Aluminum alloy ingot and method for producing the same

CN114761152BActive Publication Date: 2024-10-25UACJ CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180006960.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-06-25
Filing Date
2021-02-05
Publication Date
2024-10-25
Estimated Expiration
2041-02-05

AI Technical Summary

Technical Problem

Existing aluminum alloy ingots are prone to linear defects during stretching processes such as rolling and extrusion, resulting in deterioration of surface quality.

Method used

By melting TiB2 particles in the molten aluminum alloy, TiB2 agglomerates with an average equivalent circle diameter of 3.0 μm or less and an average circularity of 0.20 or more are formed, which function as heterogeneous nuclei and refine the aluminum matrix phase, Suppresses the generation of linear defects.

Benefits of technology

The grains of the aluminum alloy ingot are fully refined, the frequency of linear defects during stretching processing is reduced, the quality of the final product is improved, and additional manufacturing cost increases are avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114761152B_ABST
    Figure CN114761152B_ABST
Patent Text Reader

Abstract

The aluminum alloy ingot of the present invention comprises an aluminum matrix phase (1); and TiB2 aggregates (2) dispersed in the aluminum matrix phase (1) formed by agglomeration of TiB2 particles (3). The average value of the equivalent circle diameter of the TiB2 aggregates (2) in the state of being exposed from the aluminum matrix phase (1) is 3.0 μm or less, and the average value of the circularity is 0.20 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an aluminum alloy ingot and a method for manufacturing the same. Background Art

[0002] When casting an aluminum alloy to make an ingot, a grain refiner is sometimes added to the molten aluminum alloy in order to refine the grains in the ingot. As the grain refiner, an Al-Ti-B based refiner is used in which a Ti-B (titanium-boron) based compound such as TiB2 is dispersed in a matrix containing aluminum (Patent Document 1).

[0003] When an Al-Ti-B series refiner is dissolved in a molten aluminum alloy, a solid Ti-B series compound is dispersed in the molten aluminum. When the molten aluminum is solidified in this state, the Ti-B series compound functions as a heterogeneous nucleus, and the grains of the aluminum matrix phase can grow starting from the Ti-B series compound. As a result, the grains of the aluminum matrix phase can be refined.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2001-191654 Summary of the invention

[0007] Problems to be solved by the invention

[0008] However, conventional aluminum alloy ingots whose crystal grains have been refined by an Al—Ti—B-based refiner may generate linear defects when subjected to stretching processing such as rolling and extrusion, which may lead to a risk of deteriorating the surface quality of the final product.

[0009] The present invention has been made in view of the above background, and provides an aluminum alloy ingot having fine crystal grains and capable of suppressing the occurrence of linear defects during stretching, and a method for producing the same.

[0010] Means used to solve problems

[0011] One embodiment of the present invention is an aluminum alloy ingot comprising:

[0012] Aluminum parent phase, and

[0013] TiB2 agglomerates, which are agglomerated TiB2 particles and dispersed in the aluminum matrix,

[0014] The average value of the equivalent circle diameter of the TiB2 aggregate in the state of being exposed from the aluminum matrix is ​​3.0 μm or less, and the average value of the circularity is 0.20 or more.

[0015] Another embodiment of the present invention is a method for producing an aluminum alloy ingot, which is the method for producing an aluminum alloy ingot of the above embodiment, comprising:

[0016] A dissolving step, wherein a grain refiner is dissolved in a molten aluminum alloy, wherein the grain refiner includes TiB2 particles in a matrix including aluminum, and an average value of a distance between centers of adjacent TiB2 particles in any cross section is 0.60 μm or more; and

[0017] A casting step, wherein the molten metal is cast after the melting step.

[0018] Another aspect of the present invention is a method for producing an aluminum alloy ingot, which is the method for producing an aluminum alloy ingot of the above aspect, and comprises:

[0019] A dissolving step, wherein a grain refining agent is dissolved in a molten aluminum alloy, wherein the grain refining agent includes TiB2 agglomerates, wherein the TiB2 agglomerates are TiB2 particles agglomerated in a matrix including aluminum; and

[0020] a casting step, wherein, after the melting step, the molten metal is cast.

[0021] The TiB2 agglomerates in the above-mentioned grain refiner have the following particle size distribution: when measuring the projected area of ​​more than 2000 TiB2 agglomerates exposed from the above-mentioned substrate, the average value of the equivalent circle diameter of the TiB2 agglomerates having a projected area above the 95th percentile is less than 3.0 μm.

