A method for evaluating cross-linked inner shielding material
Through the combined method of thermal extension test and temperature rise test, the problem of early cross-linking of cross-linked inner shielding materials is solved, the quality and performance of cross-linked cables are ensured, and a reliable method for evaluating cross-linked inner shielding materials is provided.
Patent Information
- Application Number
- CN202210484444.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-06
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-05-06
AI Technical Summary
In the production of cross-linked cables, cross-linked inner shielding materials are prone to pre-cross-linking, which leads to deterioration of surface roundness and smoothness and affects cable quality. It is difficult to accurately judge this phenomenon according to existing standards.
Using a combined method of thermal elongation testing and temperature rise testing, sample pieces are prepared through plasticization and vulcanization, and their thermal elongation properties and extruder temperature rise are measured to determine whether the cross-linked inner shielding material is qualified.
Accurately determine whether cross-linked inner shielding materials are prone to early cross-linking, select materials that are less prone to cross-linking, and improve the quality and performance of cross-linked cable products.
Smart Images

Figure BDA0003628690580000091 
Figure BDA0003628690580000092 
Figure BDA0003628690580000101
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cross-linked cables, and in particular to an evaluation method for a cross-linked inner shielding material. Background Art
[0002] In the production of cross-linked cables with rated voltages of 3.6 / 6 to 26 / 35kV, cross-linked inner shielding materials must be used, and the inner shielding materials must be tightly extruded onto the surface of the conductor, in a concentric circle with the circular conductor, and tightly bonded to the insulation layer. Therefore, the higher the surface roundness and smoothness of the inner shielding materials, the more conducive it is to obtain cross-linked cables of excellent quality. During the preparation process, the temperature of the cross-linked inner shielding material will increase with the increase of the temperature in the extruder. When the process temperature of the cross-linked inner shielding material is exceeded, the cross-linked inner shielding material will undergo a cross-linking reaction in the extruder. To ensure product quality, the cross-linked inner shielding material cannot undergo a cross-linking reaction in the extruder during normal production.
[0003] However, it is found in actual production that, under the condition of stable process conditions, the extrusion effect of inner shielding materials produced by different manufacturers that meet the current standard ("JB / T10738-2007 Semi-conductive shielding materials for extruded insulated cables with rated voltages of 35kV and below") or cross-linked inner shielding materials produced by the same manufacturer in different batches will be different, and sometimes even premature cross-linking will occur, which will deteriorate the surface roundness and smoothness of the inner shielding material, thereby affecting the quality of the cable product. In severe cases, the inner shielding material will be embedded in the insulation layer, causing the product to be scrapped. Therefore, a method is urgently needed to evaluate whether the cross-linked inner shielding material will undergo premature cross-linking. Summary of the invention
[0004] The purpose of the present invention is to provide an evaluation method for a cross-linked inner shielding material. The evaluation method provided by the present invention can accurately determine whether the cross-linked inner shielding material will undergo premature cross-linking.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides an evaluation method for a cross-linked inner shielding material, comprising respectively performing a heat extension test and a temperature rise test on the cross-linked inner shielding material to be evaluated; if both the heat extension test and the temperature rise test of the cross-linked inner shielding material to be evaluated are qualified, the cross-linked inner shielding material to be evaluated is determined to be a qualified product;
[0007] The thermal extension test comprises the following steps:
[0008] (1) plasticizing the cross-linked inner shielding material to be evaluated to obtain a film;
[0009] (2) vulcanizing the film obtained in step (1) to obtain a sample to be tested;
[0010] (3) testing the thermal extension performance of the sample to be tested obtained in step (2); if the thermal extension change trend of the sample to be tested meets the following requirements: the elongation after vulcanization for 3 minutes is ≥300%, the elongation after vulcanization for 5 minutes is 150-200%, the elongation after vulcanization for 10 minutes is 100-120%, and the elongation after vulcanization for 15 minutes is 50-80%, then the thermal extension test of the cross-linked inner shielding material to be evaluated is determined to be qualified; if the thermal extension change trend of the sample to be tested does not meet the above requirements, then the thermal extension test of the cross-linked inner shielding material to be evaluated is determined to be unqualified;
[0011] The temperature rise test includes: extruding the cross-linked internal shielding material to be evaluated in three stages, and then testing the temperature rise of the extruder body; if the temperature rise meets the following conditions: feeding stage <3°C, melting stage <4°C, homogenization stage <5°C, the temperature rise test of the cross-linked internal shielding material to be evaluated is qualified; otherwise, the temperature rise test of the cross-linked internal shielding material to be evaluated is judged to be unqualified.
