A composite adsorbent and its preparation method and application

By loading rare earth metal carbonates on aquatic animal gill biofilm-like materials, an efficient composite adsorbent is prepared, which solves the problems of low adsorption capacity and poor selectivity in the existing technology, and achieves efficient removal of phosphate and Full utilization of resources.

CN114762820BActive Publication Date: 2024-10-01XIAMEN INST OF RARE EARTH MATERIALS +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202110045210.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-01-13
Publication Date
2024-10-01
Estimated Expiration
2041-01-13

AI Technical Summary

Technical Problem

The phosphate-modified adsorbents prepared from agricultural and forestry wastes in the existing technology have problems with low adsorption capacity and poor selective adsorption, and aquatic animal gill biofilm-like materials are not used for deep processing, resulting in waste of resources and failure to improve economic benefits.

Method used

Using aquatic animal gill biofilm-like materials as carriers, loading rare earth metal carbonates, a composite adsorbent is obtained through the reaction, using its high specific surface area and the coordination of rare earth metal carbonates to improve the adsorption capacity and selection of phosphates sex.

Benefits of technology

The composite adsorbent with high specific surface area has excellent adsorption performance for phosphate, effectively utilizing waste gill materials, reducing resource waste, and improving economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114762820B_ABST
    Figure CN114762820B_ABST
Patent Text Reader

Abstract

The present invention discloses a composite adsorbent and a preparation method and application thereof, wherein the composite adsorbent comprises a carrier of a biofilm structure and a rare earth metal carbonate loaded on the carrier. The present invention recycles and utilizes the discarded gill biofilm materials of discarded aquatic animals, such as discarded crab gills, and turns waste into treasure. The high specific surface area membrane structure of the crab gills can effectively load the rare earth metal carbonate to prepare a dephosphorization adsorbent for treating phosphorus-containing wastewater, thereby achieving excellent phosphorus adsorption capacity and adsorption selectivity, and achieving full utilization of resources.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of adsorbents, and in particular relates to a composite adsorbent and a preparation method and application thereof. Background Art

[0002] Phosphorus is a mineral element, which mainly comes from the development and utilization of phosphate rock. Phosphorus is an essential element for plant growth. The lack of phosphorus will cause morphological and physiological changes in plants. However, due to the indiscriminate discharge of mining, industrial and agricultural activities, the phosphorus content in water bodies has risen sharply, leading to eutrophication of water bodies and affecting the ecological balance. Phosphorus in water bodies mainly exists in the form of phosphate. China's wastewater discharge standard is that the total phosphorus content in water bodies is less than or equal to 0.5 mg / L. Therefore, how to effectively treat phosphorus-containing wastewater has become an urgent problem that needs to be solved.

[0003] Domestic and foreign scholars have done a lot of research on the treatment of phosphate. The phosphate treatment methods that have been developed and applied mainly include chemical precipitation, biological method and adsorption method. The adsorption method has the advantages of low cost, easy operation and recyclable adsorbent, thus becoming a hot research direction. In recent years, some researchers (such as Zhang Bowen. Study on the adsorption and phosphorus removal performance and mechanism of iron-modified peanut shell biochar [D]. China University of Geosciences (Beijing), 2018; Ao Hanting, Cao Wei, Kan Jin, Deng Caijun, Wei Lin. Structural characterization and phosphorus adsorption effect of zirconium-loaded corn straw biochar [J]. Journal of Huaqiao University (Natural Science Edition), 2018, 39(06): 851-858.; Chen Ziyan. Preparation and adsorption research of phosphate adsorbent based on mesoporous silica and bagasse materials [D]. Shanghai Normal University, 2010.) have used agricultural, forestry and fishery wastes, such as peanut shells, corn straw, and bagasse, as basic raw materials to prepare new phosphate-modified adsorbents. The coordination effect between the metal ions contained in the modified adsorbents and phosphate can be used for chemical and physical adsorption of phosphate, so phosphate can be removed from water to a certain extent. However, the agricultural and forestry wastes reported so far generally have problems such as low adsorption capacity and poor phosphate selectivity.

