Low-smoke, non-drip, halogen-free flame-retardant polycarbonate composition and preparation method and application thereof

By combining grafting silicone and perfluorobutyl polymer flame retardant with specific polycarbonate, the problem of poor smoke and drip resistance of flame retardant polycarbonate materials is solved, and high flame retardant performance and excellent performance are achieved The mechanical properties are suitable for the application of thin film materials.

CN114773822BActive Publication Date: 2024-12-03NINGBO GANGZHI NEW MATERIAL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202210346574.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-31
Publication Date
2024-12-03
Estimated Expiration
2042-03-31

AI Technical Summary

Technical Problem

The existing flame-retardant polycarbonate materials emit large amounts of smoke and poor drip resistance during combustion, resulting in safety hazards and limited application.

Method used

Using grafted silicone and perfluorobutyl polymer flame retardant, combined with specific types of polycarbonate, a low-fume-free flame retardant polycarbonate combination is formed through three-phase grafting and ternary blending method. The substance was mixed and granulated by a twin screw extruder.

Benefits of technology

It achieves low smoke and drip-free performance, and at the same time improves the tensile strength, elongation of break, bending modulus and impact resistance of the material, and is suitable for film and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003576708340000091
    Figure BDA0003576708340000091
Patent Text Reader

Abstract

The present invention relates to the technical field of polymer materials, and in particular to a low-smoke, drip-free, halogen-free flame-retardant polycarbonate composition, and a preparation method and application thereof. The low-smoke, drip-free, halogen-free flame-retardant polycarbonate composition is mainly prepared from the following components by weight: 24 to 30 parts of polycarbonate with a melt index of 6 to 8, 57 to 63 parts of polycarbonate with a melt index of 10 to 12, 5 to 10 parts of flame retardant, and 5 to 8 parts of auxiliary agent; the flame retardant includes a grafted silicone and a perfluorobutyl polymer flame retardant. The polycarbonate composition of the present invention can improve tensile strength, elongation at break, flexural modulus, impact resistance, etc. while achieving high flame retardant properties, has high fluidity, and can be applied to fields such as films.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a low-smoking, drip-free, halogen-free flame-retardant polycarbonate composition, a preparation method and application thereof. Background Art

[0002] Polycarbonate (PC) is a high molecular polymer containing carbonate groups in the molecular chain. According to the different ester groups, it can be divided into aliphatic, aromatic, aliphatic-aromatic and other types. Aromatic polycarbonate has excellent optical properties, dimensional stability and mechanical strength, and has become a widely used general engineering plastic.

[0003] The traditional method of preparing flame-retardant PC materials is to add a series of different types of flame retardants to the PC matrix to reduce the combustion performance. General flame retardants include bromine, phosphorus, boron, aromatic sulfonates, etc. However, at present, most flame-retardant materials produce a large amount of smoke during combustion, easily releasing toxic, corrosive, and carcinogenic gases, and the smoke spreads quickly, with low visibility. Once a fire occurs, it will cause great problems, thus limiting the application of PC materials.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The object of the present invention is to provide a low-smoking, non-drip, halogen-free flame-retardant polycarbonate composition to solve the technical problems of the flame-retardant polycarbonate in the prior art, such as large smoke generation and poor anti-drip performance.

[0006] Another object of the present invention is to provide a method for preparing a low-smoking, non-drip, halogen-free flame-retardant polycarbonate composition.

[0007] Another object of the present invention is to provide an application of a low-smoking, non-drip, halogen-free flame-retardant polycarbonate composition in the field of preparing film materials.

[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0009] The low-smoking, non-drip, halogen-free flame-retardant polycarbonate composition is mainly prepared from the following components in parts by weight:

[0010] 24-30 parts of polycarbonate with a melt index of 6-8, 57-63 parts of polycarbonate with a melt index of 10-12, 5-10 parts of flame retardant and 5-8 parts of auxiliary agent; the flame retardant comprises a grafted silicone and a perfluorobutyl polymer flame retardant.

[0011] The polycarbonate composition of the present invention adopts grafted silicone and perfluorobutyl polymer flame retardant, and has the performance of low smoke and no dripping; and, in combination with specific polycarbonate, it can achieve high flame retardant performance while improving tensile strength, elongation at break, bending modulus and impact resistance.

[0012] In a specific embodiment of the present invention, the auxiliary agent includes polycarbonate with a melt index of 10 to 12, an anti-drip agent, a release agent and a heat stabilizer.