[0012] Preferably, the plasticizing temperature in step (1) is less than 70°C.
[0013] Preferably, the equipment used for plasticization in step (1) is a double-drum plastic refiner; the roller spacing of the double-drum plastic refiner is 2.0 to 2.5 mm.
[0014] Preferably, the plasticizing process in step (1) further includes making triangle bags; the time for making triangle bags is 3 to 4 minutes.
[0015] Preferably, the vulcanization temperature in step (2) is 180-183°C.
[0016] Preferably, the test samples obtained in step (2) include samples with vulcanization times of 3 min, 4 min, 5 min, 10 min and 15 min.
[0017] Preferably, the pressurization method before vulcanization in step (2) is: first pressurize to 13-15 MPa for 20-25 seconds, then reduce the pressure to 0 MPa and maintain for 10-15 seconds, and finally pressurize to 15-20 MPa.
[0018] Preferably, the size of the sample to be tested in step (2) is 200 mm×200 mm, and the thickness is 1.0±0.1 mm.
[0019] Preferably, the initial temperature of the feeding section body is 95-98°C, the initial temperature of the melting section body is 100-103°C, and the initial temperature of the homogenizing section body is 105-108°C.
[0020] Preferably, the time for testing the temperature rise of the extruder body is 5 to 6 minutes after the three-stage extrusion.
[0021] The present invention provides an evaluation method for a cross-linked inner shielding material, comprising: performing a heat extension test and a temperature rise test on the cross-linked inner shielding material to be evaluated; if both the heat extension test and the temperature rise test of the cross-linked inner shielding material to be evaluated are qualified, the cross-linked inner shielding material to be evaluated is judged to be a qualified product; the heat extension test comprises the following steps: (1) plasticizing the cross-linked inner shielding material to be evaluated to obtain a film; (2) vulcanizing the film obtained in step (1) to obtain a sample to be tested; (3) testing the heat extension performance of the sample to be tested obtained in step (2); if the heat extension change trend of the sample to be tested satisfies: the elongation after vulcanization for 3 minutes is ≥300%, the elongation after vulcanization for 5 minutes is ≥300%, and the elongation after vulcanization for 5 minutes is ≥300%. If the elongation rate is 150-200%, the elongation rate after vulcanization for 10 minutes is 100-120%, and the elongation rate after vulcanization for 15 minutes is 50-80%, then the cross-linked inner shielding material to be evaluated is judged to be qualified in the heat extension test; if the heat extension change trend of the sample to be tested does not meet the above requirements, then the cross-linked inner shielding material to be evaluated is judged to be unqualified in the heat extension test; the temperature rise test includes: extruding the cross-linked inner shielding material to be evaluated in three stages, and then testing the temperature rise of the extruder body; if the temperature rise meets: the feeding stage <3°C, the melting stage <4°C, and the homogenization stage <5°C, then the temperature rise test of the cross-linked inner shielding material to be evaluated is qualified; otherwise, the temperature rise test of the cross-linked inner shielding material to be evaluated is judged to be unqualified. The method provided by the present invention can select the cross-linked inner shielding material that is not prone to premature cross-linking from a large number of inner shielding materials by measuring the heat extension performance of the test sample made of the cross-linked inner shielding material and the temperature rise of the extruder body when the cross-linked inner shielding material is extruded, thereby providing necessary technical support for selecting the cross-linked inner shielding material with the best performance for the preparation of cross-linked cables and improving the quality of cross-linked cable products. DETAILED DESCRIPTION
[0022] The present invention provides an evaluation method for a cross-linked inner shielding material, comprising respectively performing a heat extension test and a temperature rise test on the cross-linked inner shielding material to be evaluated; if both the heat extension test and the temperature rise test of the cross-linked inner shielding material to be evaluated are qualified, the cross-linked inner shielding material to be evaluated is determined to be a qualified product;
[0023] The thermal extension test comprises the following steps:
[0024] (1) plasticizing the cross-linked inner shielding material to be evaluated to obtain a film;
[0025] (2) vulcanizing the film obtained in step (1) to obtain a sample to be tested;