[0004] The gill biomembrane materials of aquatic animals, such as crab gills, are mainly composed of gill axes and gill leaves arranged in layers to form a biomembrane structure. It has a large specific surface area and regular layered stacking. It is an important organ for crabs to ingest a variety of nutrients and trace elements from water. The annual output of river crabs in China is about 800,000 tons, and crab gills are the inedible parts of crabs. At present, there are no deep processing methods and utilization channels for a large number of discarded crab gills. Therefore, the comprehensive utilization of crab gills is of great significance for reducing resource waste and improving economic benefits. However, crab gills themselves do not have phosphate adsorption properties. There is currently no relevant literature on the preparation of adsorbents based on membranous biological structures such as crab gills. And the existing technology has few studies on the modification of membranous biomass materials such as crab gills. Therefore, how to use a large number of discarded gill biomembrane materials of aquatic animals, especially crab gills, to prepare phosphorus removal adsorbents with high phosphate adsorption capacity and good selective adsorption has become a technical problem to be solved. Summary of the invention

[0005] In order to improve the above technical problems, the present invention provides a composite adsorbent, which includes a carrier with a biofilm structure and a rare earth metal carbonate loaded on the carrier.

[0006] According to an embodiment of the present invention, the carrier of the biofilm-like structure may be a biofilm-like material of the gills of aquatic animals, preferably a biofilm-like material of the gills of crabs.

[0007] According to an embodiment of the present invention, the specific surface area of ​​the carrier of the biofilm-like structure is greater than 8m 2 / g.

[0008] According to an embodiment of the present invention, based on the weight of the carrier' in the composite adsorbent, the content of rare earth ions loaded on the carrier' is (1.0-5.5) mmol / g, for example, (2-5) mmol / g, exemplified by 1.0 mmol / g, 1.5 mmol / g, 2.5 mmol / g, 2.9 mmol / g, 3 mmol / g, 3.5 mmol / g, 4 mmol / g, 4.5 mmol / g, 5.5 mmol / g;

[0009] The carrier' is composed of a carrier with a biofilm structure and carbonate and / or bicarbonate loaded on the carrier.

[0010] According to an embodiment of the present invention, the rare earth metal carbonate may be obtained by reacting a water-soluble salt containing a rare earth metal element with at least one of a water-soluble carbonate and a water-soluble bicarbonate.

[0011] According to an embodiment of the present invention, the water-soluble salt containing rare earth metal elements can be selected from at least one of hydrochlorides, nitrates and sulfates containing rare earth metal elements; preferably selected from hydrochlorides of rare earth metal elements.

[0012] According to an embodiment of the present invention, the rare earth metal element may be selected from one, two or more of the following rare earth metal elements: La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Y and Sc. Preferably, the rare earth metal element is selected from one, two or more of Y, La, Ce, Eu and Yb.

[0013] According to an exemplary embodiment of the present invention, the water-soluble salt containing a rare earth metal element can be selected from one, two or more of yttrium chloride, lanthanum chloride, cerium chloride, europium chloride, ytterbium chloride, lanthanum nitrate, cerium nitrate, yttrium nitrate, europium nitrate, ytterbium nitrate, yttrium sulfate, lanthanum sulfate, cerium sulfate, europium sulfate and ytterbium sulfate.

[0014] According to an embodiment of the present invention, the water-soluble carbonate may be selected from one, two or more of the following substances: sodium carbonate, ammonium carbonate, potassium carbonate, preferably sodium carbonate.

[0015] According to an embodiment of the present invention, the water-soluble bicarbonate may be selected from one, two or more of the following substances: sodium bicarbonate, ammonium bicarbonate, potassium bicarbonate, preferably sodium bicarbonate or the like.

[0016] According to an exemplary embodiment of the present invention, the rare earth metal carbonate is obtained by reacting a hydrochloride containing a rare earth metal element with a water-soluble carbonate.

[0017] For example, the rare earth metal carbonate is lanthanum carbonate, which is obtained by reacting lanthanum chloride and sodium carbonate.

[0018] For example, the rare earth metal carbonate is cerium carbonate, and the cerium carbonate is obtained by reacting cerium chloride and sodium carbonate.

[0019] For example, the rare earth metal carbonate is yttrium carbonate, and the yttrium carbonate is obtained by reacting yttrium chloride and sodium carbonate.

[0020] For example, the rare earth metal carbonate is europium carbonate, which is obtained by reacting europium chloride and sodium carbonate.

