Preparation method of friction nanogenerator based on three-dimensional multilayer film structure composite electrode

By using a three-dimensional multilayer film structure composite electrode and a laser-induced graphene electrode in a triboelectric nanogenerator, combined with silver nanowires and different fabric materials, the problem of unstable output performance of stretchable triboelectric nanogenerators in the existing technology is solved. , achieving high power density and good tensile stability, suitable for energy supply of wearable devices and human body monitoring.

CN114826015BActive Publication Date: 2024-10-18HEBEI UNIV OF TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202210533726.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-16
Publication Date
2024-10-18
Estimated Expiration
2042-05-16

AI Technical Summary

Technical Problem

Existing stretchable triboelectric nanogenerators suffer from unstable output performance and complex manufacturing processes during the stretching process, which limits their wide application in wearable electronic devices.

Method used

Using a three-dimensional multi-layer film structure composite electrode, laser-induced graphene electrodes are combined with silver nanowires, and an Ag NWs/LIG composite electrode is formed on a composite silicone rubber substrate. Different fabric materials are combined as triboelectric layers to prepare a high-power Density and good tensile stability of triboelectric nanogenerators.

Benefits of technology

The triboelectric nanogenerator has strong stretchability and high output stability. It can maintain good conductivity after 500 stretches and maintain stable electrical output under 10,000 working cycles. It is suitable for wearable electronic devices. Energy supply and human posture monitoring.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114826015B_ABST
    Figure CN114826015B_ABST
Patent Text Reader

Abstract

The present invention is a method for preparing a friction nanogenerator based on a composite electrode with a three-dimensional multilayer film structure. First, a laser-induced graphene electrode is obtained by laser etching on a polyimide film, a mixed silicone rubber solution is scraped on the laser-induced graphene electrode, and a composite silicone rubber substrate is obtained after heating and curing; then, silver nanowires are sprayed on the laser-induced graphene electrode in a pre-stretched state to form an Ag NWs / LIG composite electrode with a three-dimensional multilayer film structure on the composite silicone rubber substrate, and then the pre-stretching force is removed; finally, a negative friction electric layer film is pasted on the Ag NWs / LIG composite electrode as a negative friction electric layer to obtain a friction nanogenerator. The Ag NWs / LIG composite electrode has good tensile stability, overcomes the defect that the electrode square resistance value becomes larger when the laser-induced graphene electrode is transferred to the composite silicone rubber substrate, and also alleviates the deterioration of the electrical performance of the laser-induced graphene electrode under tensile deformation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of friction nanogenerator preparation, and specifically relates to a method for preparing a friction nanogenerator based on a three-dimensional multilayer film structure composite electrode. Background Art

[0002] The rapid development of the Internet of Things and artificial intelligence has greatly promoted the development of smart wearable electronic devices. In order to better realize functions such as human motion sensing and health monitoring, wearable electronic devices have higher requirements for flexibility, so they also have higher requirements for power supply flexibility.

[0003] Triboelectric nanogenerators (TENGs) are widely used in wearable electronic devices. As a new type of energy harvester, TENG has become a research hotspot in the field of nanotechnology. It mainly utilizes the friction electrification effect coupled with the electrostatic induction effect to effectively convert the mechanical energy generated by the external environment and the human body into electrical energy. TENG stands out from other power sources because of its wide range of material sources, simple and fast manufacturing process, flexibility and versatility. Although many studies have reported that TENG has ultra-high stretchability, most stretchable TENGs have the disadvantages of low power density, complex manufacturing process, and unstable electrical output performance after stretching.

[0004] The Chinese patent with publication number CN109889081A discloses "a stretchable friction nanogenerator in a single-electrode mode and a method for preparing the same". This method uses the spiral structure of the steel wire electrode to give TENG good stretchability, but due to the poor flexibility of the steel wire electrode, the output performance stability of the generator during the stretching process is poor. The patent application with publication number CN112260573A discloses "a stretchable friction nanogenerator and a method for preparing the same", using liquid metal as a conductive electrode to give TENG good flexibility. However, this method uses a method of simultaneously preparing the electrode layer by high-voltage electrostatic spraying of liquid metal micro-nanoparticles and high-voltage electrostatic spinning of polymer elastomer materials. Its production process is relatively complicated and costly, which is not conducive to large-scale production, limiting its development and application.

[0005] In summary, designing a TENG that combines low cost, large-scale production, good stretchability, high power density, and practicality is of great significance for the development of wearable electronic devices. Summary of the invention

[0006] In view of the deficiencies in the prior art, the technical problem to be solved by the present invention is to provide a method for preparing a friction nanogenerator based on a three-dimensional multilayer film structure composite electrode.