[0022] Effects of the Invention

[0023] The aluminum alloy ingot has TiB2 agglomerates with TiB2 particles as primary particles in the aluminum matrix. In addition, the average value of the equivalent circle diameter and the average value of the circularity of the TiB2 agglomerates are each within the above-mentioned specific ranges. This means that the aluminum alloy ingot is produced by casting a molten metal containing the above-mentioned specific TiB2 agglomerates.

[0024] The TiB2 agglomerates having the average values ​​of the equivalent circle diameter and the average values ​​of the circularity within the above-mentioned specific ranges have a high ability to refine the grains of the aluminum matrix phase. Therefore, by forming the TiB2 agglomerates in the molten metal, the grains of the aluminum matrix phase can be sufficiently refined. In addition, the TiB2 agglomerates have a small particle size, so the generation of linear defects when the aluminum alloy ingot is subjected to stretching processing can be suppressed.

[0025] According to the above aspect, it is possible to provide an aluminum alloy ingot having fine crystal grains and capable of suppressing the occurrence of linear defects during stretching.

[0026] In addition, in the method for manufacturing the aluminum alloy ingot, the grain refiner is dissolved in the molten aluminum alloy, and then the molten aluminum is solidified to produce the ingot. The method for manufacturing the aluminum alloy ingot can form TiB2 agglomerates in the molten aluminum, wherein the average value of the equivalent circle diameter and the average value of the circularity are each within the above-mentioned specific ranges, by dissolving the grain refiner having the above-mentioned specific structure in the molten aluminum in the above-mentioned melting step. Furthermore, by solidifying the molten aluminum, the grains of the aluminum alloy ingot finally obtained can be easily refined, and the generation of linear defects when the aluminum alloy ingot is subjected to stretching processing can be suppressed.

[0027] In addition, the above-mentioned method for manufacturing an aluminum alloy can improve the quality of an aluminum alloy ingot by dissolving the above-mentioned grain refiner in the molten aluminum alloy, which is a conventional method, and therefore, there is no need to add a special process or equipment for refining the grains of the aluminum matrix phase. Therefore, according to the above-mentioned method for manufacturing an aluminum alloy, an aluminum alloy ingot with excellent quality can be obtained while avoiding an increase in the manufacturing cost of the aluminum alloy ingot. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is an enlarged photograph of TiB2 particles contained in the aluminum alloy ingot of Example 1.

[0029] Figure 2 This is an enlarged photograph of TiB2 particles contained in the aluminum alloy ingot of Comparative Example 1. DETAILED DESCRIPTION

[0030] The chemical composition of the aluminum alloy ingot is not particularly limited, and may be any aluminum alloy. It should be noted that the "aluminum alloy" is a concept including pure aluminum. For example, the aluminum alloy ingot may have a chemical composition classified as A1000 series aluminum, or may have a chemical composition classified as A2000 series alloy, A3000 series alloy, A4000 series alloy, A5000 series alloy, A6000 series alloy, A7000 series alloy or A8000 series alloy.

[0031] From the viewpoint of suppressing the agglomeration of TiB2 particles during casting and reducing the average value of the equivalent circle diameter of TiB2 agglomerates, the above-mentioned aluminum alloy ingot preferably has the following chemical composition: it contains one or more elements selected from Si (silicon): 0.01 mass% or more and 14.0 mass% or less, Fe (iron): 0.01 mass% or more and 2.0 mass% or less, Cu (copper): 0.01 mass% or more and 7.0 mass% or less, Mg (magnesium): 0.01 mass% or more and 7.0 mass% or less, Mn (manganese): 0.01 mass% or more and 2.0 mass% or less, and Ti (titanium): 0.003 mass% or more and 0.3 mass% or more, and the remainder is composed of Al (aluminum) and unavoidable impurities.

[0032] The aluminum alloy ingot contains an aluminum matrix phase and TiB2 agglomerates. The aluminum alloy ingot may contain crystals according to its chemical composition. In addition, the aluminum alloy ingot may contain unagglomerated TiB2 particles.

[0033] The aluminum matrix phase may contain aluminum atoms and solid solution elements corresponding to the chemical composition of the aluminum alloy ingot. In addition, the aluminum matrix phase is composed of a large number of grains. The grain size of the aluminum matrix phase varies according to the chemical composition of the aluminum alloy ingot. In the aluminum alloy ingot containing the specific TiB2 agglomerates, the average grain size of the aluminum matrix phase is usually within a range of 50 μm or more and 5000 μm or less.