[0013] In a specific embodiment of the present invention, among the auxiliary agents, the amounts of the anti-dripping agent, the release agent and the heat stabilizer are 1.5% to 2%, 5% to 10% and 1.5% to 2% of the mass of the polycarbonate with a melt index of 10 to 12, respectively.

[0014] In a specific embodiment of the present invention, the preparation of the polymer flame retardant grafted with organosilicon and perfluorobutyl includes: reacting acrylic acid, eugenol-terminated silicone oil and perfluorobutyl sulfonate at 30-60° C. for 1-5 hours.

[0015] In a specific embodiment of the present invention, the mass ratio of the acrylic acid, the eugenol-terminated silicone oil and the perfluorobutyl sulfonate is 1:0.05-0.1:0.005-0.01.

[0016] In a specific embodiment of the present invention, the polycarbonate with a melt index of 6 to 8 is a branched polycarbonate; and the polycarbonate with a melt index of 10 to 12 is a linear polycarbonate.

[0017] In a specific embodiment of the present invention, the polycarbonate composition has a melt index of 5 to 8 g / 10 min, a tensile strength of 65 to 80 MPa, an elongation at break of 100% to 120%, a flexural modulus of 2500 to 3000 MPa, and a notched cantilever beam impact strength of 800 to 900 J / m.

[0018] The present invention also provides a method for preparing any one of the above-mentioned low-smoke, non-drip, halogen-free flame-retardant polycarbonate compositions, comprising the following steps:

[0019] The components are mixed and granulated.

[0020] In a specific embodiment of the present invention, the mixing and granulation comprises using a twin-screw extruder.

[0021] In a specific embodiment of the present invention, the preparation of the auxiliary agent comprises: pre-mixing polycarbonate with a melt index of 10 to 12, an anti-dripping agent, a release agent and a heat stabilizer at a low speed for 60 to 120 seconds, and then mixing at a high speed for 150 to 210 seconds.

[0022] In a specific embodiment of the present invention, the mixing temperature is 40-50°C.

[0023] In a specific embodiment of the present invention, the low speed is 50-70 r / min.

[0024] In a specific embodiment of the present invention, the high speed is 200-400 r / min.

[0025] The present invention also provides use of any one of the above-mentioned low-smoking, non-drip, halogen-free flame-retardant polycarbonate compositions in the preparation of film materials.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] (1) The polycarbonate composition of the present invention adopts grafted silicone and perfluorobutyl polymer flame retardant, compounded with anti-dripping agent, and orderly combines the components together through three-phase grafting and ternary blending to form a more stable system, thereby achieving low smoke and no dripping performance;

[0028] (2) The polycarbonate composition of the present invention, by using a specific polycarbonate, can achieve high flame retardancy while improving tensile strength, elongation at break, flexural modulus, impact resistance, etc., has high fluidity, and can be applied to the fields of films. DETAILED DESCRIPTION

[0029] The technical scheme of the present invention will be clearly and completely described below in conjunction with specific embodiments, but it will be appreciated by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work, all belong to the scope of protection of the present invention. If specific conditions are not indicated in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0030] The low-smoking, non-drip, halogen-free flame-retardant polycarbonate composition is mainly prepared from the following components in parts by weight:

[0031] 24-30 parts of polycarbonate with a melt index of 6-8, 57-63 parts of polycarbonate with a melt index of 10-12, 5-10 parts of flame retardant and 5-8 parts of auxiliary agent; the flame retardant comprises a grafted silicone and a perfluorobutyl polymer flame retardant.

[0032] The polycarbonate composition of the present invention adopts grafted silicone and perfluorobutyl polymer flame retardant, and has the performance of low smoke and no dripping; and, in combination with specific polycarbonate, it can achieve high flame retardant performance while improving tensile strength, elongation at break, bending modulus and impact resistance.

[0033] The unit of melt index (MI) in the present invention is g / 10min, and the test condition is 300°C / 1.2kg.

[0034] For example, in different embodiments, the amounts of the raw material components in the low-smoke, non-drip, halogen-free flame-retardant polycarbonate composition can be as follows:

[0035] The amount of polycarbonate with a melt index of 6 to 8 can be 24 parts, 24.5 parts, 25 parts, 25.5 parts, 26 parts, 26.5 parts, 27 parts, 27.5 parts, 28 parts, 28.5 parts, 29 parts, 29.5 parts, 30 parts, etc.;

[0036] The amount of polycarbonate with a melt index of 10 to 12 can be 57 parts, 57.5 parts, 58 parts, 58.5 parts, 59 parts, 59.5 parts, 60 parts, 60.5 parts, 61 parts, 61.5 parts, 62 parts, 62.5 parts, 63 parts, etc.;

[0037] The amount of flame retardant can be 5 parts, 5.5 parts, 6 parts, 6.5 parts, 7 parts, 7.5 parts, 8 parts, 8.5 parts, 9 parts, 9.5 parts, 10 parts, etc.;

[0038] The dosage of the auxiliary agent can be 5 parts, 5.5 parts, 6 parts, 6.5 parts, 7 parts, 7.5 parts, 8 parts and the like.