[0007] The technical solution adopted by the present invention to solve the technical problem is as follows:

[0008] A method for preparing a triboelectric nanogenerator based on a three-dimensional multilayer film structure composite electrode, wherein the triboelectric nanogenerator prepared by the method comprises, from top to bottom, a positive triboelectric layer, a negative triboelectric layer, an Ag NWs / LIG composite electrode and a composite silicone rubber substrate; the method comprising the following steps:

[0009] 1) performing laser etching on a polyimide film to obtain a laser-induced graphene electrode;

[0010] 2) Mixing a polydimethylsiloxane base solution and a curing agent in a volume ratio of 10:1 and performing magnetic stirring to prepare a polydimethylsiloxane solution; mixing solution A and solution B in a volume ratio of 1:1 and performing magnetic stirring to prepare an Ecolflex solution; mixing a polydimethylsiloxane solution and an Ecolflex solution in a volume ratio of 1:1 and performing magnetic stirring to obtain a mixed silicone rubber solution, and vacuuming the mixed silicone rubber solution to remove bubbles; wherein the Ecolflex solution is an aromatic random copolyester solution;

[0011] 3) The mixed silicone rubber solution from which bubbles are removed is evenly scraped onto the laser-induced graphene electrode of the polyimide film, and then vacuum-treated in a vacuum drying oven, dried, and cured to obtain a composite silicone rubber substrate, at which point the laser-induced graphene electrode is transferred to the composite silicone rubber substrate;

[0012] 4) pre-stretching the composite silicone rubber substrate, uniformly spraying a silver nanowire solution on the laser-induced graphene electrode in the pre-stretched state, forming a silver nanowire film on the laser-induced graphene electrode, and then forming a Ag NWs / LIG composite electrode with a three-dimensional multilayer film structure on the composite silicone rubber substrate, and then removing the pre-stretching force;

[0013] 5) evenly spin coating a solution for preparing a negative triboelectric layer on a glass plate, and heating and curing the solution to obtain a negative triboelectric layer film; removing the negative triboelectric layer film from the glass plate and pasting it onto the Ag NWs / LIG composite electrode;

[0014] 6) placing the cut fabric in an anhydrous ethanol solution for ultrasonic treatment, and drying the fabric after the ultrasonic treatment; placing the dried fabric as a positive triboelectric layer opposite to the negative triboelectric layer;

[0015] In step 5), the negative triboelectric layer film is a pure PDMS film, a PDMS / Ecoflex film or a MXene / silicone rubber composite film. When the MXene / silicone rubber composite film is used as the negative triboelectric layer, the output performance of the friction nanogenerator is optimal.

[0016] Compared with the prior art, the present invention has the following beneficial effects:

[0017] 1) The present invention transfers the laser-induced graphene electrode to a composite silicone rubber substrate, and sprays silver nanowires on the laser-induced graphene electrode to form a silver nanowire (Ag NWs) / laser-induced graphene (LIG) composite electrode with a three-dimensional multilayer film structure, so that the prepared friction nanogenerator has the characteristics of strong stretchability and high output stability. It is used as a power source for wearable electronic devices, which enhances the interactivity between wearable electronic devices and the human body and prolongs the service life of wearable electronic devices. Compared with pure LIG electrodes, the Ag NWs / LIG composite electrode prepared by the present invention not only overcomes the defect that the electrode square resistance value becomes larger when LIG is transferred to the composite silicone rubber substrate, but also alleviates the deterioration of the electrical properties of LIG under tensile deformation. The test results show that the Ag NWs / LIG composite electrode still has good conductivity after 500 stretchings, which indicates that the Ag NWs / LIG composite electrode has good tensile stability. In addition, the friction nanogenerator produced by this method has excellent tensile stability and durability. Under 30% tensile strain, the open circuit voltage attenuation of the generator is small, and it can still maintain stable electrical output after 10,000 working cycles (one working cycle is one contact and separation of the positive and negative friction electric layers).

[0018] 2) The friction nanogenerator prepared by the present invention can be attached to clothes or human skin and can be used as a wearable electronic device. On the one hand, as an energy collection device, it is attached to a joint with large deformation. The friction nanogenerator converts the mechanical energy generated during irregular human body movement into electrical energy, which provides energy for wearable electronic devices and solves the energy supply problem of wearable devices. On the other hand, it can also be used as a self-powered sensor. It is attached to a joint with small deformation. The friction nanogenerator can recognize human posture and monitor human breathing status to a certain extent. For example, the friction nanogenerator is attached to clothes, and the bending of human joints makes it contact with clothes to generate electrical signals, thereby identifying human posture; it can also be attached to the abdomen of the human body. The rise and fall of the abdomen when the human body breathes makes the generator contact with clothes to generate electrical signals, thereby monitoring the breathing frequency. All these show that the friction nanogenerator has good flexibility and practicality.

