A preparation method of modified sodium iron phosphate composite material
By introducing graphene oxide and a carbon source into sodium iron phosphate materials and employing Ti/W co-coating technology, the conductivity and ion diffusion rate of sodium iron phosphate composite materials were improved, solving the problems of poor conductivity and insufficient stability in existing materials and achieving a high-efficiency improvement in sodium-ion battery performance.
Patent Information
- Application Number
- CN202210436639.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-24
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-04-24
AI Technical Summary
Existing sodium iron phosphate cathode materials have complex operation processes and high costs. Their conductivity, specific capacity and rate performance need to be improved, and their structural stability and thermal stability are insufficient, which affects the cycle stability and safety of sodium-ion batteries.
By introducing a mixture of graphene oxide and a carbon source into sodium iron phosphate material, a sodium iron phosphate composite material is formed. The Ti/W co-coating technology is used to shorten the sodium ion diffusion distance, improve electronic conductivity and ion diffusion rate, and enhance the cycling stability of the material.
The discharge specific capacity and cycle stability of sodium iron phosphate composite materials were improved, the structural stability and thermal stability of the materials were enhanced, and the electrochemical performance and safety of sodium-ion batteries were improved.
Smart Images

Figure CN114824212B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of sodium ion battery positive electrode materials, and particularly relates to a method for preparing a modified sodium iron phosphate composite material. Background Art
[0002] The development of green energy storage technology can effectively alleviate energy crisis, environmental pollution and other issues. Lithium-ion batteries have become one of the most advanced energy storage technologies with their high energy density, safety and environmental protection. However, the limited lithium resources, uneven distribution and high cost have hindered the development of lithium-ion batteries. Sodium and lithium belong to the same main group with similar chemical properties. Sodium has the advantages of abundant and extensive resources and low cost, and is considered to be one of the potential alternative products to lithium-ion batteries.
[0003] Among the many positive electrode materials for sodium ion batteries, polyanionic compounds are considered to be the most promising type of electrode materials due to their excellent structural stability, safety and suitable voltage platform. Among them, sodium iron phosphate materials are abundant in raw materials, low in price, have three-dimensional ion diffusion channels, and good safety performance, which has attracted widespread attention. At present, researchers have made a lot of efforts to improve the electrochemical properties and structural stability of sodium iron phosphate. For example, CN105161688A discloses a carbon-coated sodium iron phosphate-sodium vanadium phosphate composite material and a preparation method thereof. Iron vanadate is first prepared, and then iron vanadate is used as a raw material to obtain carbon-coated sodium iron phosphate-sodium vanadium phosphate through ball milling, re-milling, calcination and other steps. The obtained material has a first charge and discharge capacity of 101.8 mAh·g at a voltage range of 2.0-4.0 V and a rate of 1C. -1 ; During the charge and discharge process, after 1C cycle 50 times, the capacity retention rate can reach 96.5%. CN113526483A discloses a pyrophosphate-type positive electrode material and a preparation method thereof, which is prepared by a sol-gel process with low-temperature heat treatment, by mixing sodium carbonate, ferrous oxalate or ferrous oxalate hydrate, ammonium dihydrogen phosphate or diammonium hydrogen phosphate, and forming a gel through ball milling, magnetic stirring, and evaporation, and then drying, low-temperature treatment, high-temperature sintering, and grinding to obtain the pyrophosphate-type positive electrode material. The obtained material has an initial charge and discharge capacity of 154 mAh g at a voltage range of 1.5-4.5 V and a rate of 0.1 C. -1 During the charge and discharge process, after 50 cycles at 1C, the capacity retention rate can reach 85.7%. Although the electrochemical performance of sodium iron phosphate has been improved to a certain extent, the operation process is complicated and costly, and its conductivity, specific capacity and rate performance still have room for further improvement.