[0026] (3) testing the thermal extension performance of the sample to be tested obtained in step (2); if the thermal extension change trend of the sample to be tested meets the following requirements: the elongation after vulcanization for 3 minutes is ≥300%, the elongation after vulcanization for 5 minutes is 150-200%, the elongation after vulcanization for 10 minutes is 100-120%, and the elongation after vulcanization for 15 minutes is 50-80%, then the thermal extension test of the cross-linked inner shielding material to be evaluated is determined to be qualified; if the thermal extension change trend of the sample to be tested does not meet the above requirements, then the thermal extension test of the cross-linked inner shielding material to be evaluated is determined to be unqualified;
[0027] The temperature rise test includes: extruding the cross-linked internal shielding material to be evaluated in three stages, and then testing the temperature rise of the extruder body; if the temperature rise meets the following conditions: feeding stage <3°C, melting stage <4°C, homogenization stage <5°C, the temperature rise test of the cross-linked internal shielding material to be evaluated is qualified; otherwise, the temperature rise test of the cross-linked internal shielding material to be evaluated is judged to be unqualified.
[0028] The present invention performs a heat extension test and a temperature rise test on the cross-linked inner shielding material to be evaluated; if the heat extension test and the temperature rise test of the cross-linked inner shielding material to be evaluated are both qualified, the cross-linked inner shielding material to be evaluated is determined to be a qualified product. The present invention can select a cross-linked inner shielding material that is not prone to premature cross-linking from a large number of inner shielding materials by respectively measuring the heat extension performance of the cross-linked inner shielding material and the temperature rise of the extruder body when the cross-linked inner shielding material is extruded.
[0029] The evaluation method provided by the present invention is applicable to various cross-linked inner shielding materials produced by various manufacturers. In the present invention, the cross-linked inner shielding materials to be evaluated preferably include: 10kV cross-linked inner shielding materials produced by Shanghai Wanyi, batch number 20509, box number 20, 10kV cross-linked inner shielding materials produced by Jiangsu Jiangyin, batch number 202003D14, box number 22, 10kV cross-linked inner shielding materials produced by Zhejiang Xinfangde, batch number 210109, box number 18 and 10kV cross-linked inner shielding materials produced by Nanjing Zhongchao, batch number 210109, box number 09.
[0030] In the present invention, the thermal extension test comprises the following steps:
[0031] (1) plasticizing the cross-linked inner shielding material to be evaluated to obtain a film;
[0032] (2) vulcanizing the film obtained in step (1) to obtain a sample to be tested;
[0033] (3) Testing the thermal extension performance of the sample to be tested obtained in step (2); if the thermal extension change trend of the sample to be tested meets the following requirements: the elongation after vulcanization for 3 minutes is ≥300%, the elongation after vulcanization for 5 minutes is 150-200%, the elongation after vulcanization for 10 minutes is 100-120%, and the elongation after vulcanization for 15 minutes is 50-80%, then the thermal extension test of the cross-linked inner shielding material to be evaluated is determined to be qualified; if the thermal extension change trend of the sample to be tested does not meet the above requirements, then the thermal extension test of the cross-linked inner shielding material to be evaluated is determined to be unqualified.
[0034] The invention plasticizes the cross-linked inner shielding material to be evaluated to obtain a film. The invention plasticizes the cross-linked inner shielding material to be evaluated to change from smaller particles to larger thick sheets and to prepare a film with a certain shape.
[0035] In the present invention, the plasticizing equipment is preferably a double-roller plasticizer; the roller distance of the double-roller plasticizer is preferably 2.0-2.5 mm. The present invention has no special limitation on the source of the double-roller plasticizer, and commercial products known to those skilled in the art can be used.
[0036] In the present invention, the plasticizing temperature is preferably less than 70° C. In the present invention, the plasticizing temperature is preferably controlled within the above range, which is beneficial to ensure the viscosity of the product after plasticizing.
