A preparation method of an ultra-sensitive MEMS VOCs gas sensor and a micro-pad printing device used therein
By preparing gas-sensitive material powder and slurry, using the pad printing process to form a gas-sensitive film on the MEMS microheater substrate, and performing annealing treatment and ceramic packaging, the problem of rapid response and mass production of MEMS VOCs gas sensors is solved. Achieving high sensitivity and effective detection of low-concentration VOCs gases.
Patent Information
- Application Number
- CN202210521750.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-13
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-05-13
AI Technical Summary
Existing MEMS VOCs gas sensors have challenges in rapid response and large-scale mass production, and the issues of sensitivity and gas cross-interference have not yet been fully resolved.
Gas-sensitive material powder is prepared using raw materials such as tin tetrachloride, nitrate, and deionized water. It is printed on the MEMS microheater substrate through a pad printing process to form a gas-sensitive film, and is annealed and ceramic encapsulated to improve the gas-sensing performance. Specific surface area and bonding properties of materials.
An ultra-sensitive MEMS VOCs gas sensor is realized with fast response and high sensitivity, suitable for large-scale mass production, and improves the detection capability of low-concentration VOCs gases.
Smart Images

Figure CN114778617B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of MEMS gas sensors, and in particular to a method for preparing an ultra-sensitive MEMS VOCs gas sensor and a micro pad printing device used therein. Background Art
[0002] VOCs (Volatile Organic Compounds) refers to a class of volatile organic compounds with a boiling point of less than 260°C at normal pressure and a saturated vapor pressure of more than 70.91Pa at room temperature. From the perspective of environmental monitoring, VOCs refers to the general term for non-methane total hydrocarbons detected by gas chromatography with a hydrogen flame ionization detector, mainly including alkanes, aromatics, olefins, aldehydes, ketones and other related organic compounds. Most VOCs are toxic, and some VOCs are carcinogenic. For example, some benzene and polycyclic aromatic hydrocarbons in the atmosphere can induce true tumors in the body and endanger people's health.
[0003] VOCs are mainly generated from fossil energy (coal, oil and natural gas) or industries that use fossil energy as fuel or raw materials and their related chemical industries. Among them, VOCs outdoors mainly come from fuel combustion and transportation; indoors they mainly come from combustion products such as coal and natural gas, fumes from heating and cooking, emissions from building and decoration materials, furniture, household appliances, detergents and the human body.
[0004] In August 2021, the Ministry of Ecology and Environment issued the "Notice on Accelerating the Resolution of Current Outstanding Issues in Volatile Organic Compounds Governance", proposing to fight a tough battle against pollution. The main goals and tasks include continuously improving environmental governance and basically eliminating heavy pollution weather. In terms of pollutant emission indicators, SO2 and NO x Replaced with VOCs and NO x The development direction of VOCs governance in my country has transitioned from extensive governance in the early stage to refined and in-depth governance. Refined and in-depth governance of VOCs is urgent in my country. As an evaluation method for VOCs governance, accurate and continuous VOCs monitoring is a necessary prerequisite for the effective implementation of the national VOCs pollution prevention and control plan.
[0005] At present, the main methods used for VOCs detection and monitoring are gas chromatography (GC), gas chromatography-mass spectrometry (GC-MS), gas chromatography-flame ionization detection (GC-FID), high performance liquid chromatography (HPLC), Fourier transform infrared spectroscopy (FTIR) and other methods. Among them, online gas chromatography-mass spectrometry / flame ionization detector has the advantages of high sensitivity and time resolution, and comprehensive detection of species. It is the main automatic monitoring method currently used at home and abroad. However, the equipment used in the above-mentioned VOCs detection and monitoring methods is large and inconvenient to carry. At the same time, there are also problems such as lengthy steps from sample collection to instrument analysis, and difficult rapid detection. In the face of the full development of VOCs monitoring, it is necessary to further improve the existing detection and detection methods or develop new detection methods to meet the current and future needs of rapid detection and monitoring.
[0006] MEMS semiconductor gas sensors came into being in response to the needs of miniaturization and rapid detection of VOCs detection and monitoring equipment. People combine microelectromechanical systems (MEMS) with categories such as semiconductor gas sensors. The developed MEMS semiconductor gas sensors have a series of advantages such as small size, high sensitivity, and fast response rate. At the same time, the development and application of technologies such as screen printing and magnetron sputtering in recent years have made the industrialization of MEMS semiconductor gas sensors possible. However, there are still some urgent problems to be solved in the industrialization of MEMS semiconductor gas sensors. For example, MEMS semiconductor gas sensors still have gas cross-interference, and the life of gas-sensitive materials needs to be further improved. In response to the detection needs of certain specific TVOCs, the sensitivity of MEMS semiconductor gas sensors needs to be further improved, etc.
[0007] There are not many patent reports on ultra-sensitive MEMS VOCs gas sensors. Patent CN107607591B discloses an ultra-sensitive toluene gas sensor based on SnO2-modified NiO nanostructured sensitive material and its preparation method. The method uses N-type SnO2 semiconductor material to modify P-type NiO semiconductor sensitive material, prepares nanostructured material powder by hydrothermal method, grinds and dips to form a sensitive material film, and finally prepares a gas sensor. It exhibits excellent selectivity and moisture resistance for toluene, as well as ultra-high sensitivity (60.2-100ppm) and extremely low detection limit (10ppb). However, its preparation method is lengthy, and its low concentration sensitivity still needs to be improved. Patent CN111017986A discloses a method for preparing a reduced graphene oxide-CuO / ZnO gas-sensitive material, which is prepared by mixing a copper-zinc precursor solution and a reduced graphene oxide colloidal solution, performing hydrothermal reaction, and annealing to obtain a gas-sensitive material. The prepared sensor has enhanced selectivity for acetone gas in the low temperature range. However, ammonia needs to be continuously introduced during the annealing process. At the same time, the addition of graphene oxide makes the device response time longer, and only the sensitivity of a single component gas is enhanced, which limits the application scenarios.