[0021] For example, the rare earth metal carbonate is ytterbium carbonate, and the ytterbium carbonate is obtained by reacting ytterbium chloride and sodium carbonate.

[0022] According to an embodiment of the present invention, the composite adsorbent may be a yttrium carbonate-loaded crab gill adsorbent, a lanthanum carbonate-loaded crab gill adsorbent, a cerium carbonate-loaded crab gill adsorbent, a europium carbonate-loaded crab gill adsorbent, or a ytterbium carbonate-loaded crab gill adsorbent.

[0023] The present invention also provides a method for preparing the composite adsorbent, which comprises loading rare earth metal carbonate on a carrier with a biofilm structure to prepare the composite adsorbent.

[0024] According to an embodiment of the present invention, the carrier of the biofilm-like structure has the meaning as described above.

[0025] According to an embodiment of the present invention, the preparation method further comprises the step of pre-treating the carrier of the biofilm-like structure.

[0026] Preferably, the pretreatment step comprises: soaking the carrier of the biofilm-like structure in deionized water, and ultrasonicating after soaking; filtering out the obtained carrier of the biofilm-like structure, washing it with deionized water, and drying it for use. For example, the soaking time can be 15-30 hours. For example, the ultrasonication time is 15-50 minutes. For example, the drying temperature is 50-70°C.

[0027] According to an embodiment of the present invention, the rare earth metal carbonate has the meaning as described above.

[0028] According to an embodiment of the present invention, the rare earth metal carbonate is obtained by reacting a water-soluble salt containing a rare earth metal element with at least one of a water-soluble carbonate and a water-soluble bicarbonate.

[0029] According to an embodiment of the present invention, the molar ratio of the water-soluble salt containing rare earth metal elements to the water-soluble carbonate is (1-8):10, for example, (1.5-6):10, exemplified by 1.5:10, 1.8:10, 2.4:10, 3:10, 2:3, 6:10.

[0030] According to an embodiment of the present invention, the molar ratio of the water-soluble salt containing rare earth metal elements to the water-soluble bicarbonate is (1-8):10, for example (1.5-6):10, exemplified by 1.5:10, 1.8:10, 2.4:10, 3:10, 2:3, 6:10.

[0031] According to an embodiment of the present invention, the water-soluble salt containing rare earth metal elements and the water-soluble carbonate or water-soluble bicarbonate are added to the reaction system in the form of solutions. For example, a hydrated ethanol solution of a water-soluble salt containing rare earth metal elements and an aqueous solution of a water-soluble carbonate or water-soluble bicarbonate are prepared separately. Preferably, the hydrated ethanol solution of a water-soluble salt containing rare earth metal elements is first mixed with a carrier of a biofilm-like structure, and then mixed with an aqueous solution of a water-soluble carbonate or an aqueous solution of a water-soluble bicarbonate, and the reaction obtains a carrier of a biofilm-like structure modified with a rare earth metal carbonate.

[0032] According to an embodiment of the present invention, the dosage ratio of the biofilm-like structure carrier to the rare earth metal ions in the water-soluble salt containing rare earth metal elements is 1g:(0.03~0.1)mol, preferably 1g:(0.05~0.1)mol, exemplified by 1g:0.03mol, 1g:0.05mol, 1g:0.08mol, and 1g:0.1mol.

[0033] According to an embodiment of the present invention, the concentration of the hydrated ethanol solution containing a water-soluble salt of a rare earth metal element is 0.3-1.0 mol / L, preferably 0.5-1.0 mol / L, exemplified by 0.3 mol / L, 0.5 mol / L, 0.8 mol / L, 1.0 mol / L.

[0034] According to an embodiment of the present invention, the ethanol concentration in the hydrated ethanol solution is 10-30%, for example, 20%.

[0035] According to an embodiment of the present invention, the concentration of the water-soluble carbonate aqueous solution or the water-soluble bicarbonate aqueous solution is 0.5-2.0 mol / L, preferably 1.0-2.0 mol / L, exemplified by 0.5 mol / L, 0.8 mol / L, 1.0 mol / L, 1.5 mol / L, 2.0 mol / L.

[0036] According to an embodiment of the present invention, the preparation method further comprises the step of stirring the mixed liquid.