[0004] Therefore, there is an urgent need to develop a sodium iron phosphate positive electrode material that is simple to operate, highly safe, and low-cost. The resulting positive electrode material has higher structural stability, thermal stability, and rapid ion diffusion kinetics, which helps to improve battery cycle stability and safety, and is of great significance for the development of sodium-ion batteries with long life, high energy density, and high thermal stability. Summary of the invention
[0005] The object of the present invention is to provide a method for preparing a modified sodium iron phosphate composite material, and the specific scheme is as follows:
[0006] A method for preparing a modified sodium iron phosphate composite material comprises the following steps:
[0007] (1) mixing a sodium source and graphene oxide uniformly in a mixer, adding iron phosphate and a carbon source to the mixture, and mixing uniformly in a mixer;
[0008] (2) sintering the product obtained in step (1) once in a nitrogen atmosphere to obtain a sintered material;
[0009] (3) crushing and sieving the calcined material obtained in step (2);
[0010] (4) mixing the sodium iron phosphate composite material obtained in step (3) with a titanium source and a tungsten source in a mixer, wherein the coating amount of the titanium source is 0.2-0.8%, the coating amount of the tungsten source is 0.3-0.8%, and the mixing time is 0.5-10 h;
[0011] (5) The product obtained in step (4) is subjected to secondary sintering under a nitrogen atmosphere, and after screening, a Ti / W co-coated sodium iron phosphate composite material is obtained.
[0012] The molar ratio of the P element, Fe element, C element and Na element in the added material in step (1) is 1:1:2:1-1.05.
[0013] In step (1), the weight ratio of graphene oxide to sodium source is 0.5-1.5:1.
[0014] The sodium source in step (1) is at least one of sodium carbonate, sodium bicarbonate, sodium hydroxide, sodium acetate, sodium nitrate, sodium phosphate, sodium hydrogen phosphate, sodium oxalate, sodium formate, sodium citrate, sodium pyrophosphate or sodium metaphosphate.
[0015] The carbon source in step (1) is any one of glucose, sucrose, PVA, citric acid, ascorbic acid, tartaric acid or oxalic acid, or a combination of at least two thereof.
[0016] In step (2), the sintering is carried out at a heating rate of 1 to 5°C / min to 500-800°C, and the holding time is 10-15h.
[0017] In step (4), the coating amount of the titanium source is 0.6%, and the coating amount of the tungsten source is 0.5%.
[0018] The mixer in step (4) is a ball mill mixer or a high-speed mixer.
[0019] The secondary sintering temperature in step (5) is 300-600° C. and the sintering time is 2-8 hours.
[0020] The present invention loads sodium carbonate on the surface of graphene oxide, and the graphene oxide is wound to a certain extent during the thermal reduction process to form a sodium iron phosphate composite material, which shortens the diffusion distance of sodium ions, so that the sodium ions can move quickly in the interface layer during the charge and discharge process, and the transmission rate is faster. At the same time, the phase transition of sodium ions during the sodium ion deintercalation process is improved, and the discharge specific capacity is improved, which solves the problems of poor electronic conductivity and slow ion diffusion rate of sodium iron phosphate in the prior art, and has excellent electrochemical performance. Subsequently, Ti / W co-coating is adopted, which can penetrate into the surface layer of the material and the lattice gap of the deep filling material, inhibit the dissolution of sodium ions in the material during the charge and discharge process, reduce the consumption of sodium ions by SEI film repair, improve the specific capacity and rate characteristics of the material, and under the condition of adding 0.2-0.8% of titanium source and 0.3-0.8% of tungsten source, the cycle stability can be well enhanced. Under the condition of adding titanium / tungsten alone or the addition amount exceeds the range, the capacity and performance of the material are reduced. By utilizing the coordinated effect between the two, the surface loss of sodium ion deintercalation during charging and discharging can be reduced, the growth of Na dendrites can be inhibited, and the side reaction with the electrolyte can be further inhibited, thereby increasing the stability of the material and enhancing the cycle stability of the sodium iron phosphate composite material. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a process flow chart of a method for preparing a modified sodium iron phosphate composite material of the present invention;
[0022] Figure 2 is a scanning electron microscope (SEM) image of the modified sodium iron phosphate composite material prepared in Example 1;
[0023] Figure 3 is the XRD diffraction spectrum of the modified sodium iron phosphate composite material prepared in Example 1;
[0024] Figure 4 It is the 1C cycle performance diagram of Example 1 and Comparative Examples 1-3. DETAILED DESCRIPTION
[0025] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments in this application can be combined with each other. In order to further understand the present invention, the present invention is further described below in conjunction with the specification and specific preferred embodiments, and these embodiments cannot be understood as limiting the scope of protection claimed in this application.