[0008] In order to achieve the rapid response of MEMS VOCs gas sensors and enable them to be applied to more ultra-sensitive application scenarios, the present invention proposes a method for preparing an ultra-sensitive MEMS VOCs gas sensor. The porous gas-sensitive material in the present invention is easy to prepare, the prepared pad printing slurry has good bonding performance, the pad printing process is used instead of the screen printing process, the sensitive material has a thinner structure, the prepared MEMS VOCs gas sensor has ultra-sensitive performance, and has the potential for large-scale batch production. It is a method for preparing an ultra-sensitive MEMS VOCs gas sensor with strong applicability. Summary of the invention
[0009] The technical problem to be solved by the present invention is how to provide a method for preparing an ultra-sensitive MEMS VOCs gas sensor, which has the advantages of fast response and strong applicability and is suitable for large-scale batch production.
[0010] The present invention solves the above technical problems through the following technical means:
[0011] On the one hand, the present invention provides a method for preparing an ultra-sensitive MEMS VOCs gas sensor, comprising the following specific steps:
[0012] S1. Preparation of gas-sensitive material powder
[0013] Mix and stir tin tetrachloride, nitrate and deionized water until they are completely dissolved, then uniformly mix the mixed solution with an organic solvent to form a mixed solution, then add 0.5-2% of a dispersant relative to the total mass of the mixed solution and stir evenly; then transfer the obtained dispersion to a reactor and let it stand at 60-100°C for 6-18h; finally, wash the mixture with ethanol by centrifugation and dry it in an oven to obtain a gas-sensitive material powder;
[0014] S2. Preparation of gas-sensitive material slurry
[0015] The gas-sensitive material powder, silica sol, polyamide resin and organic solvent prepared above are uniformly mixed to form a suspension; the suspension is then sand-milled to obtain a gas-sensitive material slurry;
[0016] S3, pad printing interdigitated electrodes
[0017] The prepared gas-sensitive material slurry is transferred to the interdigital electrodes of the MEMS micro-heater substrate using a micro-pad printing device, and the interdigital electrodes are completely covered; after the pad printing is completed, it is placed in an oven for baking to form a gas-sensitive film on the MEMS micro-heater substrate.
[0018] S4. Device annealing
[0019] The MEMS substrate printed with the sensitive material slurry is placed in a muffle furnace for annealing, and then cut to obtain a MEMS sensor chip.
[0020] S5, gold wire ball welding, ceramic packaging
[0021] The prepared MEMS sensor chip is subjected to gold wire ball welding and ceramic packaging to finally obtain a MEMS VOCs gas sensor.
[0022] Beneficial effects: The present application prepares a powdered gas-sensitive material by mixing, dissolving, reacting and drying raw materials such as tin tetrachloride, nitrate, deionized water and a dispersant; then mixing the gas-sensitive material powder with silica sol, polyamide resin, an organic solvent and the like into a suspension, and sand-milling the suspension to obtain a slurry-like gas-sensitive material; then transferring the obtained gas-sensitive material slurry to the interdigital electrodes of a MEMS microheater substrate by a pad printing process, and baking to form a gas-sensitive film; annealing and cutting to obtain a MEMS sensor chip, and finally performing gold wire ball welding and ceramic packaging to obtain a MEMS VOCs gas sensor.
[0023] In the present application, the gas-sensitive material is first prepared into a powder, then into a slurry, and then printed onto a MEMS microheater substrate through a pad printing process to form a thinner gas-sensitive film to obtain a MEMS VOCs gas sensor with ultra-sensitive performance; and in the process of preparing the gas-sensitive slurry, the formed suspension is sanded to effectively prevent the gas-sensitive material from agglomerating, thereby ensuring the integrity of the microstructure of the gas-sensitive material, and further ensuring the ultra-sensitive performance of the gas-sensitive material.
[0024] The silica sol, polyamide resin, organic solvent, etc. of the present invention make the gas-sensitive material slurry have good bonding properties, improve the firmness of the connection between the gas-sensitive film and the MEMS micro-heater substrate, and ensure the gas-sensitive detection effect.
[0025] After the device of the present application is annealed, a porous structure is formed on the gas-sensitive film, thereby increasing the specific surface area of the gas-sensitive material, which is beneficial to the contact area between the gas and the gas-sensitive material, and further improving the sensitivity of gas-sensitive detection.
[0026] Preferably, in step S1, the mass ratio of tin tetrachloride, nitrate and deionized water is 20:8-12:70.
[0027] Preferably, in step S1, the mass ratio of the three components after mixing to the organic solvent is 20:50-50:20.
[0028] Preferably, the nitrate in step S1 is one or more combinations of zinc nitrate, nickel nitrate, copper nitrate, chromium nitrate and cobalt nitrate.
[0029] Preferably, the organic solvent in step S1 is one or more combinations of ethanol and acetone.
[0030] Preferably, the dispersant in step S1 is one or more combinations of polyvinyl pyrrolidone 1000, polyethylene glycol, polyvinyl alcohol, polyethylene oxide, and carboxymethyl cellulose.
[0031] Preferably, the oven drying temperature in step S1 is 60-80°C.
[0032] Preferably, the organic solvent in step S2 is one or more combinations of diisobutyl ketone, ethyl triethoxypropionate, and propylene carbonate.
[0033] Preferably, in step S2, the mass ratio of the gas-sensitive material powder, silica sol, polyamide resin and organic solvent is 5:1:15:80.
[0034] Preferably, in step S2, the particle size D90 of the suspension after sand grinding is less than 500 nm.
[0035] Preferably, the micro pad printing device in step S3 includes a base, a gravure plate, a moving component and a transfer component, the gravure plate is engraved with a pattern to be printed and is coated with a sensitive material, and the gravure plate and the MEMS substrate are both placed on the base; the moving component drives the transfer component to move from the gravure plate position to the MEMS substrate, the transfer component includes a planar pad head and an alignment camera fixedly mounted on the moving component, the sensitive material on the gravure plate is transferred to the MEMS substrate through the pad head, and the alignment camera aligns the pad head with the corresponding positions of the gravure plate and the MEMS substrate.
[0036] Beneficial effects: When in use, after placing the MEMS substrate on the base, start the moving component to move the pad head to the top of the gravure plate, compare and adjust the position of the pad head through the alignment camera until the pad head is aligned with the gravure plate, then move down and dip the sensitive material; then continue to control the moving component to move the pad head to the top of the MEMS substrate, also compare and adjust the position of the pad head through the alignment camera until the pad head is aligned with the corresponding position of the MEMS substrate, and move down to transfer the sensitive material to the MEMS substrate, thereby achieving high-precision printing of thinner sensitive materials.