[0037] According to an embodiment of the present invention, the stirring speed is 200-400 r / min. Further, the stirring temperature is 50-80° C., and the stirring time is 4-24 h.

[0038] Preferably, the stirring speed is 300 r / min, the stirring temperature is 60° C., and the stirring time is 12 h.

[0039] According to an embodiment of the present invention, the preparation method further comprises the step of solid-liquid separation of the carrier of the gill biomembrane structure modified by rare earth metal carbonate. For example, the solid-liquid separation can be carried out by means known in the art, such as filtration and centrifugation.

[0040] According to an embodiment of the present invention, the preparation method further comprises washing the reaction product obtained by solid-liquid separation. Preferably, the solvent used for washing can be deionized water, NaCl solution, hydrated ethanol solution. For example, the order of washing can be first eluting with deionized water until it is neutral, and then eluting with 5wt% NaCl solution and 50% hydrated ethanol solution in sequence.

[0041] According to an embodiment of the present invention, the preparation method further comprises drying the washed reaction product to obtain the composite adsorbent. For example, the drying temperature is 90-120°C, preferably 100-110°C, and exemplarily 90°C, 100°C, 105°C, and 110°C. Further, the drying time is 8-24h, preferably 12-18h, and exemplarily 8h, 12h, 18h, 20h, and 24h.

[0042] According to an embodiment of the present invention, the preparation method comprises the following steps:

[0043] (1) preparing a hydrated ethanol solution of a rare earth metal hydrochloride having a concentration of 0.3 to 1.0 mol / L;

[0044] (2) adding the pre-treated crab gills to the hydrated ethanol solution of the rare earth metal hydrochloride, heating and stirring, for example, stirring at 60° C. for 12 h at 300 r / min;

[0045] (3) filtering and removing the crab gills after heating and stirring in step (2), placing them in a Na2CO3 solution with a concentration of 0.5 to 2.0 mol / L, and heating and stirring, for example, stirring at 60°C at 300 r / min for 12 h;

[0046] (4) filtering and removing the crab gills treated in step (3), rinsing with deionized water until neutral, and then rinsing with a NaCl solution and a hydrated ethanol solution in sequence;

[0047] (5) Drying the crab gills obtained in step (4) to prepare the composite adsorbent.

[0048] The present invention also provides the use of the composite adsorbent in the adsorption and removal of phosphate, preferably in the selective adsorption of phosphate.

[0049] The present invention also provides a method for removing phosphate by adsorption using the composite adsorbent, comprising contacting the composite adsorbent with a phosphate solution.

[0050] Preferably, the method for removing phosphate by adsorption using the composite adsorbent comprises adding the composite adsorbent into a phosphate solution and oscillating and adsorbing for 12 to 48 hours.

[0051] According to an embodiment of the present invention, the phosphate solution is a neutral solution at room temperature, for example, the pH value is 6.5-7.5, preferably 7. According to an embodiment of the present invention, the mass volume ratio of the composite adsorbent to the phosphate solution is 1 mg: (1.5-5) mL, preferably 1 mg: 2 mL.

[0052] According to an embodiment of the present invention, the content of phosphate in the phosphate solution is 15-50 mg / L, preferably 30 mg / L.

[0053] For example, 0.05 g of the above composite adsorbent is added to 100 mL of a 30 mg / L phosphate solution with a pH of 7.0; the solution is placed in a shaker at 180 r / min and 25° C. for 48 h, and the residual phosphate content is determined at 700 nm using the molybdenum antimony colorimetric method to determine the adsorption performance of the adsorbent.

[0054] Beneficial effects of the present invention:

[0055] The present invention recycles discarded gill biomembrane materials of aquatic animals, such as discarded crab gills, and turns waste into treasure. The high specific surface area membrane structure of crab gills can be used to effectively load rare earth metal carbonates to prepare phosphorus removal adsorbents for treating phosphorus-containing wastewater, thereby achieving excellent phosphorus adsorption capacity and adsorption selectivity and achieving full utilization of resources. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] Figure 1 This is a SEM image of an unmodified crab gill.

[0057] Figure 2 This is a SEM image of the lanthanum carbonate-loaded crab gill composite adsorbent prepared in Example 1.