[0026] Example 1
[0027] This embodiment provides a modified sodium iron phosphate composite material, and the preparation method of the modified sodium iron phosphate composite material is as follows:
[0028] Take graphene oxide and sodium carbonate, weigh them according to the weight ratio of graphene oxide to sodium carbonate of 1:1, add them into a high-speed mixing device, mix them at 1000rpm for 20min, then add iron phosphate and citric acid according to the molar ratio of P element, Fe element, C element and Na element of 1:1:2:1-1.05, mix them evenly at 800rpm, and load them into a tube furnace. After nitrogen is passed for 30min, the temperature is increased at a rate of 3℃ / min to 700℃, kept at this temperature for 10h, cooled to room temperature, crushed, pulverized, and passed through a 400-mesh sieve to obtain a primary sintered material.
[0029] The obtained primary sintered material was mixed with nano titanium oxide and nano tungsten trioxide in a molar ratio of 1:0.006:0.005, heated to 500°C at a heating rate of 3°C / min in a nitrogen atmosphere, and sintered for 5 hours. After cooling to room temperature and screening, the final modified sodium iron phosphate composite material was obtained.
[0030] Example 2
[0031] Similar to Example 1, graphene oxide and sodium carbonate were weighed and added to a high-speed mixing device at a weight ratio of 0.5:1, mixed at 1000 rpm for 20 min, and then iron phosphate and citric acid were added at a molar ratio of 1:1:2:1-1.05 among P element, Fe element, C element, and Na element, mixed evenly at 800 rpm, and loaded into a tubular furnace. After nitrogen was passed for 30 min, the temperature was increased at a heating rate of 3°C / min to 700°C, kept warm for 10 h, cooled to room temperature, crushed, pulverized, and passed through a 400-mesh sieve to obtain a primary sintered material.
[0032] The obtained primary sintered material was mixed with nano titanium oxide and nano tungsten trioxide in a molar ratio of 1:0.006:0.005, heated to 500°C at a heating rate of 3°C / min in a nitrogen atmosphere, and sintered for 5 hours. After cooling to room temperature and screening, the final modified sodium iron phosphate composite material was obtained.
[0033] Example 3
[0034] Similar to Example 1, graphene oxide and sodium carbonate were weighed and added to a high-speed mixing device at a weight ratio of 1:1 to graphene oxide and sodium carbonate, and then iron phosphate and citric acid were added at a molar ratio of 1:1:2:1-1.05 among P element, Fe element, C element, and Na element, mixed at 1000 rpm for 20 minutes, then mixed at 800 rpm, and loaded into a tubular furnace. After nitrogen was passed for 30 minutes, the temperature was increased at a heating rate of 3°C / min to 700°C, kept warm for 10 hours, cooled to room temperature, crushed, and pulverized, and then passed through a 400-mesh sieve to obtain a primary sintered material.
[0035] The obtained primary sintered material was mixed with nano titanium oxide and nano tungsten trioxide in a molar ratio of 1:0.006:0.005, heated to 500°C at a heating rate of 3°C / min in a nitrogen atmosphere, and sintered for 5 hours. After cooling to room temperature and screening, the final modified sodium iron phosphate composite material was obtained.