[0037] Preferably, the baking temperature in step S3 is 60-80° C. and the baking time is 30-40 min.
[0038] Preferably, the thickness of the gas-sensitive film after baking in step S3 is 1-5 μm.
[0039] Preferably, the annealing temperature in step S4 is 350-450° C. and the time is 2-3 h.
[0040] On the other hand, the present invention provides a micro-pad printing device for preparing the above-mentioned ultra-sensitive MEMS VOCs gas sensor. The micro-pad printing device includes a base, a gravure plate, a moving component and a transfer component. The gravure plate is engraved with a pattern to be printed and is coated with a sensitive material. The gravure plate and the MEMS substrate are both placed on the base; the moving component drives the transfer component to move from the gravure plate position to the MEMS substrate. The transfer component includes a planar pad printing head and an alignment camera fixedly mounted on the moving component. The sensitive material on the gravure plate is transferred to the MEMS substrate through the pad printing head. The alignment camera aligns the pad printing head with the corresponding positions of the gravure plate and the MEMS substrate.
[0041] The advantages of the present invention are:
[0042] 1. In the present application, the gas-sensitive material is first prepared into a powder, then into a slurry, and then printed onto a MEMS microheater substrate through a pad printing process to form a thinner gas-sensitive film to obtain a MEMS VOCs gas sensor with ultra-sensitive performance; and in the process of preparing the gas-sensitive slurry, the formed suspension is sand-milled to effectively prevent the gas-sensitive material from agglomerating, thereby ensuring the integrity of the microstructure of the gas-sensitive material, and further ensuring the ultra-sensitive performance of the gas-sensitive material.
[0043] 2. The silica sol, polyamide resin, organic solvent, etc. of the present application make the gas-sensitive material slurry have good bonding properties, improve the firmness of the connection between the gas-sensitive film and the MEMS micro-heater substrate, and ensure the gas-sensitive detection effect.
[0044] 3. After annealing treatment, a porous structure is formed on the gas-sensitive film of the device of the present application, thereby increasing the specific surface area of the gas-sensitive material, which is beneficial to the contact area between the gas and the gas-sensitive material, and further improving the sensitivity of gas-sensitive detection.
[0045] 4. This application utilizes a moving component to move the pad head between the gravure plate and the MEMS substrate, and uses an alignment camera to accurately adjust the position of the pad head, so that the pad head dips the sensitive material from the gravure plate and then transfers it to the MEMS substrate, thereby achieving high-precision printing of thinner sensitive materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 Schematic diagram of the overall structure of the micro pad printing device in Example 1 of the present invention.
[0047] Figure 2 This is the response recovery curve of the MEMS gas sensor prepared in Example 2 of the present invention to 20 ppm ethanol.
[0048] Figure 3 This is the response recovery curve of the MEMS gas sensor prepared in Example 2 of the present invention to 1 ppm ethanol.
[0049] Figure 4 This is a sensitivity characteristic curve diagram of the MEMS gas sensor prepared in Example 2 of the present invention.
[0050] Explanation of the reference numerals in the accompanying drawings: 1. base; 11. base; 12. support table; 121. slide; 13. sample table; 14. adjustment bracket; 15. cleaning roller; 2. gravure; 21. roller rack; 22. ink roller; 3. moving assembly; 31. X-axis guide rail; 32. Y-axis guide rail; 33. Z-axis guide rail; 34. displacement block; 35. motor; 4. transfer assembly; 41. pad printing head; 42. alignment camera; 43. alignment mark; 5. MEMS substrate; 6. negative pressure device; 61. sample box; 62. negative pressure suction port; 63. dust collection bag; 64. vacuum nozzle; 65. heater. DETAILED DESCRIPTION
[0051] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0052] The present application embodiment discloses a method for preparing an ultra-sensitive MEMS VOCs gas sensor, comprising the following specific steps:
[0053] S1. Preparation of gas-sensitive material powder
[0054] Tin tetrachloride, nitrate and deionized water are stirred at a speed of 600 rpm in a ratio of 20:8-12:70 until they are completely dissolved; then the above solution and organic solvent are mixed in a mass ratio of 20:50-50:20 to form a mixed solution, 0.5-2% of a dispersant relative to the total mass of the above mixed solution is added, and then stirred at a speed of 600 rpm for 30 minutes; then the obtained dispersion is transferred to a reactor and allowed to stand at 60-100°C for 6-18 hours; finally, the mixture is centrifuged and washed with ethanol, placed in an oven at 60-80°C for drying, and finally a gas-sensitive material powder is obtained.
[0055] Among them, the nitrate is one or more combinations of zinc nitrate, nickel nitrate, copper nitrate, chromium nitrate, and cobalt nitrate; the organic solvent is one or more combinations of ethanol and acetone; and the dispersant is one or more combinations of polyvinyl pyrrolidone 1000, polyethylene glycol, polyvinyl alcohol, polyethylene oxide, and carboxymethyl cellulose.
[0056] S2. Preparation of gas-sensitive material slurry
[0057] The gas-sensitive material powder prepared above: silica sol: polyamide resin: organic solvent are uniformly mixed in a mass ratio of 5:1:15:80 to form a suspension; the suspension is sand-milled to control the particle size D90 to be less than 500 nm to obtain a gas-sensitive material slurry.
[0058] The organic solvent is one or more combinations of diisobutyl ketone, ethyl triethoxypropionate and propylene carbonate.
[0059] S3, pad printing interdigitated electrodes
[0060] The prepared gas-sensitive material slurry is transferred to the interdigital electrodes of the MEMS microheater substrate using a micro pad printing device, and the interdigital electrodes are completely covered; after pad printing, the slurry is placed in an oven at 60-80°C and baked for 30-40 minutes; the thickness of the baked gas-sensitive film is 1-5μm.
[0061] S4. Device annealing
[0062] The MEMS substrate printed with the sensitive material slurry is placed in a muffle furnace and annealed at 350-450°C for 2-3 hours. After the annealing is completed, cutting is performed to obtain a MEMS sensor chip.
[0063] S5, gold wire ball welding, ceramic packaging
[0064] The prepared MEMS sensor chip is subjected to gold wire ball welding and ceramic packaging to finally obtain a MEMS VOCs gas sensor.