[0034] Agglomerates of TiB2 particles as primary particles, namely TiB2 agglomerates, are dispersed in the aluminum matrix. The particle size of each TiB2 particle included in the TiB2 agglomerate can be, for example, 0.1 μm or more and 5.0 μm or less.

[0035] The average value of the equivalent circle diameter of the TiB2 agglomerates exposed from the aluminum matrix is ​​3.0 μm or less. By setting the average value of the equivalent circle diameter of the TiB2 agglomerates to 3.0 μm or less, the generation of linear defects during the stretching process such as rolling and extrusion of the aluminum alloy ingot can be suppressed.

[0036] When the average equivalent circle diameter of TiB2 agglomerates is greater than 3.0 μm, the possibility of the presence of coarse TiB2 agglomerates in the aluminum alloy ingot increases. Accordingly, in this case, when the aluminum alloy ingot is subjected to stretching processing, there is a risk that linear defects originating from coarse TiB2 agglomerates are easily generated.

[0037] From the viewpoint of suppressing the generation of linear defects, the lower limit of the average value of the equivalent circle diameter of the TiB2 agglomerates is not particularly limited, and the average value of the equivalent circle diameter of the TiB2 agglomerates formed by the manufacturing method described above is usually 1.0 μm or more.

[0038] The average value of the equivalent circular diameter of the above-mentioned TiB2 agglomerates is a value calculated by the following method. First, a test piece is collected from the inside of an aluminum alloy ingot. Then, the aluminum matrix phase on the surface of the test piece is removed by deep etching or the like. The surface of the test piece is observed with an electron microscope or the like, thereby obtaining an enlarged photograph of the TiB2 agglomerates. Based on the projected area of ​​the TiB2 agglomerates in the obtained enlarged photograph, the equivalent circular diameter of each TiB2 agglomerate is calculated. The above operation is performed on a plurality of randomly selected TiB2 agglomerates, and their equivalent circular diameters are arithmetic averaged, thereby obtaining the average value of the equivalent circular diameters of the TiB2 agglomerates. The number of TiB2 agglomerates used when calculating the average value of the equivalent circular diameter may be, for example, 3 or more.

[0039] In addition, the average circularity of the TiB2 aggregates exposed from the aluminum matrix is ​​greater than 0.20. The circularity of the TiB2 aggregates is an indicator of whether the shape of the TiB2 aggregates is close to a sphere, and the closer the circularity is to 1, the more it means that the TiB2 aggregates are close to a sphere.

[0040] During the casting process of the aluminum alloy ingot, TiB2 agglomerates of various shapes are usually formed in the molten metal. Furthermore, the greater the circularity of the TiB2 agglomerates in the molten metal, the closer the shape is to a sphere, and the easier it is to function as a heterogeneous nucleus. Therefore, by setting the average circularity of the TiB2 agglomerates to 0.20 or more, the proportion of TiB2 agglomerates that can function as heterogeneous nuclei among the TiB2 agglomerates formed during casting can be increased.

[0041] When the average circularity of TiB2 aggregates is less than 0.20, the proportion of TiB2 aggregates that can function as heterogeneous nuclei among the TiB2 aggregates formed during casting tends to be low. Therefore, in this case, there is a risk that the grain refinement of the aluminum matrix phase becomes insufficient.

[0042] From the viewpoint of improving the effect of miniaturization of the crystal grains utilizing TiB2 agglomerates, the upper limit of the average circularity of the TiB2 agglomerates is not particularly limited, and the average circularity of the TiB2 agglomerates formed by the manufacturing method described above is usually 0.8 or less.

[0043] Specifically, the average circularity of the TiB2 aggregates is calculated by the following method. First, an enlarged photograph of the TiB2 aggregates is obtained in the same manner as the calculation method of the equivalent circle diameter. The circularity of each TiB2 aggregate is calculated using the area S [μm] of the TiB2 aggregates in the obtained enlarged photograph. 2 ] and the circumference L [μm] are expressed by the following formula.

[0044] Circularity = 4πS / L 2

[0045] The above operation is performed on a plurality of randomly selected TiB2 aggregates, and their circularity is arithmetic averaged, thereby obtaining the average circularity of the TiB2 aggregates. The number of TiB2 aggregates used in calculating the average circularity may be, for example, 3 or more.

[0046] In addition, by setting the average value of the equivalent circle diameter and the average value of the circularity of the TiB2 agglomerates contained in the above-mentioned aluminum alloy ingot to the above-mentioned specific ranges, in addition to the above-mentioned respective effects, it is also possible to reduce the amount of grain refining agent added during the casting process while ensuring the effect of grain refining.