[0036] Example 4
[0037] Similar to Example 1, an equal amount of sodium carbonate was added to a high-speed mixing device, mixed at 1000 rpm for 20 min, and then ferric phosphate and citric acid were added according to the molar ratio of P element, Fe element, C element, and Na element of 1:1:2:1-1.05, mixed evenly at 800 rpm, and loaded into a tubular furnace. After nitrogen was passed for 30 min, the temperature was increased at a rate of 3°C / min to 700°C, kept warm for 10 h, cooled to room temperature, crushed, pulverized, and passed through a 400-mesh sieve to obtain a primary sintered material.
[0038] The obtained primary sintered material was mixed with nano titanium oxide and nano tungsten trioxide in a molar ratio of 1:0.006:0.005, heated to 500°C at a heating rate of 3°C / min in a nitrogen atmosphere, and sintered for 5 hours. After cooling to room temperature and screening, the final modified sodium iron phosphate composite material was obtained.
[0039] Example 5
[0040] Take graphene oxide and sodium bicarbonate, weigh them according to the weight ratio of graphene oxide to sodium bicarbonate of 1:1, add them into a high-speed mixing device, mix them at 1000rpm for 20min, then add iron phosphate and citric acid according to the molar ratio of P element, Fe element, C element and Na element of 1:1:2:1-1.05, mix them evenly at 800rpm, and load them into a tubular furnace. After nitrogen is passed for 30min, the temperature is increased at a heating rate of 3℃ / min to 700℃, and the temperature is kept for 10h, cooled to room temperature, crushed, pulverized, and passed through a 400-mesh sieve to obtain a primary sintered material.
[0041] The obtained primary sintered material was mixed with nano titanium oxide and nano tungsten trioxide in a molar ratio of 1:0.006:0.005, heated to 500°C at a heating rate of 3°C / min in a nitrogen atmosphere, and sintered for 5 hours. After cooling to room temperature and screening, the final modified sodium iron phosphate composite material was obtained.
[0042] Example 6
[0043] Take graphene oxide and sodium oxalate, weigh them according to the weight ratio of graphene oxide to sodium oxalate of 1:1, add them into a high-speed mixing device, mix them at 1000rpm for 20min, then add ferric phosphate and citric acid according to the molar ratio of P element, Fe element, C element and Na element of 1:1:2:1-1.05, mix them evenly at 800rpm, and load them into a tube furnace. After nitrogen is passed for 30min, the temperature is increased at a rate of 3℃ / min to 700℃, kept warm for 10h, cooled to room temperature, crushed, pulverized, and passed through a 400-mesh sieve to obtain a primary sintered material.
[0044] The obtained primary sintered material was mixed with nano titanium oxide and nano tungsten trioxide in a molar ratio of 1:0.006:0.005, heated to 500°C at a heating rate of 3°C / min in a nitrogen atmosphere, and sintered for 5 hours. After cooling to room temperature and screening, the final modified sodium iron phosphate composite material was obtained.
[0045] Example 7
[0046] Take graphene oxide and sodium acetate, weigh them according to the weight ratio of graphene oxide to sodium acetate of 1:1, add them into a high-speed mixing device, mix them at 1000rpm for 20min, then add iron phosphate and citric acid according to the molar ratio of P element, Fe element, C element and Na element of 1:1:2:1-1.05, mix them evenly at 800rpm, and load them into a tubular furnace. After nitrogen is passed for 30min, the temperature is increased at a rate of 3℃ / min to 700℃, and the temperature is kept for 10h, cooled to room temperature, crushed, pulverized, and passed through a 400-mesh sieve to obtain a primary sintered material.
[0047] The obtained primary sintered material was mixed with nano titanium oxide and nano tungsten trioxide in a molar ratio of 1:0.006:0.005, heated to 500°C at a heating rate of 3°C / min in a nitrogen atmosphere, and sintered for 5 hours. After cooling to room temperature and screening, the final modified sodium iron phosphate composite material was obtained.