[0065] Example 1
[0066] The present application embodiment discloses a method for preparing an ultra-sensitive MEMS VOCs gas sensor, comprising the following specific steps:
[0067] S1. Preparation of gas-sensitive material powder
[0068] Tin tetrachloride, zinc nitrate, nickel nitrate and deionized water are stirred at a speed of 600 rpm in a ratio of 20:5:5:70 until they are completely dissolved; then the above solution and ethanol are mixed in a mass ratio of 50:20 to form a mixed solution, 1% of polyvinyl pyrrolidone relative to the total mass of the above mixed solution is added, and then stirred at a speed of 600 rpm for 30 minutes; then the obtained dispersion is transferred to a reactor and allowed to stand at 80°C for 12 hours; finally, the mixture is centrifuged and washed with ethanol, placed in an oven at 80°C for drying, and finally a gas-sensitive material powder is obtained.
[0069] S2. Preparation of gas-sensitive material slurry
[0070] The gas-sensitive material powder prepared above: silica sol: polyamide resin: diisobutyl ketone are uniformly mixed in a mass ratio of 5:1:15:80 to form a suspension; the suspension is sand-milled to control the particle size D90 to be less than 200 nm to obtain a gas-sensitive material slurry.
[0071] S3, pad printing interdigitated electrodes
[0072] The prepared gas-sensitive material slurry was transferred to the interdigital electrodes of the MEMS microheater substrate using a micro pad printing device, and the interdigital electrodes were completely covered; after pad printing, the slurry was placed in an oven and baked at 80°C for 30 minutes; the thickness of the gas-sensitive film after baking was 1 μm.
[0073] S4. Device annealing
[0074] The MEMS substrate printed with the sensitive material slurry is placed in a muffle furnace and annealed at 400°C for 2 hours. After the annealing is completed, the substrate is cut to obtain a MEMS sensor chip.
[0075] S5, gold wire ball welding, ceramic packaging
[0076] The prepared MEMS sensor chip is subjected to gold wire ball welding and ceramic packaging to finally obtain a MEMS VOCs gas sensor.
[0077] The present application also discloses a micro pad printing device for preparing the above-mentioned ultra-sensitive MEMS VOCs gas sensor, such as Figure 1 As shown, the micro pad printing device includes a base 1, a gravure 2, a moving component 3, a transfer component 4, a MEMS substrate 5 and a negative pressure device 6. The base 1 includes a base 11, a support table 12, a sample table 13 and an adjustment bracket 14. The support table 12 and the adjustment bracket 14 are both fixedly connected to the base 11, the gravure 2 is fixedly placed on the support table 12, and the transfer component 4 is slidably connected to the adjustment bracket 14 through the moving component 3. The sample table 13 is slidably set on the base 11, and the MEMS substrate 5 is fixedly placed on the sample table 13. The MEMS substrate 5 is etched with cutting paths to form a plurality of grid units, each of which is a chip with interdigitated electrodes. The micro pad printing device is suitable for pad printing operations of 6-8 inch silicon wafers.
[0078] The gravure plate 2 includes a single crystal silicon wafer and an oxide layer, the oxide layer is deposited on the surface of the single crystal silicon wafer, and the surface of the oxide layer is etched by a mask to form a pattern to be printed and an alignment mark 43. The oxide can be selected from one or more of silicon nitride, gallium arsenide, silicon oxide, and gallium nitride, which effectively improves the mechanical strength of the gravure plate 2. Silicon nitride is selected in this embodiment; the thickness of the gravure plate 2 is 500μm-2mm, and 1mm is selected in this embodiment.
[0079] A slide groove 121 is provided on the side wall of the support platform 12, and a roller frame 21 is slidably arranged in the slide groove 121. The roller frame 21 is located on both sides of the gravure plate 2, and the top of the roller frame 21 extends upward from the top surface of the gravure plate 2. An ink roller 22 is detachably mounted on the roller frame 21, and the ink roller 22 is rotatably connected to the roller frame 21. When the roller frame 21 slides along the support platform 12, the ink roller 22 rolls on the top surface of the gravure plate 2, thereby evenly brushing the sensitive material on the gravure plate 2. When the ink roller 22 of different diameters is replaced, or the rotation speed of the ink roller 22 is further controlled by controlling the sliding speed of the roller frame 21, the thickness of the sensitive material can be changed, and the structure is simple and easy to operate.
[0080] The moving assembly 3 includes an X-axis guide rail 31, a Y-axis guide rail 32, a Z-axis guide rail 33 and a displacement block 34, wherein the X-axis guide rail 31 and the Y-axis guide rail 32 are both screw rods, and the Z-axis guide rail 33 is a cylinder. The X-axis guide rail 31 is rotatably arranged on the adjustment bracket 14, and the displacement block 34 is threadedly sleeved on the X-axis guide rail 31; the cylinder body of the Z-axis guide rail 33 is fixedly installed on the displacement block 34, the telescopic rod of the cylinder extends downward, and the transfer assembly 4 is fixedly installed at the bottom end of the telescopic rod. A motor 35 is fixedly installed on the adjustment bracket 14, and the output shaft of the motor 35 is fixedly connected to the X-axis guide rail 31. When the motor 35 rotates, the motor 35 drives the X-axis guide rail 31 to rotate, and at this time, the displacement block 34 and the X-axis guide rail 31 are threadedly matched to move horizontally, thereby driving the transfer assembly 4 to move horizontally on the horizontal plane; when the cylinder is started, the Z-axis guide rail 33 drives the transfer assembly 4 to move up and down, thereby realizing the adjustment of the position of the transfer assembly 4.
[0081] The Y-axis guide rail 32 is rotatably arranged on the base 11, and the sample stage 13 is threadedly connected to the Y-axis guide rail 32. A motor 35 is fixedly installed on the base 11, and the output shaft of the motor 35 is fixedly connected to the Y-axis guide rail 32. When the motor 35 rotates, the motor 35 drives the Y-axis guide rail 32 to rotate, and at this time, the sample stage 13 and the Y-axis guide rail 32 are threadedly matched to move horizontally, thereby driving the MEMS substrate 5 to move longitudinally on the horizontal plane, so as to adjust the position of the MEMS substrate 5.