[0039] In a specific embodiment of the present invention, the low-smoking, non-drip, halogen-free flame-retardant polycarbonate composition is mainly prepared from the following components in parts by weight:

[0040] 25-28 parts of polycarbonate with a melt index of 6-8, 58-61 parts of polycarbonate with a melt index of 10-12, 6-9 parts of flame retardant and 5.5-7 parts of auxiliary agent.

[0041] In a specific embodiment of the present invention, the low-smoking, non-drip, halogen-free flame-retardant polycarbonate composition is mainly prepared from the following components in parts by weight:

[0042] 26-27 parts of polycarbonate with a melt index of 6-8, 58.5-60 parts of polycarbonate with a melt index of 10-12, 7-8.5 parts of flame retardant and 5.5-6.5 parts of auxiliary agent.

[0043] In a specific embodiment of the present invention, the auxiliary agent includes polycarbonate with a melt index of 10 to 12, an anti-drip agent, a release agent and a heat stabilizer.

[0044] In a specific embodiment of the present invention, among the auxiliary agents, the amounts of the anti-dripping agent, the release agent and the heat stabilizer are 1.5% to 2%, 5% to 10% and 1.5% to 2% of the mass of the polycarbonate with a melt index of 10 to 12, respectively.

[0045] For example, in different embodiments, among the auxiliary agents, the amount of the anti-dripping agent can be 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2% or the like of the mass of the polycarbonate with a melt index of 10 to 12; the amount of the release agent can be 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10% or the like of the mass of the polycarbonate with a melt index of 10 to 12; the amount of the heat stabilizer can be 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2% or the like of the mass of the polycarbonate with a melt index of 10 to 12.

[0046] In a specific embodiment of the present invention, the preparation of the grafted silicone and perfluorobutyl polymer flame retardant includes: the preparation of the grafted silicone and perfluorobutyl polymer flame retardant includes: acrylic acid, eugenol-terminated silicone oil and perfluorobutyl sulfonate react at 30-60°C for 1-5h.

[0047] In a specific embodiment of the present invention, the mass ratio of the acrylic acid, the eugenol-terminated silicone oil and the perfluorobutyl sulfonate is 1:0.05-0.1:0.005-0.01.

[0048] In a specific embodiment of the present invention, the length of the siloxane chain in the eugenol-terminated silicone oil is 40 to 50.

[0049] In a specific embodiment of the present invention, the perfluorobutanesulfonate salt includes one or both of sodium perfluorobutanesulfonate and potassium perfluorobutanesulfonate.

[0050] In a specific embodiment of the present invention, the polycarbonate with a melt index of 6 to 8 is a branched polycarbonate; and the polycarbonate with a melt index of 10 to 12 is a linear polycarbonate.

[0051] In a specific embodiment of the present invention, the polycarbonate having a melt index of 6 to 8 includes Mitsubishi MX 2021; the polycarbonate having a melt index of 10 to 12 includes Lotte PC-1100.

[0052] In a specific embodiment of the present invention, the anti-drip agent includes one or more of SN3307PF, SN3310, SN3308 and SN3300B7; the anti-drip agent can be purchased from Guangzhou Entropy Innovation Materials Co., Ltd.

[0053] In a specific embodiment of the present invention, the release agent includes one or both of SP10S and B50H1; the release agent can be purchased from BASF.

[0054] In a specific embodiment of the present invention, the thermal stabilizer comprises B900 and One or both of B225 and heat stabilizer can be purchased from BASF.

[0055] In a specific embodiment of the present invention, the polycarbonate composition has a melt index of 5 to 8 g / 10 min, a tensile strength of 65 to 80 MPa, an elongation at break of 100% to 120%, a flexural modulus of 2500 to 3000 MPa, and a notched cantilever beam impact strength of 800 to 900 J / m.

[0056] The polycarbonate composition of the present invention has high flame retardancy, high impact resistance, high fluidity and excellent bending performance, and can be applied to the fields of films and the like.