[0037] In the present invention, the operation of controlling the plasticizing temperature is preferably as follows: during the plasticizing process, the rubber material is tested with a temperature measuring gun; when the temperature approaches 70°C, the rubber material is pulled off the roller, and when the temperature of the rubber material drops to 50-60°C, the rubber material is placed on a plasticizer for plasticizing.
[0038] In the present invention, the plasticizing process preferably further includes making triangle packs; the time for making triangle packs is preferably 3 to 4 minutes; and the number of times of making triangle packs is preferably 6 to 8 times.
[0039] After the plasticization is completed, the present invention preferably air cools the plasticized product to room temperature to obtain a film. In the present invention, the thickness of the film is preferably 2 to 3 mm.
[0040] After obtaining the film, the present invention vulcanizes the film to obtain a sample to be tested. The present invention cross-links the cross-linked inner shielding material through vulcanization to obtain the sample to be tested.
[0041] In the present invention, the upper and lower surfaces of the film are preferably covered with polyester films respectively before vulcanization.
[0042] In the present invention, the melting point of the polyester film is preferably ≥ 200° C. In the present invention, the polyester film is preferably covered on the upper and lower surfaces of the film respectively, which is conducive to preparing a better sample.
[0043] In the present invention, the vulcanization temperature is preferably 180-183°C, more preferably 180°C. In the present invention, the vulcanization temperature is preferably controlled within the above range, which is conducive to ensuring sufficient cross-linking of the cross-linked inner shielding material. In the present invention, the vulcanization pressure is preferably 15-20MPa, more preferably 15MPa.
[0044] In the present invention, the pressurization method before vulcanization is preferably: first pressurize to 13-15MPa for pre-pressing for 20-25s, then reduce the pressure to 0MPa and maintain for 10-15s, and finally pressurize to 15-20MPa; more preferably: first pressurize to 13MPa for pre-pressing for 20s, then reduce the pressure to 0MPa and maintain for 10s, and finally pressurize to 15MPa.
[0045] In the present invention, the vulcanization time is preferably 3min, 4min, 5min, 10min and 15min. The present invention preferably prepares samples with vulcanization time of 3min, 4min, 5min, 10min and 15min, respectively, so as to smoothly carry out the subsequent cross-linked inner shielding material thermal extension test.
[0046] In the present invention, the size of the sample to be tested is preferably 200 mm×200 mm; the thickness is preferably 1.0±0.1 mm.
[0047] After obtaining the sample to be tested, the present invention tests the thermal extension performance of the sample to be tested described in the above technical solution. The present invention determines whether the cross-linked inner shielding material to be evaluated is a qualified product by testing the thermal extension performance of the sample to be tested.
[0048] In the present invention, if the thermal extension change trend of the sample to be tested meets the following requirements: the elongation after vulcanization for 3 minutes is ≥300%, the elongation after vulcanization for 5 minutes is 150-200%, the elongation after vulcanization for 10 minutes is 100-120%, and the elongation after vulcanization for 15 minutes is 50-80%, then the thermal extension test of the cross-linked inner shielding material to be evaluated is determined to be qualified; if the thermal extension change trend of the sample to be tested does not meet the above requirements, then the thermal extension test of the cross-linked inner shielding material to be evaluated is determined to be unqualified.
[0049] In the present invention, the method for the thermal extension test preferably adopts GB / T2951.21-2008 "General test methods for insulation and sheath materials of electrical and optical cables Part 21: Special test methods for elastomer mixtures - Ozone resistance test - Thermal extension test - Mineral oil immersion test".
[0050] In the present invention, the temperature rise test includes: extruding the cross-linked internal shielding material to be evaluated in three stages, and then testing the temperature rise of the extruder body; if the temperature rise meets the following conditions: feeding stage <3°C, melting stage <4°C, homogenization stage <5°C, then the temperature rise test of the cross-linked internal shielding material to be evaluated is qualified; otherwise, the temperature rise test of the cross-linked internal shielding material to be evaluated is judged to be unqualified.