[0082] The transfer assembly 4 includes a pad printing head 41 and an alignment camera 42, both of which are fixedly mounted at the bottom end of the Z-axis guide rail 33. The pad printing head 41 is a planar sheet structure made of polyimide material, which has good flexibility and light transmission performance. The alignment camera 42 adopts a high-definition CCD camera, which is installed above the pad printing head 41. An alignment mark 43 is etched at the center of the top surface of the gravure 2, and an alignment mark 43 is also printed on the top surface of the corresponding position of the pad printing head 41. The alignment mark 43 is in a cross shape, and the pad printing head 41 is aligned with the gravure 2 through the fixed alignment mark 43. Four alignment marks 43 are respectively provided at corresponding positions of the gravure plate 2 and the MEMS substrate 5. When the pad printing head 41 dips the sensitive material on the gravure plate 2, the alignment mark 43 of the gravure plate 2 is printed on the pad printing head 41. When the pad printing head 41 moves above the MEMS substrate 5, the four alignment marks 43 of the pad printing head 41 are aligned with the four alignment marks 43 on the MEMS substrate 5, thereby realizing the alignment of the pad printing head 41 and the MEMS substrate 5.
[0083] When in use, after placing the MEMS substrate 5 and the gravure plate 2, the sliding roller frame 21 makes the ink roller 22 roll on the gravure plate 2 so that the sensitive material is evenly brushed on the gravure plate 2; then the motor 35 on the adjustment bracket 14 is started, and the driving action of the X-axis guide rail 31 makes the pad printing head 41 move horizontally to the top of the gravure plate 2, and at the same time, through the alignment camera 42 for comparison and observation, the alignment mark 43 on the pad printing head 41 is aligned with the alignment mark 43 on the gravure plate 2; then the Z-axis guide rail 33 is started to move the pad printing head 41 downward, and dip the sensitive material on the gravure plate 2, at this time, the alignment mark 43 pattern on the gravure plate 2 is printed on the pad printing head 41 together; continue to control the X-axis guide rail 31 and the Z-axis guide rail 33, so that the pad printing head 41 moves to the top of the MEMS substrate 5, and also through the alignment camera 42 for comparison and observation, at this time, the motor 35 on the base 11 is started, and the Y The Z-axis guide 32 drives the sample stage 13 to move forward and backward until the four alignment marks 43 printed on the pad head 41 are aligned one by one with the four alignment marks 43 on the MEMS substrate 5, and then the Z-axis guide 33 is started to move the pad head 41 downward, so that the sensitive material can be transferred to the MEMS substrate 5, thereby achieving high-precision coating of thinner sensitive materials.
[0084] A cleaning roller 15 is rotatably provided on the base 1, and the cleaning roller 15 is located between the support table 12 and the sample table 13. After the pad printing head 41 transfers the sensitive material to the MEMS substrate 5, the pad printing head 41 is moved to the position of the cleaning roller 15 by the moving component 3. The cleaning roller 15 can be rotated to clean the sensitive material remaining on the pad printing head 41, so that the pad printing head 41 remains clean for the next printing.
[0085] The negative pressure device 6 includes a sample box 61, a negative pressure suction port 62, a dust collection bag 63, a vacuum suction nozzle 64 and a heater 65. The sample box 61 is fixedly mounted on the sample stage 13, and the vacuum suction nozzle 64 is fixedly mounted on the inner bottom surface of the sample box 61. There are multiple vacuum suction nozzles 64, and four are used in this embodiment. The MEMS substrate 5 is fixed in the sample box 61 by suction through the vacuum suction nozzle 64, which prevents the MEMS substrate 5 from moving during the pad printing process, further ensuring the pad printing effect.
[0086] The top of the sample box 61 is provided with an opening, and the transfer assembly 4 enters and exits the sample box 61 through the opening to achieve the transfer of the MEMS substrate 5. The opening position of the sample box 61 is slidably provided with an opening and closing cover. When the transfer assembly 4 does not need to enter the sample box 61, the opening and closing cover of the sample box 61 remains in a closed state. The negative pressure suction port 62 is fixedly installed on the inner wall of the sample box 61. There are multiple negative pressure suction ports 62, and 4 are taken in this embodiment. The small mouth end of the dust collection bag 63 is connected to the negative pressure suction port 62 through a pipeline, and the large mouth end extends out of the sample box 61. When the transfer assembly 4 does not need to enter the sample box 61, the opening and closing cover remains in a closed state, and at the same time, the negative pressure suction port 62 continuously sucks out the dust in the sample box 61, and is discharged by the dust collection bag 63, which effectively ensures the cleanliness of the surface of the MEMS substrate 5 and prevents dust from contaminating the MEMS substrate 5 and affecting the coating quality. A heater 65 is installed at the bottom of the sample box 61. After the pad printing is completed, the heater 65 is started to bake the MEMS substrate 5, which is beneficial to accelerate the drying of the sensitive material of the pad printing.
[0087] When in use, after placing the MEMS substrate 5 and the gravure plate 2, the sliding roller frame 21 makes the ink roller 22 roll on the gravure plate 2, so that the sensitive material is evenly brushed on the gravure plate 2; then the motor 35 on the adjustment bracket 14 is started, and the driving action of the X-axis guide rail 31 makes the pad printing head 41 move horizontally to the top of the gravure plate 2, and at the same time, the alignment mark 43 on the pad printing head 41 is aligned with the alignment mark 43 on the gravure plate 2 through comparison and observation by the alignment camera 42; then the Z-axis guide rail 33 is started. Move the pad head 41 downward and dip the sensitive material on the gravure plate 2; continue to control the X-axis guide rail 31 and the Z-axis guide rail 33 to move the pad head 41 above the MEMS substrate 5, and also compare and observe through the alignment camera 42. At this time, start the motor 35 on the base 11, and drive the sample stage 13 to move back and forth through the Y-axis guide rail 32 until the alignment mark 43 on the pad head 41 is aligned with the alignment mark 43 on the MEMS substrate 5, and then start the Z-axis guide rail 33 to move the pad head 41 downward, so that the sensitive material can be transferred to the MEMS substrate 5, so as to achieve high-precision printing of thinner sensitive materials and good adaptation between the pad head and the sample.
[0088] Example 2
[0089] The present application embodiment discloses a method for preparing an ultra-sensitive MEMS VOCs gas sensor, comprising the following specific steps:
[0090] S1. Preparation of gas-sensitive material powder
[0091] Tin tetrachloride, zinc nitrate, copper nitrate and deionized water are stirred at a speed of 600 rpm in a ratio of 20:3:7:70 until they are completely dissolved; then the above solution and ethanol are mixed in a mass ratio of 50:20 to form a mixed solution, polyethylene glycol is added in an amount of 1% relative to the total mass of the above mixed solution, and then stirred at a speed of 600 rpm for 30 minutes; then the obtained dispersion is transferred to a reactor and allowed to stand at 80°C for 12 hours; finally, the mixture is centrifuged and washed with ethanol, and dried in an oven at 80°C to obtain a gas-sensitive material powder.