[0058] Figure 3 This is the XRD image of the lanthanum carbonate-loaded crab gill composite adsorbent prepared in Example 1.

[0059] Figure 4 This is the SEM image of the cerium carbonate-loaded crab gill composite adsorbent prepared in Example 4.

[0060] Figure 5 This is the XRD image of the cerium carbonate-loaded crab gill composite adsorbent prepared in Example 4. DETAILED DESCRIPTION

[0061] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.

[0062] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.

[0063] Pre-treatment of crab gill materials:

[0064] The crab gills were soaked in deionized water for 24 hours, and then ultrasonicated for 30 minutes. The crab gills were filtered out, washed with deionized water, and dried in an oven at 60°C for later use.

[0065] The obtained crab gills have a specific surface area greater than 8m 2 / g.

[0066] Figure 1 The unmodified dried crab gills are shown in the figure. As can be seen from the figure, the unmodified crab gills have a layered membrane structure with a high specific surface area.

[0067] Example 1

[0068] (1) preparing 0.3 mol / L, 15 mL of lanthanum chloride hydrated ethanol solution, wherein the ethanol concentration in the hydrated ethanol solution is 20%;

[0069] (2) adding 0.15 g of pre-treated crab gills to the lanthanum chloride hydrate ethanol solution, and stirring the solution at 300 r / min and 60° C. for 12 h;

[0070] (3) Filter the crab gills after heating and stirring in step (2), put them into 25 mL of 1.0 mol / L Na2CO3 solution, and continue stirring at 300 r / min and 60°C for 12 h;

[0071] (4) filtering the crab gills treated in step (3), rinsing with deionized water until neutral, and then rinsing with 50 mL of a 5 wt % NaCl solution and a 50 % hydrated ethanol solution in sequence;

[0072] (5) The crab gills obtained in step (4) are placed in a vacuum oven at 105° C. for 12 h to prepare a lanthanum carbonate-loaded crab gill adsorbent.

[0073] The performance of the lanthanum carbonate-loaded crab gill composite adsorbent prepared in this example was characterized by scanning electron microscopy and X-ray diffractometer. The results are as follows: Figure 2 , Figure 3As shown, it is proved that the crab gill adsorbent loaded with lanthanum carbonate was successfully prepared.

[0074] Example 2

[0075] (1) preparing 0.5 mol / L, 15 mL of lanthanum chloride hydrated ethanol solution, wherein the ethanol concentration in the hydrated ethanol solution is 20%;

[0076] (2) adding 0.15 g of pre-treated crab gills to the lanthanum chloride hydrate ethanol solution, and stirring the solution at 300 r / min and 60° C. for 12 h;

[0077] (3) filtering the crab gills after heating and stirring in step (2), placing them in 25 mL of 0.5 mol / L Na2CO3 solution, and continuing to stir at 300 r / min and 60°C for 12 h;

[0078] (4) filtering the crab gills obtained in step (3), rinsing with deionized water until neutral, and then rinsing with 50 mL of a 5 wt % NaCl solution and a 50 % hydrated ethanol solution in sequence;

[0079] (5) The crab gills obtained in step (4) are placed in a vacuum oven at 105° C. for 12 h to prepare a lanthanum carbonate-loaded crab gill adsorbent.

[0080] Example 3

[0081] (1) Prepare 1.0 mol / L, 15 mL of lanthanum chloride hydrated ethanol solution, wherein the ethanol concentration in the hydrated ethanol solution is 20%.

[0082] (2) adding 0.15 g of pre-treated crab gills to the lanthanum chloride hydrate ethanol solution, and stirring the solution at 300 r / min and 60° C. for 12 h;

[0083] (3) filtering the crab gills after heating and stirring in step (2), placing them in 25 mL of 2 mol / L Na2CO3 solution, and continuing to stir at 300 r / min and 60°C for 12 h;

[0084] (4) filtering the crab gills treated in step (3), rinsing with deionized water until neutral, and then rinsing with 50 mL of a 5 wt % NaCl solution and a 50 % hydrated ethanol solution in sequence;

[0085] (5) The crab gills obtained in step (4) are placed in a vacuum oven at 105° C. for 12 h to prepare a lanthanum carbonate-loaded crab gill adsorbent.