[0051] In the present invention, the initial temperature of the feeding section body is preferably 95-98°C, more preferably 95-96°C; the initial temperature of the melting section body is preferably 100-103°C, more preferably 100-102°C; the initial temperature of the homogenizing section body is preferably 105-108°C, more preferably 105-106°C.
[0052] In the present invention, the time for testing the temperature rise of the extruder body is preferably 5 to 6 minutes after the three-stage extrusion.
[0053] In the present invention, the die temperature of the extruder is preferably 108-111° C.; the rotation speed of the extruder is preferably 40-50 r / min; and the flow rate of the cooling compressed air in each section of the extruder body is preferably 10-11 L / min.
[0054] The method provided by the present invention can select a cross-linked inner shielding material that is not prone to premature cross-linking from a variety of inner shielding materials by measuring the thermal extension properties of a test sample made of a cross-linked inner shielding material and the temperature rise of an extruder body when the cross-linked inner shielding material is extruded, thereby providing necessary technical support for selecting the cross-linked inner shielding material with the best performance for the preparation of cross-linked cables and improving the quality of cross-linked cable products.
[0055] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0056] Example 1
[0057] The 10kV cross-linked inner shielding material with batch number 20509 and box number 20 produced by Shanghai Wanyi was evaluated and recorded as 1#;
[0058] Thermal extension test:
[0059] (1) Take 400 g of the cross-linked inner shielding material No. 1 to be evaluated, place it on a double-drum plasticizer with a temperature not exceeding 70°C and a roller distance of 2.0 mm for plasticization, and monitor the temperature of the rubber material with a temperature measuring gun. When the temperature of the rubber material is close to 70°C, pull all the rubber material from the roller, and when the temperature drops to 60°C, put the rubber material on the plasticizer again; during plasticization, make eight triangular packages, the time is controlled within 3 minutes, and after plasticization is completed, air cool to room temperature to obtain a film with a thickness of 2 mm;
[0060] (2) placing the film obtained in step (1) in a mold, and covering the upper and lower surfaces thereof with polyester films having a melting point ≥ 200°C, respectively; then placing the mold in a flat-plate vulcanizer at a temperature of 180°C, first pressurizing to 13 MPa for pre-pressing for 20 seconds, then reducing the pressure to 0 MPa and maintaining for 10 seconds, and finally pressurizing to 15 MPa, and vulcanizing at this pressure; when the temperature of the flat-plate vulcanizer returns to 180°C, start timing, stop heating after 3 minutes, but keep the pressure constant, pass cooling water to cool, cool to room temperature, remove the mold, remove the sample from the mold, and obtain a sample to be tested with a size of 200 mm × 200 mm and a thickness of 1.0 ± 0.1 mm;
[0061] (3) Repeat steps (1) and (2) to prepare test pieces with curing times of 4 min, 5 min, 10 min, and 15 min, respectively;
[0062] (4) According to the thermal extension test method in GB / T2951.21-2008 "General test methods for insulation and sheath materials of electric and optical cables Part 21: Special test methods for elastomer mixtures - Ozone resistance test - Thermal extension test - Mineral oil immersion test", the test samples prepared in steps (2) and (3) were tested respectively. The test results are shown in Table 1. It can be seen that the elongation of the 1# inner shielding cross-linked material after vulcanization for 3 minutes is 325%, the elongation after vulcanization for 5 minutes is 175%, the elongation after vulcanization for 10 minutes is 117%, and the elongation after vulcanization for 15 minutes is 78%, which meets the thermal extension change trend. It is determined that the thermal extension test of the 1# cross-linked inner shielding material to be evaluated is qualified;
[0063] Temperature rise test:
[0064] The 1# cross-linked inner shielding material to be evaluated was extruded in three stages, and the temperature of the extruder body was set as follows: the initial temperature of the feeding section was 95°C, the initial temperature of the melting section was 100°C, the initial temperature of the homogenizing section was 105°C, and the die temperature was 108°C; at a speed of 40r / min, the cooling compressed air flow rate in each section of the body was maintained at 10L / min, and the test extrusion was performed for 5 minutes. At the same time, the temperature rise of the extruder body was tested. The test results are shown in Table 2; it can be seen that the temperature rise of the feeding section is 0°C, the temperature rise of the melting section is 1°C, and the temperature rise of the homogenizing section is 1°C, which meets the temperature rise requirements, and the temperature rise test of the 1# cross-linked inner shielding material to be evaluated is qualified;
[0065] The thermal extension test and temperature rise test of the 1# cross-linked inner shielding material to be evaluated are both qualified, and the 1# cross-linked inner shielding material is determined to be a qualified product.