[0048] Example 8
[0049] Take graphene oxide and sodium carbonate, weigh them according to the weight ratio of graphene oxide to sodium carbonate of 1:1, add them into a high-speed mixing device, mix them at 1000rpm for 20min, then add iron phosphate and citric acid according to the molar ratio of P element, Fe element, C element and Na element of 1:1:2:1-1.05, mix them evenly at 800rpm, and load them into a tube furnace. After nitrogen is passed for 30min, the temperature is increased at a rate of 3℃ / min to 700℃, kept at this temperature for 10h, cooled to room temperature, crushed, pulverized, and passed through a 400-mesh sieve to obtain a primary sintered material.
[0050] The obtained primary sintered material was mixed with nano titanium oxide and nano tungsten trioxide in a molar ratio of 1:0.003:0.005, heated to 500°C at a heating rate of 3°C / min in a nitrogen atmosphere, and sintered for 5 hours. After cooling to room temperature and screening, the final modified sodium iron phosphate composite material was obtained.
[0051] Example 9
[0052] Take graphene oxide and sodium carbonate, weigh them according to the weight ratio of graphene oxide to sodium carbonate of 1:1, add them into a high-speed mixing device, mix them at 1000rpm for 20min, then add iron phosphate and citric acid according to the molar ratio of P element, Fe element, C element and Na element of 1:1:2:1-1.05, mix them evenly at 800rpm, and load them into a tube furnace. After nitrogen is passed for 30min, the temperature is increased at a rate of 3℃ / min to 700℃, kept at this temperature for 10h, cooled to room temperature, crushed, pulverized, and passed through a 400-mesh sieve to obtain a primary sintered material.
[0053] The obtained primary sintered material was mixed with nano titanium oxide and nano tungsten trioxide in a molar ratio of 1:0.006:0.002, heated to 500°C at a heating rate of 3°C / min in a nitrogen atmosphere, and sintered for 5 hours. After cooling to room temperature and screening, the final modified sodium iron phosphate composite material was obtained.
[0054] Example 10
[0055] Take graphene oxide and sodium carbonate, weigh them according to the weight ratio of graphene oxide to sodium carbonate of 1:1, add them into a high-speed mixing device, mix them at 1000rpm for 20min, then add iron phosphate and citric acid according to the molar ratio of P element, Fe element, C element and Na element of 1:1:2:1-1.05, mix them evenly at 800rpm, and load them into a tube furnace. After nitrogen is passed for 30min, the temperature is increased at a rate of 3℃ / min to 700℃, kept at this temperature for 10h, cooled to room temperature, crushed, pulverized, and passed through a 400-mesh sieve to obtain a primary sintered material.
[0056] The obtained primary sintered material was mixed with nano titanium oxide and nano tungsten trioxide in a molar ratio of 1:0.003:0.002, heated to 500°C at a heating rate of 3°C / min in a nitrogen atmosphere, and sintered for 5 hours. After cooling to room temperature and screening, the final modified sodium iron phosphate composite material was obtained.
[0057] Embodiment 11
[0058] Take graphene oxide and sodium carbonate, weigh them according to the weight ratio of graphene oxide to sodium carbonate of 1:1, add them into a high-speed mixing device, mix them at 1000rpm for 20min, then add iron phosphate and citric acid according to the molar ratio of P element, Fe element, C element and Na element of 1:1:2:1-1.05, mix them evenly at 800rpm, and load them into a tube furnace. After nitrogen is passed for 30min, the temperature is increased at a rate of 3℃ / min to 700℃, kept at this temperature for 10h, cooled to room temperature, crushed, pulverized, and passed through a 400-mesh sieve to obtain a primary sintered material.