[0086] Example 4

[0087] 1) preparing 0.5 mol / L, 15 mL cerium chloride hydrated ethanol solution, wherein the ethanol concentration in the hydrated ethanol solution is 20%;

[0088] (2) adding 0.15 g of pre-treated crab gills to the cerium chloride hydrate ethanol solution, and stirring the solution at 300 r / min and 60° C. for 12 h;

[0089] (3) filtering the crab gills after heating and stirring in step (2), placing them in 25 mL of 2.0 mol / L Na2CO3 solution, and continuing to stir at 300 r / min and 60°C for 12 h;

[0090] (4) filtering the crab gills treated in step (3), rinsing with deionized water until neutral, and then rinsing with 50 mL of a 5 wt % NaCl solution and a 50 % hydrated ethanol solution in sequence;

[0091] (5) The crab gills obtained in step (4) are placed in a vacuum oven at 105° C. for 12 h to prepare a cerium carbonate-loaded crab gill adsorbent.

[0092] The performance of the cerium carbonate-loaded crab gill composite adsorbent prepared in this example was characterized by scanning electron microscopy and X-ray diffractometer. The results are as follows: Figure 4 , Figure 5 As shown, it was proved that the crab gill adsorbent loaded with cerium carbonate was successfully prepared.

[0093] Example 5

[0094] (1) preparing 0.8 mol / L, 15 mL of cerium chloride hydrated ethanol solution, wherein the ethanol concentration in the hydrated ethanol solution is 20%;

[0095] (2) adding 0.15 g of pre-treated crab gills to the cerium chloride hydrate ethanol solution, and stirring the solution at 300 r / min and 60° C. for 12 h;

[0096] (3) filtering the crab gills after heating and stirring in step (2), placing them in 25 mL of 2 mol / L Na2CO3 solution, and continuing to stir at 300 r / min and 60°C for 12 h;

[0097] (4) filtering the crab gills treated in step (3), rinsing with deionized water until neutral, and then rinsing with 50 mL of a 5 wt % NaCl solution and a 50 % hydrated ethanol solution in sequence;

[0098] (5) The crab gills obtained in step (4) are placed in a vacuum oven at 105° C. for 12 h to prepare a cerium carbonate-loaded crab gill adsorbent.

[0099] Example 6

[0100] (1) preparing 1 mol / L, 15 mL cerium chloride hydrated ethanol solution, wherein the ethanol concentration in the hydrated ethanol solution is 20%;

[0101] (2) adding 0.15 g of pre-treated crab gills to the cerium chloride hydrate ethanol solution, and stirring the solution at 300 r / min and 60° C. for 12 h;

[0102] (3) filtering the crab gills after heating and stirring in step (2), placing them in 25 mL of 2 mol / L Na2CO3 solution, and continuing to stir at 300 r / min and 60°C for 12 h;

[0103] (4) filtering the crab gills treated in step (3), rinsing with deionized water until neutral, and then rinsing with 50 mL of a 5 wt % NaCl solution and a 50 % hydrated ethanol solution in sequence;

[0104] (5) The crab gills obtained in step (4) are placed in a vacuum oven at 105° C. for 12 h to prepare a cerium carbonate-loaded crab gill adsorbent.

[0105] Example 7

[0106] (1) preparing 0.5 mol / L, 15 mL of yttrium chloride hydrated ethanol solution, wherein the ethanol concentration in the hydrated ethanol solution is 20%;

[0107] (2) adding 0.15 g of pre-treated crab gills to the yttrium chloride hydrate ethanol solution, and stirring the solution at 300 r / min and 60° C. for 12 h;

[0108] (3) filtering the crab gills after heating and stirring in step (2), placing them in 25 mL of 2 mol / L Na2CO3 solution, and continuing to stir at 300 r / min and 60°C for 12 h;

[0109] (4) filtering the crab gills treated in step (3), rinsing with deionized water until neutral, and then rinsing with 50 mL of a 5 wt % NaCl solution and a 50 % hydrated ethanol solution in sequence;

[0110] (5) The crab gills obtained in step (4) are placed in a vacuum oven at 105° C. for 12 h to prepare a yttrium carbonate-loaded crab gill adsorbent.