[0047] That is, as described above, during the casting process of the aluminum alloy ingot, by setting the average value of the equivalent circle diameter of the TiB2 agglomerates formed in the molten metal to the above-mentioned specific range, it is possible to reduce coarse TiB2 agglomerates and increase the total number of TiB2 agglomerates in the molten metal. In addition, by setting the average value of the circularity of the TiB2 agglomerates to the above-mentioned specific range, it is possible to increase the proportion of TiB2 agglomerates in the molten metal that can function as heterogeneous nuclei.

[0048] Therefore, during the casting process of the above-mentioned aluminum alloy ingot, by setting the average value of the equivalent circle diameter and the average value of the circularity of the TiB2 agglomerates to the above-mentioned specific ranges, the number of TiB2 agglomerates that can function as heterogeneous nuclei can be increased, thereby improving the effect of refining the grains of the aluminum parent phase.

[0049] As described above, by setting the average value of the equivalent circle diameter and the average value of the circularity of the TiB2 aggregates contained in the aluminum alloy ingot to the above-mentioned specific ranges, the effect due to the reduction of the equivalent circle diameter and the effect due to the increase of the circularity can be synergistically achieved. As a result, when producing the aluminum alloy ingot, the amount of the grain refining agent added during casting can be reduced compared to the past while maintaining the effect of refining the crystal grains.

[0050] For example, the content of TiB2 aggregates in the above-mentioned aluminum alloy ingot can be set to 0.0001 mass% or more and 0.0010 mass% or less in terms of boron atoms.

[0051] When producing the aluminum alloy ingot, a method including a melting step of melting a grain refiner in a molten aluminum alloy and a casting step of casting the molten aluminum alloy after the melting step may be used.

[0052] In the above-mentioned production method, the grain refining agent added to the molten metal has a matrix containing aluminum. The shape of the matrix is ​​not particularly limited, and may have, for example, a rod-like shape, a plate-like shape, or the like.

[0053] In addition, the matrix contains TiB2 particles. The TiB2 particles may be dispersed in the matrix and exist in an unagglomerated state. In addition, a plurality of TiB2 particles may agglomerate to form TiB2 agglomerates in the matrix. More specifically, all TiB2 particles in the matrix may exist in an unagglomerated state, or all TiB2 particles in the matrix may exist in the form of TiB2 agglomerates. Furthermore, both unagglomerated TiB2 particles and TiB2 agglomerates may exist in the matrix.

[0054] At least a portion of the TiB2 particles in the matrix agglomerate in the molten metal to form TiB2 agglomerates after the grain refiner melts in the molten metal in the melting step. In addition, the TiB2 agglomerates in the matrix are directly transferred to the molten metal while maintaining the agglomerate state when the grain refiner melts in the molten metal in the melting step. Accordingly, by melting the grain refiner containing TiB2 particles in the aluminum molten metal, TiB2 agglomerates can be formed in the molten metal.

[0055] In the above-mentioned melting step, for example, a grain refiner of any of the following forms may be melted in the melt. That is, in the first form of the grain refiner, the average value of the center-to-center distance of the adjacent TiB2 particles in any cross section of the grain refiner is 0.60 μm or more. By setting the center-to-center distance of the TiB2 particles in the grain refiner to the above-mentioned specific range, the agglomeration of the TiB2 particles and the growth of the TiB2 agglomerates when the grain refiner is melted in the melt can be suppressed. As a result, the average value of the equivalent circle diameter and the average value of the circularity of the TiB2 agglomerates formed in the melt can be easily set to the above-mentioned specific range.

[0056] When the average value of the center-to-center distance between adjacent TiB2 particles is less than 0.60 μm, the TiB2 particles are likely to aggregate when the grain refiner is dissolved in the molten metal. As a result, coarse TiB2 aggregates are likely to form in the molten metal, which may reduce the effect of grain refinement and increase the frequency of linear defects during stretching.

[0057] It should be noted that the average value of the center-to-center distance of the above-mentioned TiB2 particles is a value calculated by the following method. First, the grain refiner is cut to expose the cut surface. The cut surface is observed using an electron microscope or the like, and an enlarged photograph of the cut surface is obtained. In the obtained enlarged photograph, the center of gravity of each TiB2 particle present in the enlarged photograph is determined. It should be noted that the TiB2 particles present in the enlarged photograph include both TiB2 particles present in an undispersed state and TiB2 particles forming a part of the TiB2 agglomerate.