[0092] S2. Preparation of gas-sensitive material slurry
[0093] The gas-sensitive material powder prepared above: silica sol: polyamide resin: diisobutyl ketone are uniformly mixed in a mass ratio of 5:1:10:85 to form a suspension; the suspension is sand-milled to control the particle size D90 to be less than 100 nm to obtain a gas-sensitive material slurry.
[0094] S3, pad printing interdigitated electrodes
[0095] The prepared gas-sensitive material slurry was transferred to the interdigital electrodes of the MEMS microheater substrate using a micro pad printing device, and the interdigital electrodes were completely covered; after pad printing, the slurry was placed in an oven and baked at 80°C for 30 minutes; the thickness of the gas-sensitive film after baking was 2μm.
[0096] S4. Device annealing
[0097] The MEMS substrate printed with the sensitive material slurry is placed in a muffle furnace and annealed at 400°C for 2 hours. After the annealing is completed, the substrate is cut to obtain a MEMS sensor chip.
[0098] S5, gold wire ball welding, ceramic packaging
[0099] The prepared MEMS sensor chip is subjected to gold wire ball welding and ceramic packaging to finally obtain a MEMS VOCs gas sensor.
[0100] Example 3
[0101] The present application embodiment discloses a method for preparing an ultra-sensitive MEMS VOCs gas sensor, comprising the following specific steps:
[0102] S1. Preparation of gas-sensitive material powder
[0103] Tin tetrachloride, zinc nitrate, chromium nitrate and deionized water are stirred at a speed of 600 rpm in a ratio of 20:4:6:70 until they are completely dissolved; then the above solution and ethanol are mixed in a mass ratio of 50:20 to form a mixed solution, 1% polyvinyl alcohol relative to the total mass of the above mixed solution is added, and then stirred at a speed of 600 rpm for 30 minutes; then the obtained dispersion is transferred to a reactor and allowed to stand at 80°C for 12 hours; finally, the mixture is centrifuged and washed with ethanol, placed in an oven at 80°C for drying, and finally a gas-sensitive material powder is obtained.
[0104] S2. Preparation of gas-sensitive material slurry
[0105] The gas-sensitive material powder prepared above: silica sol: polyamide resin: triethoxyethyl propionate are uniformly mixed in a mass ratio of 5:1:20:75 to form a suspension; the suspension is sand-milled to control the particle size D90 to be less than 300 nm to obtain a gas-sensitive material slurry.
[0106] S3, pad printing interdigitated electrodes
[0107] The prepared gas-sensitive material slurry was transferred to the interdigital electrodes of the MEMS microheater substrate using a micro pad printing device, and the interdigital electrodes were completely covered; after pad printing, the slurry was placed in an oven and baked at 80°C for 30 minutes; the thickness of the gas-sensitive film after baking was 3μm.
[0108] S4. Device annealing
[0109] The MEMS substrate printed with the sensitive material slurry is placed in a muffle furnace and annealed at 400°C for 2 hours. After the annealing is completed, the substrate is cut to obtain a MEMS sensor chip.
[0110] S5, gold wire ball welding, ceramic packaging
[0111] The prepared MEMS sensor chip is subjected to gold wire ball welding and ceramic packaging to finally obtain a MEMS VOCs gas sensor.
[0112] Example 4
[0113] The present application embodiment discloses a method for preparing an ultra-sensitive MEMS VOCs gas sensor, comprising the following specific steps:
[0114] S1. Preparation of gas-sensitive material powder
[0115] Tin tetrachloride, zinc nitrate, cobalt nitrate and deionized water are stirred at a speed of 600 rpm in a ratio of 20:7:3:70 until they are completely dissolved; then the above solution and ethanol are mixed in a mass ratio of 50:20 to form a mixed solution, 1% polyethylene oxide relative to the total mass of the above mixed solution is added, and then stirred at a speed of 600 rpm for 30 minutes; then the obtained dispersion is transferred to a reactor and allowed to stand at 80°C for 12 hours; finally, the mixture is centrifuged and washed with ethanol, placed in an oven at 80°C for drying, and finally a gas-sensitive material powder is obtained.
[0116] S2. Preparation of gas-sensitive material slurry
[0117] The gas-sensitive material powder prepared above: silica sol: polyamide resin: diisobutyl ketone, propylene carbonate are uniformly mixed in a mass ratio of 5:1:25:70 to form a suspension; the suspension is sand-milled to control the particle size D90 to be less than 400nm to obtain a gas-sensitive material slurry.
[0118] S3, pad printing interdigitated electrodes
[0119] The prepared gas-sensitive material slurry was transferred to the interdigital electrodes of the MEMS microheater substrate using a micro-pad printing device, and the interdigital electrodes were completely covered; after pad printing, it was placed in an oven and baked at 80°C for 30 minutes. The thickness of the baked gas-sensitive film was 4μm.
[0120] S4. Device annealing
[0121] The MEMS substrate printed with the sensitive material slurry is placed in a muffle furnace and annealed at 400°C for 2 hours. After the annealing is completed, the substrate is cut to obtain a MEMS sensor chip.
[0122] S5, gold wire ball welding, ceramic packaging
[0123] The prepared MEMS sensor chip is subjected to gold wire ball welding and ceramic packaging to finally obtain a MEMS VOCs gas sensor.
[0124] Example 5
[0125] The present application embodiment discloses a method for preparing an ultra-sensitive MEMS VOCs gas sensor, comprising the following specific steps:
[0126] S1. Preparation of gas-sensitive material powder
[0127] Tin tetrachloride, nickel nitrate, copper nitrate and deionized water are stirred at a speed of 600 rpm in a ratio of 20:5:5:70 until they are completely dissolved; then the above solution and ethanol are mixed in a mass ratio of 50:20 to form a mixed solution, 1% carboxymethyl cellulose relative to the total mass of the above mixed solution is added, and then stirred at a speed of 600 rpm for 30 minutes; then the obtained dispersion is transferred to a reactor and allowed to stand at 80°C for 12 hours; finally, the mixture is centrifuged and washed with ethanol, placed in an oven at 80°C for drying, and finally a gas-sensitive material powder is obtained.