[0066] Example 2
[0067] The 10kV cross-linked inner shielding material with batch number 202003D14 and box number 22 produced in Jiangyin, Jiangsu Province was evaluated and recorded as 2#;
[0068] The process of the heat extension test and the temperature rise test is the same as that of Example 1. The results of the heat extension test are shown in Table 1, and the results of the temperature rise test are shown in Table 2. It can be seen from Table 1 that the elongation of the 2# inner shielding cross-linked material after vulcanization for 3 minutes is 225%, the elongation of the vulcanization for 5 minutes is 102%, the elongation of the vulcanization for 10 minutes is 95%, and the elongation of the vulcanization for 15 minutes is 84%, which does not meet the trend of the heat extension change, and it is determined that the heat extension test of the 2# cross-linked inner shielding material to be evaluated is unqualified. It can be seen from Table 2 that the temperature rise of the 2# feeding section is 0°C, the temperature rise of the melting section is 6°C, and the temperature rise of the homogenization section is 7°C, which does not meet the temperature rise requirements, and the temperature rise test of the 2# cross-linked inner shielding material to be evaluated is unqualified.
[0069] The thermal extension test and temperature rise test of the 2# cross-linked inner shielding material to be evaluated were both unqualified, and the 2# cross-linked inner shielding material was determined to be a substandard product.
[0070] Example 3
[0071] The 10kV cross-linked inner shielding material with batch number 210109 and box number 18 produced by Zhejiang Xinfangde was evaluated and recorded as 3#;
[0072] The process of the heat extension test and the temperature rise test is the same as that of Example 1. The results of the heat extension test are shown in Table 1, and the results of the temperature rise test are shown in Table 2. It can be seen from Table 1 that the elongation of the 3# inner shielding cross-linked material after vulcanization for 3 minutes is 200%, the elongation of the vulcanization for 5 minutes is 90%, the elongation of the vulcanization for 10 minutes is 80%, and the elongation of the vulcanization for 15 minutes is 70%, which does not meet the trend of the heat extension change, and it is determined that the heat extension test of the 3# cross-linked inner shielding material to be evaluated is unqualified; it can be seen from Table 2 that the temperature rise of the 3# feeding section is 3°C, the temperature rise of the melting section is 8°C, and the temperature rise of the homogenization section is 10°C, which does not meet the temperature rise requirements, and the temperature rise test of the 3# cross-linked inner shielding material to be evaluated is unqualified;
[0073] The thermal extension test and temperature rise test of the 3# cross-linked inner shielding material to be evaluated were both unqualified, and the 3# cross-linked inner shielding material was determined to be a substandard product.
[0074] Example 4
[0075] The 10kV cross-linked inner shielding material with batch number 210109 and box number 09 produced by Nanjing Zhongchao was evaluated and recorded as 4#;
[0076] The process of the heat extension test and the temperature rise test is the same as that of Example 1. The results of the heat extension test are shown in Table 1, and the results of the temperature rise test are shown in Table 2. It can be seen from Table 1 that the elongation of the 4# inner shielding cross-linked material after vulcanization for 3 minutes is 80%, the elongation of the vulcanization for 5 minutes is 65%, the elongation of the vulcanization for 10 minutes is 60%, and the elongation of the vulcanization for 15 minutes is 60%, which does not meet the trend of the heat extension change, and it is determined that the heat extension test of the 4# cross-linked inner shielding material to be evaluated is unqualified; it can be seen from Table 2 that the temperature rise of the 4# feeding section is 7°C, the temperature rise of the melting section is 12°C, and the temperature rise of the homogenization section is 15°C, which does not meet the temperature rise requirements, and the temperature rise test of the 4# cross-linked inner shielding material to be evaluated is unqualified;
[0077] The thermal extension test and temperature rise test of the 4# cross-linked inner shielding material to be evaluated were both unqualified, and the 4# cross-linked inner shielding material was determined to be a substandard product.