[0058] Next, the TiB2 particles to be measured for the center-to-center distance are determined from the TiB2 particles present in the magnified photograph. Furthermore, the distance between the center of gravity of the TiB2 particle to be measured and the TiB2 particle closest to the TiB2 particle to be measured is measured, and this value is recorded as the center-to-center distance of the TiB2 particle to be measured. The above operation is performed for all TiB2 particles present in the magnified photograph, and the arithmetic mean of the obtained center-to-center distances is recorded as the average value of the center-to-center distances of the TiB2 particles.

[0059] In the second embodiment of the grain refiner, the TiB2 agglomerates in the grain refiner have a particle size distribution such that when the projected area of ​​more than 2000 TiB2 agglomerates exposed from the matrix is ​​measured, the average value of the equivalent circle diameters of the TiB2 agglomerates having a projected area of ​​more than the 95th percentile is less than or equal to 3.0 μm. In the grain refiner containing TiB2 agglomerates, the TiB2 agglomerates with a large equivalent circle diameter effectively function as heterogeneous nuclei in the aluminum melt.

[0060] However, if the equivalent circle diameter of the TiB2 agglomerates in the grain refiner becomes excessively large, coarse TiB2 agglomerates are easily mixed into the molten aluminum when the grain refiner is dissolved in the molten aluminum. As a result, when the cast aluminum alloy ingot is subjected to stretching processing, there is a risk that linear defects originating from the coarse TiB2 agglomerates are easily generated.

[0061] Therefore, by setting the particle size distribution of the TiB2 agglomerates in the grain refiner to the above-mentioned specific manner, the possibility of containing coarse TiB2 agglomerates in the grain refiner can be reduced, and the mixing of coarse TiB2 agglomerates in the melt can be suppressed. As a result, the average value of the equivalent circle diameter and the average value of the circularity of the TiB2 agglomerates formed in the melt can be easily set to the above-mentioned specific range.

[0062] When the average value of the equivalent circle diameter of TiB2 agglomerates having a projected area of ​​95th percentile or more is greater than 3.0 μm, the possibility of containing coarse TiB2 agglomerates in the grain refiner increases. Therefore, when the grain refiner is dissolved in the molten metal, coarse TiB2 agglomerates are easily mixed into the molten metal, which may reduce the effect of grain refinement and increase the frequency of linear defects during stretching.

[0063] It should be noted that the average value of the equivalent circle diameter of the TiB2 agglomerate is a value calculated by the following method. First, the grain refiner is cut to expose the cut surface. The cutting direction of the grain refiner is not particularly limited. For example, when the grain refiner is rod-shaped, the grain refiner can be cut through its center on a surface perpendicular to the long side direction.

[0064] Next, after grinding the cut surface of the grain refiner, the peripheral portion of the TiB2 aggregate in the matrix is ​​removed, thereby exposing the TiB2 aggregate from the matrix. As a method for removing the matrix, for example, a method such as deep etching can be used.

[0065] Next, the TiB2 aggregates exposed from the substrate are observed using an electron microscope or the like, and an enlarged photograph of the TiB2 aggregates is obtained. The area of ​​the TiB2 aggregates in the enlarged photograph is recorded as the projected area of ​​each TiB2 aggregate. It should be noted that the calculation of the projected area of ​​the TiB2 aggregates and the calculation of the equivalent circle diameter can be performed using an image analysis device or the like.

[0066] The above operation is performed on more than 2000 TiB2 agglomerates randomly selected from the TiB2 agglomerates existing in the cross section of the grain refiner. Based on the projected area of ​​the TiB2 agglomerates obtained in this way, the 95th percentile of the projected area is calculated. It should be noted that the percentile refers to the value at which the number of values ​​counted from the smaller value reaches the desired percentage relative to the total number of values ​​when multiple values ​​are arranged in order from the smaller value to the larger value. In the absence of such a value, the largest value among the values ​​at which the number of values ​​counted from the smaller value reaches a percentage lower than the desired percentage relative to the total number of values ​​is recorded as the percentile. More specifically, the 95th percentile of the projected area refers to the value at which the number of TiB2 agglomerates having a projected area of ​​more than the 95th percentile reaches 5% of the total number of TiB2 agglomerates of the measured projected area.

[0067] After determining the 95th percentile of the projected area in this way, the equivalent circle diameter of the TiB2 agglomerate having a projected area greater than the 95th percentile is calculated. It should be noted that the equivalent circle diameter is the diameter of a circle having an area equal to the projected area of ​​the TiB2 agglomerate. In addition, the equivalent circle diameters of the obtained TiB2 agglomerates are arithmetic averaged, thereby obtaining the average value of the equivalent circle diameters of the TiB2 agglomerates having a projected area greater than the 95th percentile.