[0128] S1. Preparation of gas-sensitive material powder
[0129] The gas-sensitive material powder prepared above: silica sol: polyamide resin: diisobutyl ketone, propylene carbonate are uniformly mixed in a mass ratio of 5:1:20:75 to form a suspension; the suspension is sand-milled to control the particle size D90 to be less than 500nm to obtain a gas-sensitive material slurry.
[0130] S3, pad printing interdigitated electrodes
[0131] The prepared gas-sensitive material slurry was transferred to the interdigital electrodes of the MEMS microheater substrate using a micro pad printing device, and the interdigital electrodes were completely covered; after pad printing, the film was placed in an oven and baked at 80°C for 30 minutes, and the thickness of the baked gas-sensitive film was 5 μm.
[0132] S4. Device annealing
[0133] The MEMS substrate printed with the sensitive material slurry is placed in a muffle furnace and annealed at 400°C for 2 hours. After the annealing is completed, the substrate is cut to obtain a MEMS sensor chip.
[0134] S5, gold wire ball welding, ceramic packaging
[0135] The prepared MEMS sensor chip is subjected to gold wire ball welding and ceramic packaging to finally obtain a MEMS VOCs gas sensor.
[0136] Comparative Example 1
[0137] The comparative example of the present application provides a method for preparing a MEMS VOCs gas sensor, which differs from Example 2 in that a brush coating method is used to coat the sensitive material in step S3, and includes the following specific steps:
[0138] S1. Preparation of gas-sensitive material powder
[0139] Tin tetrachloride, zinc nitrate, copper nitrate and deionized water are stirred at a speed of 600 rpm in a ratio of 20:3:7:70 until they are completely dissolved; then the above solution and ethanol are mixed in a mass ratio of 50:20 to form a mixed solution, polyethylene glycol is added in an amount of 1% relative to the total mass of the above mixed solution, and then stirred at a speed of 600 rpm for 30 minutes; then the obtained dispersion is transferred to a reactor and allowed to stand at 80°C for 12 hours; finally, the mixture is centrifuged and washed with ethanol, and dried in an oven at 80°C to obtain a gas-sensitive material powder.
[0140] S2. Preparation of gas-sensitive material slurry
[0141] The gas-sensitive material powder prepared above: silica sol: polyamide resin: diisobutyl ketone are uniformly mixed in a mass ratio of 5:1:10:85 to form a suspension; the suspension is sand-milled to control the particle size D90 to be less than 100 nm to obtain a gas-sensitive material slurry.
[0142] S3, brush-coated interdigital electrodes
[0143] The gas-sensitive material slurry is brushed onto the interdigital electrodes of the MEMS microheater substrate and completely covers the interdigital electrodes; after brushing, it is placed in an oven and baked at 80°C for 30 minutes; the thickness of the gas-sensitive film after baking is 2μm.
[0144] S4. Device annealing
[0145] The MEMS substrate coated with the sensitive material slurry is placed in a muffle furnace and annealed at 400°C for 2 hours. After the annealing is completed, the substrate is cut to obtain a MEMS sensor chip.
[0146] S5, gold wire ball welding, ceramic packaging
[0147] The prepared MEMS sensor chip is subjected to gold wire ball welding and ceramic packaging to finally obtain a MEMS VOCs gas sensor.
[0148] Device gas sensing performance test 1
[0149] The encapsulated MEMS VOCs gas sensors of Examples 1-5 and Comparative Example 1 were tested for device gas sensing performance. The device gas sensing performance was tested using a source-meter multi-channel gas sensing test platform (SMP-4) developed by the Institute of Solid State Physics, Hefei Institutes of Physical Science, Chinese Academy of Sciences. The multimeter / DC power supply (Agilent U3606A and U8002A) provided a voltage source and collected voltage signals.
[0150] Gases or steam of different concentrations are injected into the test chamber from the injection port. Two 300rpm rotating fans are symmetrically distributed near the gas injection port. The uniform mixing of the gas in the chamber can be completed within 0.1 seconds. The gas injection will cause the resistance of the device to change, which is reflected as a voltage change in the circuit.
[0151] LabVIEW software was used to control and collect signals, with an acquisition rate of 20 times / second. The tests were all carried out under the environmental conditions of 60% RH and 25°C room temperature. The test results are shown in Table 1.
[0152] Table 1 Gas Sensing Performance Test Results of Sensors in Examples 1-5
[0153]
[0154] According to the results in Table 1, the sensors of Examples 1-5 are more sensitive to ethanol than Comparative Example 1, while the response times to 20 ppm and 1 ppm ethanol are shorter than Comparative Example 1, indicating that the gas-sensitive material slurry is printed on the interdigital electrodes by pad printing, and the sensitivity and response speed of the prepared sensors to VOCs gas are better than those by brushing.
[0155] The MEMS VOCs gas sensor prepared in Example 2 has the highest sensitivity to 20ppm ethanol, followed by Example 1, Example 3, Example 4, and Example 5. According to the analysis of various parameters in the sensor preparation steps, the sensitivity is negatively correlated with the particle size of the gas-sensitive material slurry, that is, the smaller the particle size of the gas-sensitive material slurry, the higher the sensitivity to VOCs gas.
[0156] The sensor prepared in Example 2 has the shortest response time to 20ppm ethanol, which is 2.24s, indicating that the smaller the particle size of the gas-sensitive material slurry, the stronger the response intensity and recovery to VOCs gas. The sensor has the shortest response time to 1ppm ethanol, which is 8.13s, followed by Example 1, Example 3, Example 4, and Example 5, indicating that the smaller the particle size of the gas-sensitive material slurry, the stronger the response intensity and recovery to low-concentration VOCs gas.
[0157] In addition, the response recovery curve of the MEMS VOCs gas sensor prepared in Example 2 to 20 ppm ethanol is as follows: Figure 2 The response recovery curve to 1 ppm ethanol is shown in Figure 3The response capability of the commercial MEMS VOCs gas sensor GM-502B in the prior art to 1ppm and 20ppm ethanol is shown in Table 1. By comparison, it can be seen that the response time of the sensor prepared in Example 2 to 20ppm and 1ppm ethanol is shorter than that of the existing commercial sensors, indicating that the sensor prepared in this application has the advantage of fast response and also has a faster reaction speed to low-concentration VOCs gas.