[0019] 3) The present invention uses nylon fabric with strong triboelectricity as the positive triboelectric layer, and together with the MXene / silicone rubber composite film as the negative triboelectric layer, it forms the triboelectric layer of the triboelectric nanogenerator, which enables the triboelectric nanogenerator to obtain more triboelectric charges when working. Since the MXene solution contains -F functional groups, the negative charge of the negative triboelectric layer can be increased; at the same time, the Ag NWs / LIG composite electrode with excellent conductivity and stretchability is used as the output electrode, so that the triboelectric charge accumulated in the triboelectric layer is easier to transfer, and finally a triboelectric nanogenerator with high power density is obtained. The triboelectric nanogenerator prepared in Example 3 can generate an open circuit voltage of 73.6V, a short circuit current of 7.75μA, and a power of 2.76W·m -2 The maximum power density. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 is a schematic structural diagram of the friction nanogenerator of the present invention;

[0021] Figure 2 It is a preparation flow chart of the present invention;

[0022] Figure 3(a) is a SEM image of a LIG electrode;

[0023] Figure 3(b) is a SEM image of the Ag NWs / LIG composite electrode;

[0024] Figure 4 It is a diagram showing the change in square resistance of the laser-induced graphene of the present invention before and after transfer and before and after pre-stretching of the Ag NWs / LIG composite electrode;

[0025] Figure 5(a) shows the open circuit voltage of the triboelectric nanogenerator with pure PDMS film, PDMS / Ecoflex film and MXene / silicone rubber composite film as negative triboelectric layer;

[0026] Figure 5(b) is a graph of the short-circuit current density of the triboelectric nanogenerators with pure PDMS film, PDMS / Ecoflex film, and MXene / silicone rubber composite film as negative triboelectric layers;

[0027] Figure 5(c) is a graph of the transferred charge density of the triboelectric nanogenerators with pure PDMS film, PDMS / Ecoflex film, and MXene / silicone rubber composite film as negative triboelectric layers;

[0028] Figure 6 The open circuit voltage diagram of the triboelectric nanogenerator obtained with different fabric materials as the positive triboelectric layer;

[0029] Figure 7(a) is a graph showing the resistance change rate of the LIG electrode and the Ag NWs / LIG composite electrode under different tensile strains;

[0030] Figure 7(b) is a graph showing the resistance change rate of the Ag NWs / LIG composite electrode under different pre-stretching conditions;

[0031] Figure 8 The open circuit voltage diagram of the triboelectric nanogenerator prepared in Example 3 under different tensile strains;

[0032] Fig. 9 This is the open circuit voltage diagram of the friction nanogenerator prepared in Example 3 after 10,000 working cycles;

[0033] FIG10( a ) is a diagram showing the load current density and load voltage of the triboelectric nanogenerator prepared in Example 3 under different load resistances;

[0034] FIG10( b ) is a diagram showing the power density of the friction nanogenerator prepared in Example 3 under different load resistances. DETAILED DESCRIPTION

[0035] The technical solution of the present invention is further explained below in conjunction with the drawings and embodiments, but the protection scope of the present application is not limited thereto.

[0036] The present invention discloses a method for preparing a triboelectric nanogenerator based on a three-dimensional multilayer film structure composite electrode. The triboelectric nanogenerator prepared by the method comprises a positive triboelectric layer, a negative triboelectric layer, an Ag NWs / LIG composite electrode and a composite silicone rubber substrate from top to bottom, wherein the Ag NWs / LIG composite electrode is located on the composite silicone rubber substrate, the negative triboelectric layer is attached to the Ag NWs / LIG composite electrode, and the positive triboelectric layer is located directly above the negative triboelectric layer. The method comprises the following steps:

[0037] 1) performing laser etching on a polyimide film to obtain a laser-induced graphene electrode; the etching power is 6.5-7.1 W, the etching speed is 348-372 mm / s, the density is 250-750 PPI, and the vertical distance between the etching grating and the polyimide film is 1.1-1.3 mm;

[0038] 2) Mixing a polydimethylsiloxane base solution and a curing agent in a volume ratio of 10:1 and performing magnetic stirring to prepare a polydimethylsiloxane solution; mixing solution A and solution B in a volume ratio of 1:1 and performing magnetic stirring to prepare an Ecolflex solution; mixing a polydimethylsiloxane solution and an Ecolflex solution in a volume ratio of 1:1 and performing magnetic stirring to obtain a mixed silicone rubber solution, and vacuuming the mixed silicone rubber solution to remove bubbles; wherein the Ecolflex solution is an aromatic random copolyester solution;

[0039] 3) The mixed silicone rubber solution from which bubbles are removed is evenly scraped onto the laser-induced graphene electrode of the polyimide film, with a scraping thickness of 0.8 to 1.2 mm, and then vacuum-treated in a vacuum drying oven, and then dried and cured to obtain a composite silicone rubber substrate, at which point the laser-induced graphene electrode is transferred to the composite silicone rubber substrate;