[0068] The content of TiB2 particles in the grain refiner can be set to, for example, 0.5 mass % or more and 3.2 mass % or less. In this case, the average value of the center-to-center distance between adjacent TiB2 particles tends to be longer. As a result, the effect of suppressing the aggregation of TiB2 particles when the grain refiner is dissolved in the molten metal can be more reliably achieved.

[0069] In the above manufacturing method, the above grain refiner is melted in a molten aluminum alloy having a desired chemical composition. At this time, the molten alloy may be stirred as needed to uniformly disperse the TiB2 particles in the grain refiner in the molten alloy.

[0070] In the above manufacturing method, after dissolving the grain refiner in the molten metal, the molten metal is cast, thereby making an aluminum alloy ingot. The casting method is not particularly limited, for example, semi-continuous casting, continuous casting and the like can be used. The aluminum alloy ingot made by these methods can be used for the production of extended materials such as rolled plates and extruded materials. In addition, the above aluminum alloy molten metal is poured into a mold or a sand mold and then cooled, thereby also being able to obtain an ingot having a desired product shape or a shape close to the product shape.

[0071] In the above-mentioned manufacturing method, it is preferred that the molten metal is cast within 30 minutes after the grain refiner is dissolved in the molten metal. TiB2 particles have a larger specific gravity than the molten metal. Therefore, if the time from the moment when the grain refiner is dissolved in the molten metal becomes longer, the TiB2 particles settle due to their own weight, and it is easy to cause the TiB2 particles to aggregate in the lower part of the crucible. As a result, there is a risk that coarse TiB2 aggregates are easily formed. By setting the time from the moment when the grain refiner is dissolved in the molten metal to the casting to within 30 minutes, the above-mentioned problem can be more easily avoided.

[0072] It should be noted that the above-mentioned aluminum alloy ingot and the method for producing the same can also be understood as the invention of a grain refining agent that specifies the dispersion state of TiB2 particles from another point of view.

[0073] That is, the first aspect of the grain refining agent has:

[0074] A substrate comprising aluminum, and

[0075] The TiB2 particles present in the above matrix,

[0076] The average value of the distance between the centers of the adjacent TiB2 particles in any cross section is 0.60 μm or more.

[0077] In addition, the second aspect of the grain refining agent has:

[0078] A substrate comprising aluminum, and

[0079] TiB2 agglomerates formed by agglomeration of TiB2 particles and present in the above-mentioned matrix;

[0080] The above-mentioned TiB2 agglomerates have the following particle size distribution: when measuring the projected areas of more than 2000 of the above-mentioned TiB2 agglomerates exposed from the above-mentioned substrate, the average value of the equivalent circle diameters of the TiB2 agglomerates having a projected area above the 95th percentile reaches less than 3.0 μm.

[0081] The above-mentioned grain refining agent is estimated to be produced by, for example, the following production method.

[0082] That is, in the method for producing the grain refining agent, a molten aluminum forming a matrix is ​​prepared,

[0083] Blowing TiB2 particles into the above-mentioned melt together with an inert gas, thereby dispersing the above-mentioned TiB2 particles in the above-mentioned melt,

[0084] Thereafter, the molten metal is solidified. In this manner, the grain refining agent can be obtained.

[0085] As TiB2 particles blown into the melt, it is preferred to use TiB2 particles with a narrow particle size distribution width, and it is more preferred to use TiB2 particles with a particle size standard deviation of 0.5 μm or less. In addition, as an inert gas, nitrogen, argon, etc. can be used. It should be noted that the standard deviation of the particle size of the TiB2 particles is a value calculated based on the particle size distribution on a volume basis. Specifically, the particle size distribution on a volume basis of the TiB2 particles can be obtained using a laser diffraction particle size distribution measuring device.

[0086] Example

[0087] The aluminum alloy ingot and the method for producing the same are described below in an embodiment. It should be noted that the specific aspects of the aluminum alloy ingot and the method for producing the same according to the present invention are not limited to those of the embodiment, and the configuration may be appropriately changed within the scope of the present invention.

[0088] (Examples 1, 2 and Comparative Examples 1, 2)

[0089] Examples 1 and 2 and Comparative Examples 1 and 2 are examples of aluminum alloy ingots containing pure aluminum. In these examples, first, an aluminum raw metal having a purity of 99.7% by mass is melted to prepare a molten metal. After the temperature of the molten metal is set to 718° C., a grain refiner in which TiB2 particles are dispersed in a matrix containing aluminum is added to the molten metal in an amount of 10 ppm by mass in terms of boron atoms.