[0158] Device gas sensing performance test 2
[0159] The MEMS VOCs gas sensor prepared in Example 2 was used to monitor ethanol, acetone, toluene, methane, hydrogen, carbon monoxide, and nitrogen dioxide, and the sensitivity characteristic curve was plotted. The results are as follows: Figure 4 As shown (the horizontal and vertical axes in the figure are logarithmic values, and the greater the degree to which the curve deviates from 1, the stronger the response). Figure 4 It can be seen that the sensor has a strong response to ethanol, toluene, and acetone, and has the advantages of high sensitivity to VOCs and wide application scenarios. In particular, the response to low concentrations of ethanol, toluene, and acetone is also very strong, indicating that the sensor has a high sensitivity to low concentrations of VOCs, that is, it has super sensitivity.
[0160] Principle and advantages of use: The present invention first prepares gas-sensitive material powder and gas-sensitive material slurry; then transfers the gas-sensitive material slurry to the interdigital electrodes of the MEMS microheater substrate through a pad printing process; finally, through annealing, gold wire ball welding, and ceramic packaging, a MEMS VOCs gas sensor is finally obtained. The MEMS VOCs gas sensor prepared based on the above steps has a thinner sensitive material and is firmly combined with the interdigital electrodes. It has ultra-sensitive gas-sensitive characteristics and has the potential for large-scale batch production. It is a method for ultra-sensitive MEMS VOCs gas sensors with strong applicability.
[0161] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing an ultra-sensitive MEMS VOCs gas sensor, characterized in that: The specific steps include: S1. Preparation of gas-sensitive material powder Mix and stir tin tetrachloride, nitrate and deionized water until they are completely dissolved, then uniformly mix the mixed solution with an organic solvent to form a mixed solution, add 0.5-2% of a dispersant relative to the total mass of the mixed solution and stir evenly; then transfer the obtained dispersion to a reactor and let it stand at 60-100°C for 6-18h; finally, wash the mixture by centrifugation with ethanol, and dry it in an oven to obtain a gas-sensitive material powder; S2. Preparation of gas-sensitive material slurry The gas-sensitive material powder, silica sol, polyamide resin and organic solvent prepared above are uniformly mixed to form a suspension; the suspension is then sand-milled to obtain a gas-sensitive material slurry; S3, pad printing interdigitated electrodes The prepared gas-sensitive material slurry is transferred to the interdigital electrodes of the MEMS micro-heater substrate by using a micro-pad printing device, and the interdigital electrodes are completely covered; after the pad printing is completed, it is placed in an oven for baking, so as to form a gas-sensitive film on the MEMS micro-heater substrate; S4. Device annealing The MEMS substrate printed with the sensitive material slurry is placed in a muffle furnace for annealing, and then cut to obtain a MEMS sensor chip; S5, gold wire ball welding, ceramic packaging The prepared MEMS sensor chip is subjected to gold wire ball welding and ceramic packaging to finally produce a MEMS VOCs gas sensor.
2. The method for preparing an ultra-sensitive MEMS VOCs gas sensor according to claim 1, characterized in that: In the step S1, the mass ratio of tin tetrachloride, nitrate and deionized water is 20:8-12:70; the mass ratio of the three components to the organic solvent after mixing is 20:50-50:
30.
3. The method for preparing an ultra-sensitive MEMS VOCs gas sensor according to claim 1, characterized in that: In step S1, the nitrate is one or more combinations of zinc nitrate, nickel nitrate, copper nitrate, chromium nitrate and cobalt nitrate.
4. The method for preparing an ultra-sensitive MEMS VOCs gas sensor according to claim 1, characterized in that: In step S1, the organic solvent is one or more combinations of ethanol and acetone; the dispersant is one or more combinations of polyethylene glycol, polyvinyl alcohol, polyethylene oxide, and carboxymethyl cellulose.
5. The method for preparing an ultra-sensitive MEMS VOCs gas sensor according to claim 1, characterized in that: The organic solvent in step S2 is one or more combinations of diisobutyl ketone, ethyl triethoxypropionate, and propylene carbonate.
6. The method for preparing an ultra-sensitive MEMS VOCs gas sensor according to claim 1, characterized in that: In the step S2, the mass ratio of the gas-sensitive material powder, silica sol, polyamide resin and organic solvent is 5:1:15:80; and the particle size D90 of the suspension after sand grinding in the step S2 is not greater than 500 nm.
7. The method for preparing an ultra-sensitive MEMS VOCs gas sensor according to claim 1, characterized in that: The micro pad printing device in step S3 includes a base, a gravure plate, a moving component and a transfer component. The gravure plate is engraved with a pattern to be printed and coated with a sensitive material. The gravure plate and the MEMS substrate are both placed on the base; the moving component drives the transfer component to move from the gravure plate position to the MEMS substrate. The transfer component includes a planar pad printing head and an alignment camera fixedly mounted on the moving component. The sensitive material on the gravure plate is transferred to the MEMS substrate through the pad printing head. The alignment camera aligns the pad printing head with the corresponding positions of the gravure plate and the MEMS substrate.
8. The method for preparing an ultra-sensitive MEMS VOCs gas sensor according to claim 1, characterized in that: In the step S3, the baking temperature is 60-80° C. and the time is 30-40 min. The thickness of the gas-sensitive film after baking is 1-5 μm.
9. The method for preparing an ultra-sensitive MEMS VOCs gas sensor according to claim 1, characterized in that: The annealing temperature in step S4 is 350-450° C. and the time is 2-3 hours.
10. A micro pad printing device for preparing the ultra-sensitive MEMS VOCs gas sensor according to any one of claims 1 to 9, characterized in that: It includes a base, a gravure plate, a moving component and a transfer component. The gravure plate is engraved with a pattern to be printed and coated with a sensitive material. The gravure plate and the MEMS substrate are both placed on the base. The moving component drives the transfer component to move from the gravure plate position to the MEMS substrate. The transfer component includes a planar pad printing head and an alignment camera fixedly mounted on the moving component. The sensitive material on the gravure plate is transferred to the MEMS substrate through the pad printing head. The alignment camera aligns the pad printing head with the corresponding positions of the gravure plate and the MEMS substrate.