[0111] Example 8

[0112] (1) preparing 0.5 mol / L, 15 mL of europium chloride hydrated ethanol solution, wherein the ethanol concentration in the hydrated ethanol solution is 20%;

[0113] (2) adding 0.15 g of pre-treated crab gills to the europium chloride hydrate ethanol solution, and stirring the solution at 300 r / min and 60° C. for 12 h;

[0114] (3) filtering the crab gills after heating and stirring in step (2), placing them in 25 mL of 2 mol / L Na2CO3 solution, and continuing to stir at 300 r / min and 60°C for 12 h;

[0115] (4) filtering the crab gills treated in step (3), rinsing with deionized water until neutral, and then rinsing with 50 mL of a 5 wt % NaCl solution and a 50 % hydrated ethanol solution in sequence;

[0116] (5) The crab gills obtained in step (4) are placed in a vacuum oven at 105° C. for 12 h to prepare a europium carbonate-loaded crab gill adsorbent.

[0117] Example 9

[0118] (1) preparing 0.5 mol / L, 15 mL of ytterbium chloride hydrated ethanol solution, wherein the ethanol concentration in the hydrated ethanol solution is 20%;

[0119] (2) adding 0.15 g of pre-treated crab gills to the hydrated ethanol solution of ytterbium chloride, and stirring the solution at 300 r / min and 60° C. for 12 h;

[0120] (3) filtering the crab gills after heating and stirring in step (2), placing them in 25 mL of 2 mol / L Na2CO3 solution, and continuing to stir at 300 r / min and 60°C for 12 h;

[0121] (4) filtering the crab gills treated in step (3), rinsing with deionized water until neutral, and then rinsing with 50 mL of a 5 wt % NaCl solution and a 50 % hydrated ethanol solution in sequence;

[0122] (5) The crab gills obtained in step (4) are placed in a vacuum oven at 105° C. for 12 h to prepare the ytterbium carbonate-loaded crab gill adsorbent.

[0123] Test Case

[0124] (1) 0.05 g of the adsorbent prepared in Examples 1 to 9 and Comparative Example 1 (taking the crab gills that have only been pretreated as the comparative sample) was added to a 150 mL stoppered conical flask, and 100 mL of a phosphate aqueous solution (prepared with potassium dihydrogen phosphate as the raw material and NaOH solution and HCl solution adjusting the pH to 7, pH=7.0 and phosphorus P concentration of 30 mg / L) was poured into it, and two groups of parallel tests were conducted. The conical flask was placed in a shaking table at 180 r / min and 25° C. for 48 hours, and the residual phosphate content was finally measured at 700 nm using the molybdenum antimony colorimetric method to determine the adsorption performance of the adsorbent for phosphate. The results are shown in Table 1 below.

[0125] Table 1

[0126]

[0127]

[0128] (2) The test method for the rare earth element content in the composite adsorbent is as follows:

[0129] Take 0.1 g of the lanthanum carbonate-loaded crab gill composite adsorbent prepared in Example 1-3, add 2 mL of concentrated nitric acid solution, place it at 180° C. for digestion, and then dissolve the digestion product in deionized water and make it dilute to 25 mL.

[0130] The aqueous solution of the above digestion product was tested by ICP (inductively coupled atomic emission spectrometer) to obtain the percentage content (mass fraction) of lanthanum ions and carrier' in the lanthanum carbonate-loaded crab gill composite adsorbent prepared in Examples 1-3 as shown in Table 2 below.

[0131] Table 2

[0132]

[0133] Note: The carrier' is composed of crab gills and carbonate ions loaded on the crab gills. The amount of the composite adsorbent is calculated as 100%, and the content of the carrier' is equal to 100% minus the content of the rare earth metal ions.

[0134] The results in Table 2 show that the loading amount of lanthanum in the composite adsorbent is not only related to the concentration of the rare earth salt solution, but also to the concentration of sodium carbonate. The content of rare earth ions in the crab gill composite adsorbent loaded with other rare earth metal ions carbonate can have a loading amount comparable to that of lanthanum ions.