[0059] The obtained primary sintered material was mixed with nano titanium oxide and nano tungsten trioxide in a molar ratio of 1:0.002:0.008, heated to 500°C at a heating rate of 3°C / min in a nitrogen atmosphere, and sintered for 5 hours. After cooling to room temperature and screening, the final modified sodium iron phosphate composite material was obtained.
[0060] Example 12
[0061] Take graphene oxide and sodium carbonate, weigh them according to the weight ratio of graphene oxide to sodium carbonate of 1:1, add them into a high-speed mixing device, mix them at 1000rpm for 20min, then add iron phosphate and glucose according to the molar ratio of P element, Fe element, C element and Na element of 1:1:2:1-1.05, mix them evenly at 800rpm, and load them into a tubular furnace. After nitrogen is passed for 30min, the temperature is increased at a rate of 3℃ / min to 700℃, kept warm for 10h, cooled to room temperature, crushed, pulverized, and passed through a 400-mesh sieve to obtain a primary sintered material.
[0062] The obtained primary sintered material was mixed with nano titanium oxide and nano tungsten trioxide in a molar ratio of 1:0.008:0.008, heated to 500°C at a heating rate of 3°C / min in a nitrogen atmosphere, and sintered for 5 hours. After cooling to room temperature and screening, the final modified sodium iron phosphate composite material was obtained.
[0063] Comparative Example 1
[0064] The difference between this comparative example and Example 1 is that only nano-titanium oxide is coated but not nano-tungsten trioxide. Other conditions and parameters are exactly the same as those in Example 1.
[0065] Comparative Example 2
[0066] The only difference between this comparative example and Example 1 is that nano-titanium oxide is not coated but nano-tungsten trioxide is coated. Other conditions and parameters are exactly the same as those in Example 1.
[0067] Comparative Example 3
[0068] The only difference between this comparative example and Example 1 is that nano titanium oxide and nano tungsten trioxide are not coated, and other conditions and parameters are exactly the same as those in Example 1.
[0069] Performance Testing:
[0070] 1) First discharge capacity and coulombic efficiency test: The button cells prepared from the positive electrode materials in Examples 1-4 were tested using a blue electric tester with a voltage range of 2.0-4.5 V and a 0.1C charge and discharge activation cycle to obtain the first charge and discharge specific capacity and the first coulombic efficiency. The test results are shown in Table 1.
[0071] 2) 1C cycle performance: The button batteries prepared with the positive electrode materials in Example 1 and Comparative Examples 1-3 were tested using a blue electric tester with a voltage range of 2.0-4.5V. They were activated for one cycle with 0.1C charge and discharge, and then charged at 0.5C constant current and constant voltage, with a cut-off current of 0.05C, and discharged at 1C current for 100 cycles to obtain relevant data on parameters such as the 100th cycle discharge capacity and the 100th cycle capacity retention rate.
[0072] The test results are shown in Table 2 and Figure 4 shown.
[0073] 3) Rate performance: The button batteries prepared with the positive electrode materials in Examples 1-4 and Comparative Examples 1-3 were tested using a blue electric tester with a voltage range of 2.0-4.5V. Constant current and constant voltage charging was performed at a current of 0.5C, and the charging cut-off current was 0.05C; constant current discharge was performed at currents of 0.1C, 0.3C, 0.5C, 1C, 2C, 5C, and 0.1C, respectively, and the discharge cut-off voltage was 2V.
[0074] The test results are shown in Table 3.
[0075] evaluate
[0076] Table 1
[0077]
[0078] From the first charge and discharge specific capacity and the first coulomb efficiency in Table 1, it can be seen that the modified sodium iron phosphate composite material of Example 1 prepared according to the present invention has a higher charge specific capacity and discharge specific capacity, and the first charge and discharge efficiency reaches 97.47%, which is higher than that of Examples 2 to 12. By compounding with graphene oxide, the discharge specific capacity is improved, the problems of poor electronic conductivity and slow ion diffusion rate of sodium iron phosphate in the prior art are solved, and it has excellent electrochemical properties.
