between the fifth prefabricated plate and the sixth prefabricated plate are 136°.

3. The tundish for low carbon high sulfur free cutting steel 1215 according to claim 1, characterized in that: The first prefabricated member includes a first prefabricated plate, a second prefabricated plate and a third prefabricated plate which are sequentially connected at an angle, and an angle between the first prefabricated plate and the second prefabricated plate, and an angle between the second prefabricated plate and the third prefabricated plate are greater than 90°.

Citation Information

Patent Citations

  • Tundish slag blocking wall, impact brick and preparation method thereof

    CN107602141A

  • Long-life tundish

    CN203917892U

  • Integral tundish impact zone prefabricated part

    CN210587148U