[0078] Table 1 Thermal extension test results of Examples 1 to 4
[0079]
[0080] It can be seen from Table 1 that the thermal extension properties of the cross-linked inner shielding materials produced by the four manufacturers after curing for 15 minutes all meet the requirements of JB / T 10738-2007 "Semi-conductive shielding materials for extruded insulated cables with rated voltages of 35kV and below". In addition, the difference in the thermal extension index of the cross-linked inner shielding materials produced by the four manufacturers becomes smaller and smaller as the curing time increases. At 15 minutes, this difference is already very small.
[0081] The cross-linked inner shielding material produced by manufacturer 4# obviously has too much cross-linking agent (either the cross-linking agent is unevenly dispersed, or the material has been pre-cross-linked at the manufacturer). The elongation under load at 3 minutes is only 80%, indicating that the cross-linking has been completed in a relatively short time. The product is unqualified and cannot be used to prepare cross-linked cables.
[0082] The change trend of the thermal extension index of the cross-linked inner shielding material produced by the 1# manufacturer is relatively slow, which is manifested in the fact that premature cross-linking is not easy to occur in production. The change trend of the thermal extension index of the cross-linked inner shielding material produced by the 2# and 3# manufacturers is relatively steep, which is manifested in the fact that premature cross-linking is easy to occur in production.
[0083] Table 2 Temperature rise test results of Examples 1 to 4
[0084]
[0085]
[0086] It can be seen from Table 2 that the cross-linked inner shielding material produced by manufacturer 1# has low frictional heat generation, which is similar to the cooling capacity of the extruder, so the temperature rise is relatively low. In addition, in actual use, no premature cross-linking phenomenon occurs.
[0087] The cross-linked inner shielding materials produced by manufacturers 2# and 3# generate large friction heat, which is greater than the cooling capacity of the extruder, so the temperature rise is relatively high. In addition, in actual use, several tests have shown that premature cross-linking occurred after a few hours of production, so the products had to be returned.
[0088] The cross-linked inner shielding material produced by the 4# manufacturer has been pre-cross-linked, so the friction heat is large and the temperature rise is the highest, which is basically unusable. In addition, in actual use, during the production preparation stage, the surface of the die head material extruded by the extruder is rough. After several adjustments, it cannot be improved. It is obvious that the phenomenon of pre-cross-linking has occurred. It cannot be used for cross-linked cable production and can only be returned.
[0089] The 10kV cross-linked inner shielding material produced by manufacturers 1#, 2# and 3# was used to make the cross-linked cable insulation core, and its electrical performance was tested. The test results are shown in Table 3.
[0090] Table 3 Electrical properties of cross-linked cable insulation cores made of 10kV cross-linked inner shielding materials produced by manufacturers 1#, 2#, and 3#
[0091]
[0092]
[0093] It can be seen from Table 3 that, voltage test: the cable insulation cores prepared with 10kV cross-linked inner shielding materials produced by 1#, 2# and 3# manufacturers all meet the standard requirements and are not broken down; partial discharge test: the cable insulation cores prepared with 10kV cross-linked inner shielding materials produced by 1# manufacturer meet the standard requirements and have a small discharge amount (when the test sensitivity is 5pC, the measured value is 3pC), the cable insulation cores prepared with 10kV cross-linked inner shielding materials produced by 2# manufacturer do not meet the standard requirements and have a high discharge amount (when the test sensitivity is 7.8pC, the measured value is 82pC), the cable insulation cores prepared with 10kV cross-linked inner shielding materials produced by 3# manufacturer do not meet the standard requirements and have a high discharge amount (when the test sensitivity is 9.5pC, the measured value is 104pC); 4h withstand voltage test: the cable insulation cores prepared with 10kV cross-linked inner shielding materials produced by 1# manufacturer meet the standard requirements and are not broken down, the cable insulation cores prepared with 10kV cross-linked inner shielding materials produced by 2# and 3# manufacturers do not meet the standard requirements and have broken down. This indicates that the cables made of 10kV cross-linked inner shielding material produced by manufacturer 1# are of higher quality, while the cables made of materials from manufacturers 2# and 3# have quality risks, thus proving that the evaluation method provided by the present invention is accurate and reliable.