[0057] The present invention also provides a method for preparing any one of the above-mentioned low-smoke, non-drip, halogen-free flame-retardant polycarbonate compositions, comprising the following steps:

[0058] The components are mixed and granulated.

[0059] In a specific embodiment of the present invention, the mixing and granulation comprises using a twin-screw extruder.

[0060] In a specific embodiment of the present invention, the preparation of the auxiliary agent comprises: pre-mixing polycarbonate with a melt index of 10 to 12, an anti-dripping agent, a release agent and a heat stabilizer at a low speed for 60 to 120 seconds, and then mixing at a high speed for 150 to 210 seconds.

[0061] In a specific embodiment of the present invention, the mixing temperature is 40-50°C.

[0062] In a specific embodiment of the present invention, the low speed is 50-70 r / min.

[0063] In a specific embodiment of the present invention, the high speed is 200-400 r / min.

[0064] The present invention also provides use of any one of the above-mentioned low-smoking, non-drip, halogen-free flame-retardant polycarbonate compositions in the preparation of film materials.

[0065] The low-smoke, non-drip, halogen-free flame-retardant polycarbonate composition of the present invention has high flame-retardant performance, high impact resistance, high fluidity, thermal deformation performance and bending performance, and can be used in the fields of films and the like.

[0066] Examples 1 to 6

[0067] This embodiment provides a plurality of low-smoke, drip-free, halogen-free flame-retardant polycarbonate compositions and preparation methods thereof, wherein the raw material information of the low-smoke, drip-free, halogen-free flame-retardant polycarbonate compositions of each embodiment is shown in Table 1 and Table 2, and the preparation method comprises the following steps:

[0068] (1) Anti-drip agent SN3307PF, release agent SP10S, thermal stabilizer B900 and polycarbonate with a melt index of 10-12 (PC-MI 10-12) were mixed in a mixer at 45° C., first at 60 rpm for 90 seconds, and then at 300 rpm for 180 seconds to obtain an additive premix.

[0069] (2) Weighing polycarbonate with a melt index of 6 to 8 (PC-MI 6-8), polycarbonate with a melt index of 10 to 12 (PC-MI 10-12), grafted silicone and perfluorobutyl polymer flame retardant and the auxiliary agent premix obtained in step (1) according to a ratio, mixing and granulating; specifically, mixing and granulating comprises: extruding and granulating in a twin-screw extruder, the die head temperature of the twin-screw extruder is 280° C., the temperature of zone 2 is 150° C., the temperature of zone 3 is 200° C., the temperature of zone 4 is 250° C., the temperature of zone 5 is 280° C., the temperature of zone 6 is 280° C., the temperature of zone 7 is 280° C., the temperature of zone 8 is 280° C., the temperature of zone 9 is 260° C., and the temperature of zone 10 is 260° C.; the speed of the screw is 550 rpm.

[0070] Table 1 Raw material information of each low-smoking, non-drip, halogen-free flame-retardant polycarbonate composition (parts by weight)

[0071] Components Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 PC-MI 6~8 26.86 copies 24 servings 30 servings 27 servings 27 servings 27 servings PC-MI 10~12 59.138 copies 63 copies 57 copies 59 copies 59 copies 59 copies Polymer flame retardant 7.935 copies 5 servings 8 servings 8 servings 8 servings 8 servings Additive premix 6.067 copies 8 servings 5 servings 6 servings 6 servings 6 servings

[0072] Table 2 Mass percentage of each component in the additive premix of each embodiment of PC-MI 10-12

[0073] Premix ingredients Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Anti-drip agent F491 1.86% 1.86% 1.86% 1.5% 2% 1.8% Release agent F538 7.1525% 7.1525% 7.1525% 10% 5% 10% Heat stabilizer F542 1.839% 1.839% 1.839% 1.5% 2% 2% PC-MI 10~12 — — — — — —

[0074] Note: The “—” in Table 2 means that when calculating the proportion of each component in the additive premix, PC-MI10~12 in the additive premix is ​​used as the basis, which is equivalent to the amount of PC-MI 10~12 being 100%.

[0075] PC-MI 6~8 are Mitsubishi MX 2021.

[0076] PC-MI 10~12 is Lotte PC-1100.

[0077] The preparation of the polymer flame retardant grafted with silicone and perfluorobutyl includes: acrylic acid, eugenol-terminated silicone oil and perfluorobutyl sulfonate in a mass ratio of 1:0.08:0.007 are reacted at 50°C for 2 hours; the length of the siloxane chain in the eugenol-terminated silicone oil is 40 to 50.