[0135] (3) The lanthanum carbonate-loaded crab gill composite adsorbent prepared in Example 3 was subjected to a competitive ion adsorption test, and the test conditions were as follows:

[0136] 0.15 g of the crab gill composite adsorbent loaded with lanthanum carbonate prepared in Example 3 and the adsorbent containing competitive ions (humate ions, F -, Cl - Br - ,I - 、CO3 2- 、SO3 2- and NO3 - ) 100mL of phosphate solution (wherein: phosphorus P concentration is 100mg / L, and the concentration of competing ions is 100mg / L) was added into a 100mL conical flask and placed in a shaker at 180r / min and 25°C. The sampling time was 24h. The measured phosphate adsorption amount exceeded 90% under the condition of no interfering ions being present, which was qualified. The results are shown in Table 3 below.

[0137] Table 3

[0138]

[0139] The above is an explanation of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a composite adsorbent, characterized in that: The preparation method comprises the following steps: (1) preparing a hydrated ethanol solution of rare earth metal hydrochloride with a concentration of 0.3-1.0 mol / L; (2) adding the pre-treated crab gills to the hydrated ethanol solution of the rare earth metal hydrochloride, heating and stirring; (3) filtering the crab gills after heating and stirring in step (2), placing them in a Na2CO3 solution with a concentration of 0.5-2.0 mol / L, and heating and stirring; (4) filtering the crab gills treated in step (3), rinsing them with deionized water until they are neutral, and then rinsing them with a NaCl solution and a hydrated ethanol solution in sequence; (5) drying the crab gills obtained in step (4) to prepare the composite adsorbent; The molar ratio of the rare earth metal hydrochloride to Na2CO3 is (1-8):10; The ratio of the crab gill carrier to the rare earth metal ion is 1 g: (0.03-0.1) mol; The composite adsorbent includes a carrier with a biofilm structure and a rare earth metal carbonate loaded on the carrier; The carrier of the biofilm-like structure is crab gills; Based on the weight of the carrier' in the composite adsorbent, the content of rare earth ions loaded on the carrier' is (1.0-5.5) mmol / g; the carrier' is composed of crab gill carrier and carbonate and / or bicarbonate loaded on the carrier.

2. The method for preparing the composite adsorbent according to claim 1, characterized in that: The specific surface area of ​​the carrier of the biofilm structure is greater than 8 m 2 / g.

3. The method for preparing the composite adsorbent according to claim 1, characterized in that: The rare earth metal element is selected from one, two or more of the following rare earth metal elements: La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Y and Sc.

4. The method for preparing the composite adsorbent according to any one of claims 1 to 3, characterized in that: The composite adsorbent is a crab gill adsorbent loaded with yttrium carbonate, a crab gill adsorbent loaded with lanthanum carbonate, a crab gill adsorbent loaded with cerium carbonate, a crab gill adsorbent loaded with europium carbonate and a crab gill adsorbent loaded with ytterbium carbonate.

5. The preparation method according to claim 1, characterized in that: The pretreatment step comprises: soaking the carrier of the biofilm-like structure in deionized water, and ultrasonicating after soaking; filtering out the obtained carrier of the biofilm-like structure, washing it with deionized water, and drying it for standby use, wherein the soaking time is 15-30 hours, the ultrasonication time is 15-50 minutes, and the drying temperature is 50-70°C.

6. The preparation method according to claim 1, characterized in that: The ethanol concentration in the hydrated ethanol solution is 10-30%.

7. Use of the composite adsorbent prepared by the preparation method according to any one of claims 1 to 6 in the adsorption and removal of phosphate.

8. A method for removing phosphate by adsorption using the composite adsorbent prepared by the preparation method according to any one of claims 1 to 6, comprising contacting the composite adsorbent with a phosphate solution.

9. The method for removing phosphate by adsorption using a composite adsorbent as claimed in claim 8, comprising adding the composite adsorbent to a phosphate solution and adsorbing by oscillation for 12 to 48 hours; and / or, the pH value of the phosphate solution at room temperature is 6.5-7.5; and / or, the mass volume ratio of the composite adsorbent to the phosphate solution is 1 mg: (1.5-5) mL; And / or, the content of phosphate in the phosphate solution is 15-50 mg / L.

Citation Information

Patent Citations

  • Squid bone adsorbent capable of being used for oil-water separation and preparation method of squid bone adsorbent

    CN110560006A

  • Lanthanum carbonate modified co-pyrolysis sludge biochar as well as preparation method and application thereof

    CN110652963A