[0094] It can be seen from the above embodiments that the evaluation method provided by the present invention can select cross-linked inner shielding materials that are not prone to premature cross-linking from a large number of inner shielding materials, and provides the necessary technical support for selecting the cross-linked inner shielding materials with the best performance for the preparation of cross-linked cables and improving the quality of cross-linked cable products.
[0095] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for evaluating a cross-linked internal shielding material, comprising performing a heat extension test and a temperature rise test on the cross-linked internal shielding material to be evaluated; if both the heat extension test and the temperature rise test of the cross-linked internal shielding material to be evaluated are qualified, the cross-linked internal shielding material to be evaluated is determined to be a qualified product; The thermal extension test comprises the following steps: (1) Plasticizing the cross-linked inner shielding material to be evaluated to obtain a film; (2) vulcanizing the film obtained in step (1) to obtain a sample to be tested; (3) Testing the thermal elongation performance of the sample to be tested obtained in step (2); if the thermal elongation change trend of the sample to be tested meets the following requirements: the elongation after vulcanization for 3 minutes is ≥300%, the elongation after vulcanization for 5 minutes is 150-200%, the elongation after vulcanization for 10 minutes is 100-120%, and the elongation after vulcanization for 15 minutes is 50-80%, then the thermal elongation test of the cross-linked inner shielding material to be evaluated is determined to be qualified; if the thermal elongation change trend of the sample to be tested does not meet the above requirements, then the thermal elongation test of the cross-linked inner shielding material to be evaluated is determined to be unqualified; The temperature rise test includes: extruding the cross-linked internal shielding material to be evaluated in three stages, and then testing the temperature rise of the extruder body; if the temperature rise meets the following conditions: feeding stage <3°C, melting stage <4°C, homogenization stage <5°C, the temperature rise test of the cross-linked internal shielding material to be evaluated is qualified; otherwise, the temperature rise test of the cross-linked internal shielding material to be evaluated is judged to be unqualified.
2. The evaluation method according to claim 1, characterized in that: The plasticizing temperature in the step (1) is less than 70°C.
3. The evaluation method according to claim 1 or 2, characterized in that: The equipment used for plasticization in step (1) is a double-drum plastic purifying machine; the roller distance of the double-drum plastic purifying machine is 2.0-2.5 mm.
4. The evaluation method according to claim 1, characterized in that: The plasticizing process in step (1) also includes making triangle bags; the time for making the triangle bags is 3 to 4 minutes.
5. The evaluation method according to claim 1, characterized in that: The vulcanization temperature in step (2) is 180-183°C.
6. The evaluation method according to claim 1, characterized in that: The test samples obtained in step (2) include samples with vulcanization times of 3 min, 4 min, 5 min, 10 min and 15 min.
7. The evaluation method according to claim 1, characterized in that: The pressurization method before vulcanization in step (2) is: first pressurize to 13-15 MPa for 20-25 seconds, then reduce the pressure to 0 MPa and hold for 10-15 seconds, and finally pressurize to 15-20 MPa.
8. The evaluation method according to claim 1, characterized in that: The size of the sample to be tested in step (2) is 200 mm×200 mm, and the thickness is 1.0±0.1 mm.
9. The evaluation method according to claim 1, characterized in that: The initial temperature of the feeding section of the extruder body is 95-98°C, the initial temperature of the melting section of the extruder body is 100-103°C, and the initial temperature of the homogenizing section of the extruder body is 105-108°C.
10. The evaluation method according to claim 1, characterized in that: The time for the temperature rise of the test extruder body is 5 to 6 minutes after the three-stage extrusion.
Citation Information
Patent Citations
Screen material for 35kV grade high / medium voltage crosslinked cable conductor layer and preparation method thereof
CN101817950A
Method for blocking water during vulcanization of rubber sleeve cable
CN113782275A
Method for evaluating rheological property of crosslinked semiconductive shielding material
CN114216926A
Evaluation method for sheath material used in fire- retardant cable
JP2003185606A
Foam of urethane-based thermoplastic elastomer composition and process for producing the foam
JP2007238958A