[0078] Comparative Example 1

[0079] The polycarbonate provided in this comparative example is 945-701.

[0080] Experimental Example 1

[0081] In order to compare and illustrate the performance of the polycarbonate compositions prepared in different embodiments and comparative examples, the performance of the polycarbonate compositions prepared in various embodiments and comparative examples were tested. The test results are shown in Table 3.

[0082] Among them, the test conditions of melt index MI are 300℃ / 1.2kg, refer to ISO 1133-1;

[0083] The test conditions for tensile strength TS are 50 mm / min, refer to ISO 527-2;

[0084] The test condition of elongation at break EL is 50 mm / min, refer to ISO 527-2;

[0085] The test condition of flexural modulus EF is 2 mm / min, refer to ISO 178;

[0086] Izod impact strength (notched), test condition 25°C, refer to ASTM D256.

[0087] Table 3 Test results of different polycarbonate compositions

[0088]

[0089] From the above test results, it can be seen that the low-smoke, drip-free, halogen-free flame-retardant polycarbonate composition of the present invention can achieve high flame retardant properties while improving tensile strength, elongation at break, flexural modulus and impact resistance, etc., has high fluidity, and can be applied to films and other fields.

[0090] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A low-smoke, non-drip, halogen-free flame-retardant polycarbonate composition, characterized in that: It is mainly made of the following components by weight: 24-30 parts of polycarbonate with a melt index of 6-8, 57-63 parts of polycarbonate with a melt index of 10-12, 5-10 parts of flame retardant and 5-8 parts of auxiliary agent; the flame retardant includes a grafted silicone and a perfluorobutyl polymer flame retardant; The preparation of the grafted silicone and perfluorobutyl polymer flame retardant comprises: reacting acrylic acid, eugenol-terminated silicone oil and perfluorobutyl sulfonate at 30-60° C. for 1-5 hours; The mass ratio of the acrylic acid, the eugenol-terminated silicone oil and the perfluorobutyl sulfonate is 1:0.05-0.1:0.005-0.01; The siloxane chain length in the eugenol-terminated silicone oil is 40 to 50; The auxiliary agent includes polycarbonate with a melt index of 10 to 12, an anti-drip agent, a release agent and a heat stabilizer; Among the auxiliary agents, the amounts of the anti-dripping agent, the release agent and the heat stabilizer are 1.5% to 2%, 5% to 10% and 1.5% to 2% of the mass of the polycarbonate with a melt index of 10 to 12, respectively; The polycarbonate with a melt index of 6 to 8 is a branched polycarbonate; the polycarbonate with a melt index of 10 to 12 is a linear polycarbonate; The polycarbonate composition has a melt index of 5 to 8 g / 10 min, a tensile strength of 65 to 80 MPa, an elongation at break of 100% to 120%, a flexural modulus of 2500 to 3000 MPa, and a notched cantilever beam impact strength of 800 to 900 J / m.

2. The low-smoke, no-drip, halogen-free flame-retardant polycarbonate composition according to claim 1, characterized in that: It is mainly made of the following components by weight: 26-27 parts of polycarbonate with a melt index of 6-8, 58.5-60 parts of polycarbonate with a melt index of 10-12, 7-8.5 parts of flame retardant and 5.5-6.5 parts of auxiliary agent.

3. The method for preparing the low-smoking, non-drip, halogen-free flame-retardant polycarbonate composition according to claim 1 or 2, characterized in that: The steps include: The components are mixed and granulated.

4. The method for preparing the low-smoke, no-drip, halogen-free flame-retardant polycarbonate composition according to claim 3, characterized in that: The mixing and granulation comprises using a twin-screw extruder.

5. The method for preparing the low-smoke, no-drip, halogen-free flame-retardant polycarbonate composition according to claim 4, characterized in that: The preparation of the auxiliary agent comprises: pre-mixing polycarbonate with a melt index of 10 to 12, an anti-dripping agent, a release agent and a heat stabilizer at a low speed for 60 to 120 seconds, and then mixing at a high speed for 150 to 210 seconds.

6. The method for preparing the low-smoke, no-drip, halogen-free flame-retardant polycarbonate composition according to claim 5, characterized in that: The mixing temperature is 40-50°C; The low speed is 50-70 r / min; The high speed is 200-400r / min.

7. Use of the low-smoking, non-drip, halogen-free flame-retardant polycarbonate composition according to claim 1 or 2 in the preparation of film materials.

Citation Information