[0090] Specifically, the grain refiner used in this example has the following chemical composition: containing Ti: 1.0 mass % or more and 5.5 mass % or less, B: 0.1 mass % or more and 1.5 mass % or less, and the remainder is composed of Al and inevitable impurities, and has a matrix containing aluminum and TiB2 particles existing in the matrix. A part of the TiB2 particles exists in an unagglomerated state, and the rest constitutes TiB2 agglomerates.

[0091] The center-to-center distance between adjacent TiB2 particles in any cross section of the grain refiner of this example is the value shown in Table 1. In addition, the TiB2 agglomerates in the grain refiner have the following particle size distribution: when the projected area of ​​more than 2000 TiB2 agglomerates exposed from the matrix is ​​measured, the average value of the equivalent circle diameter of the TiB2 agglomerates having a projected area of ​​more than the 95th percentile reaches the value shown in Table 1.

[0092] After adding the grain refining agent to the melt, the melt was stirred for 30 seconds using a graphite rod while maintaining the melt temperature at 718° C. to fully dissolve the grain refining agent. Furthermore, after 9 minutes and 15 seconds had passed since the grain refining agent was added, the melt was stirred for 15 seconds using a graphite rod again.

[0093] After the second stirring, an iron ladle according to the AA-TP1 standard was immersed in the molten metal, and the cup of the ladle was filled with the molten metal. Then, 10 minutes after the addition of the grain refiner, the ladle was lifted from the molten metal and the molten metal was drawn into the cup. Thereafter, the cup of the ladle was cooled using a water cooling device according to the AA-TP1 standard to solidify the molten metal. Through the above, aluminum alloy ingots of Examples 1 and 2 and Comparative Examples 1 and 2 were obtained. These aluminum alloy ingots all had a truncated cone shape.

[0094] The calculation method of the average value of the equivalent circle diameter and the average value of the circularity of the TiB2 agglomerates in the aluminum alloy ingots of Examples 1 and 2 and Comparative Examples 1 and 2 is as follows. Table 1 shows these values ​​in the aluminum alloy ingots of Examples 1 and 2 and Comparative Examples 1 and 2.

[0095] The average value of equivalent circle diameter and circularity of TiB2 agglomerates

[0096] The aluminum alloy ingot was cut at a cross section of 38 mm from a surface with a small diameter (i.e., a surface in contact with the bottom surface of the ladle) among the circular end surfaces of the aluminum alloy ingot to expose the cut surface. After grinding the cut surface, deep etching was performed to remove the aluminum matrix phase and expose the TiB2 aggregate as a whole.

[0097] Next, an electron microscope was used to obtain a magnified photograph of the TiB2 aggregate. As an example, Figure 1 An enlarged photograph of the TiB2 agglomerates contained in the aluminum alloy ingot of Example 1 is shown in FIG. Figure 2 An enlarged photograph of the TiB2 aggregate contained in the aluminum alloy ingot of Comparative Example 2 is shown in FIG. Figure 1 and Figure 2 As shown, the TiB2 aggregate 2 in the aluminum matrix 1 is in the form of a block in which a large number of TiB2 particles 3 are aggregated.

[0098] The area of ​​the TiB2 agglomerate 2 in the enlarged photograph was calculated using image analysis software, and then the equivalent circular diameter of each TiB2 agglomerate was calculated based on the area of ​​the TiB2 agglomerate 2. The above operation was performed on 8 randomly selected TiB2 agglomerates, and the value obtained by arithmetic averaging of these equivalent circular diameters was recorded as the average value of the equivalent circular diameters of the TiB2 agglomerates. Table 1 shows the average value of the equivalent circular diameters of the TiB2 agglomerates in each aluminum alloy ingot.

[0099] In addition, the perimeter of the TiB2 agglomerate 2 in the above-mentioned enlarged photograph, i.e., the length of the outline, is calculated using image analysis software. Furthermore, the circularity of each TiB2 agglomerate is calculated from the area and perimeter of the TiB2 agglomerate 2. The above operation is performed on three or more randomly selected TiB2 agglomerates, and the value obtained by arithmetic averaging of these circularities is recorded as the average circularity of the TiB2 agglomerates. Table 1 shows the average circularity of the TiB2 agglomerates in each aluminum alloy ingot.