[0079] Table 2
[0080]
[0081] Table 2 is the cycle performance related data of Example 1 and Comparative Examples 1-3. It can be seen from the table that the capacity retention rate of the modified sodium iron phosphate composite material prepared in Example 1 after 100 cycles is improved to 98.35%, while the capacity retention rates of Comparative Examples 1-3 after 100 cycles of the test are all reduced under the experimental conditions without Ti / W co-coating.
[0082] Figure 4 It is a 1C cycle performance diagram of Example 1 and Comparative Examples 1-3. The diagram shows that the capacity retention rate of the modified sodium iron phosphate composite material co-coated with Ti / W is increased from 94.70% to 98.35% after 100 cycles compared with the sodium iron phosphate material not co-coated with Ti / W, thereby improving the cycle stability of the sodium iron phosphate composite material.
[0083] Table 3
[0084]
[0085]
[0086] Table 3 is the relevant data of the rate performance of Examples 1-4 and Comparative Examples 1-3. It can be seen from the table that the capacity retention rate of the modified sodium iron phosphate composite material prepared in Example 1 at 5C rate reaches 91.20%, and the 0.1C capacity retention rate after the large rate test is still as high as 99.1%. The capacity retention rate of the Ti / W co-coated modified sodium iron phosphate composite material at 5C rate is increased from 61.70% to 91.2% compared with the uncoated sodium iron phosphate composite material, which proves that the Ti / W co-coating method can effectively improve the electronic conductivity and ionic conductivity of the material, increase the stability of the material, and improve the capacity and rate performance.
[0087] By comparing the embodiment with the comparative example, it is shown that before sintering, the surface of graphene oxide is loaded with sodium carbonate, and the sodium iron phosphate composite material is formed by sintering, which improves the phase transition of sodium ions during the sodium ion deintercalation process, improves the discharge specific capacity, solves the problems of poor electronic conductivity and slow ion diffusion rate of sodium iron phosphate in the prior art, and has excellent electrochemical performance. Subsequently, Ti / W co-coating can reduce the surface loss of sodium ion deintercalation during charging and discharging, inhibit the growth of Na dendrites, further inhibit the side reaction with the electrolyte, and enhance the cycle stability of the sodium iron phosphate composite material.
[0088] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a modified sodium iron phosphate composite material, characterized in that: The preparation method of the modified sodium iron phosphate composite material is as follows: Take graphene oxide and sodium carbonate, weigh them according to the weight ratio of graphene oxide to sodium carbonate of 1:1, add them into a high-speed mixing equipment, mix them at 1000rpm for 20min, then add iron phosphate and citric acid according to the molar ratio of P element, Fe element, C element and Na element of 1:1:2:1-1.05, mix them evenly at 800rpm, load them into a tubular furnace, heat them at a heating rate of 3°C / min after passing nitrogen for 30min, heat them to 700°C, keep them warm for 10h, cool them to room temperature, crush them and pass them through a 400-mesh sieve to obtain a primary sintered material; The obtained primary sintered material was mixed with nano titanium oxide and nano tungsten trioxide in a molar ratio of 1:0.006:0.005, heated to 500°C at a heating rate of 3°C / min in a nitrogen atmosphere, sintered for 5 hours, cooled to room temperature, and sieved to obtain a modified sodium iron phosphate composite material.
Citation Information
Patent Citations
Carbon-coated iron phosphate sodium-vanadium phosphate sodium composite material and preparation method thereof
CN105161688A
Ferrophosphorus sodium ore type positive electrode material and preparation method and application thereof
CN113526483A
Mixed conductor composite material LiFePO4-MXy and preparation method thereof
CN102427134A
Preparation method of lithium iron phosphate / graphene composite material, lithium ion battery cathode, and lithium ion battery
CN107170977A
Modified lithium iron phosphate positive electrode material and preparation method thereof, positive plate and lithium secondary battery
CN109390563A