[0100] (Example 3)

[0101] Example 3 is an example of an aluminum alloy ingot containing an A3000 series alloy. In Example 3, first, a molten metal containing an A3000 series alloy is prepared using a heating furnace, and then a grain refiner is added to the molten metal in an amount of 10 mass ppm in terms of boron atoms. The grain refiner used in this example has a chemical composition containing 5.0 mass % Ti, 1.0 mass % B, and the remainder consisting of Al and unavoidable impurities, and the center-to-center distance between adjacent TiB2 particles in any cross section of the grain refiner is the value shown in Table 1, and the average value of the equivalent circular diameter of TiB2 agglomerates having a projected area of ​​95th percentile or more reaches the value shown in Table 1. Other than this, it is the same as Example 1.

[0102] After adding the grain refiner to the molten metal, the molten metal was stirred for 30 seconds using a graphite rod. Thereafter, the molten metal was cast by a DC casting method. Through the above, an aluminum alloy ingot of Example 3 was obtained. The aluminum alloy ingot of Example 3 was in a rectangular parallelepiped shape.

[0103] (Example 4)

[0104] Example 4 is an example of an aluminum alloy ingot containing A1000 series aluminum. In Example 4, the molten aluminum alloy is cast by the same method as in Example 3 except that a molten aluminum containing A1000 series aluminum is prepared using a heating furnace. Thus, the aluminum alloy ingot of Example 4 is obtained. The aluminum alloy ingot of Example 4 is in the same rectangular parallelepiped shape as in Example 3.

[0105] The method for calculating the average value of the equivalent circle diameter and the average value of the circularity of the TiB2 agglomerates in the aluminum alloy ingots of Examples 3 and 4 is as follows.

[0106] The average value of equivalent circle diameter and circularity of TiB2 agglomerates

[0107] The aluminum alloy ingot was cut and a test piece was collected from the central part in the width direction and the thickness direction. After the surface of the test piece was ground, deep etching was performed to remove the aluminum matrix phase and expose the TiB2 aggregate as a whole. Thereafter, the average value of the equivalent circle diameter of the TiB2 aggregate and the average value of the circularity were calculated by the same method as in Example 1. Table 1 shows these values ​​for the aluminum alloy ingots of Examples 3 and 4.

[0108]

Table 1

[0109]

[0110] As shown in Table 1, the average values ​​of the equivalent circle diameters and the average values ​​of the circularity of the TiB2 agglomerates contained in the aluminum alloy ingots of Examples 1 to 4 are each within the above-mentioned specific ranges. Accordingly, in these aluminum alloy ingots, the grains of the aluminum matrix phase are sufficiently refined, and at the same time, there are few coarse TiB2 agglomerates, which can suppress the generation of linear defects during processing such as rolling.

[0111] The average value of the equivalent circle diameter of the TiB2 agglomerates contained in the aluminum alloy ingots of Comparative Examples 1 and 2 is larger than the above-mentioned specific range. Therefore, these aluminum alloy ingots are prone to contain coarse TiB2 agglomerates, and linear defects are easily generated during stretching.

Claims

1. An aluminum alloy ingot, comprising: Aluminum parent phase, and TiB2 agglomerates, which are agglomerated TiB2 particles and dispersed in the aluminum matrix, The average value of the equivalent circle diameter of the TiB2 agglomerates in the state of being exposed from the aluminum matrix is ​​3.0 μm or less, and the average value of the circularity is 0.20 or more, The content of the TiB2 aggregate is greater than or equal to 0.0001 mass % and less than or equal to 0.0010 mass % in terms of boron atoms.

2. The method for producing the aluminum alloy ingot according to claim 1, comprising the following steps: A melting step, wherein A grain refiner is dissolved in a molten aluminum alloy, wherein the grain refiner contains TiB2 particles in a matrix containing aluminum, and the average value of the center-to-center distance between adjacent TiB2 particles in any cross section is 0.60 μm or more; and A casting step, wherein the molten metal is cast after the melting step.

3. The method for producing the aluminum alloy ingot according to claim 1, comprising the following steps: A melting step, wherein Dissolving a grain refining agent in a molten aluminum alloy, the grain refining agent comprising TiB2 agglomerates, the TiB2 agglomerates being TiB2 particles agglomerated in a matrix comprising aluminum; and a casting step, wherein, after the melting step, the molten metal is cast. The TiB2 agglomerates in the grain refiner have the following particle size distribution: when measuring the projected area of ​​more than 2000 TiB2 agglomerates exposed from the substrate, the average value of the equivalent circle diameters of the TiB2 agglomerates having a projected area above the 95th percentile is less than 3.0 μm.

4. The method for producing an aluminum alloy ingot according to claim 2 or 3, wherein: After the grain refining agent is dissolved in the molten metal, the molten metal is cast within 30 minutes.