[0040] 4) pre-stretching the composite silicone rubber substrate, uniformly spraying a silver nanowire solution on the laser-induced graphene electrode in the pre-stretched state, forming a silver nanowire film on the laser-induced graphene electrode, and then forming a Ag NWs / LIG composite electrode with a three-dimensional multilayer film structure on the composite silicone rubber substrate, and then removing the pre-stretching force;

[0041] 5) evenly spin coating a solution for preparing a negative triboelectric layer on a glass plate, and heating and curing the solution to obtain a negative triboelectric layer film; removing the negative triboelectric layer film from the glass plate and pasting it onto the Ag NWs / LIG composite electrode;

[0042] 6) placing the cut fabric in an anhydrous ethanol solution for ultrasonic treatment, and drying the fabric after the ultrasonic treatment; placing the dried fabric as a positive triboelectric layer opposite to the negative triboelectric layer;

[0043] In step 5), the thickness of the negative triboelectric layer film is 1.5 to 2.5 mm, and the negative triboelectric layer film is a pure PDMS film, a PDMS / Ecoflex film or a MXene / silicone rubber composite film. When the MXene / silicone rubber composite film is used as the negative triboelectric layer, the output performance of the friction nanogenerator is optimal.

[0044] Furthermore, the fabric can be serge, corduroy, damask polyester cloth, polyester canvas, cotton and linen, nylon fabric, imitation silk, wool fabric, etc. When nylon fabric is used as the positive triboelectric layer, the open circuit voltage of the friction nanogenerator is the largest.

[0045] The working principle of the friction nanogenerator prepared by the above method is:

[0046] When in use, one end of the Ag NWs / LIG composite electrode is coated with a conductive coating and connected to an external load through a copper wire; the positive triboelectric material of the clothes or skin is in contact with the negative triboelectric layer of the generator, and the triboelectric nanogenerator is tapped at a certain frequency by hand or tool substitutes, so that the positive triboelectric layer and the negative triboelectric layer are frequently in contact and separation. Due to the coupling of frictional electricity and electrostatic induction, the generator can induce positive and negative charges, and transmit alternating current to the external load through the Ag NWs / LIG composite electrode, so that the generator has the ability to output electricity.

[0047] Example 1

[0048] In this embodiment, a pure PDMS film is used as a negative triboelectric layer to prepare a triboelectric nanogenerator based on a three-dimensional multilayer film structure composite electrode, including the following steps:

[0049] 1) A 60 μm thick polyimide (PI) film was pasted onto a glass plate using a hydrosol, and a laser was used to etch the polyimide film to obtain a laser-induced graphene (LIG) electrode with a size of 2×2 cm;

[0050] The laser source can be a continuous laser or a pulsed laser. The continuous laser has the characteristics of low power consumption, high universality and the ability to induce a highly porous structure. The pulsed laser is mainly used to induce high-resolution laser-induced graphene electrodes. The laser uses a CO2 laser. The working power of the carbon dioxide laser is 6.8W, the etching speed is 360mm / s, the density is 500PPI, and the vertical distance between the carbon dioxide laser etching grating and the polyimide film is 1.2mm.

[0051] 2) The polydimethylsiloxane base solution and the curing agent were magnetically stirred at a speed of 2000r / min for 2 minutes at a volume ratio of 10:1 to prepare 2.5ml polydimethylsiloxane (PDMS) solution; the A solution and the B solution were magnetically stirred at a speed of 2000r / min for 2 minutes at a volume ratio of 1:1 to prepare 0.5ml Ecolflex (aromatic random copolyester) solution; 0.5ml polydimethylsiloxane solution and Ecolflex solution were mixed at a volume ratio of 1:1, and magnetically stirred at a speed of 2000r / min for 2 minutes to obtain 1ml mixed silicone rubber solution; 1ml mixed silicone rubber solution and 2ml polydimethylsiloxane solution were placed in a vacuum box and evacuated for 15 minutes to remove bubbles in the solution;

[0052] The polydimethylsiloxane solution uses Dow Corning DC184 PDMS solution, and the Ecolflex solution uses EcoflexTM00-50 silicone rubber solution;

[0053] 3) Scrape 1 ml of the mixed silicone rubber solution from which bubbles have been removed onto the laser-induced graphene electrode of the polyimide film to a thickness of 1 mm, and vacuum treat in a vacuum drying oven for 30 min to allow the mixed silicone rubber solution to fill the porous structure of the laser-induced graphene electrode and remove excess air, and then dry at 80° C. for 2 h, cure the mixed silicone rubber solution, and form a composite silicone rubber substrate on a glass plate, and then transfer the laser-induced graphene electrode to the composite silicone rubber substrate, the composite silicone rubber substrate increasing the tensile properties of the laser-induced graphene electrode; soak the glass plate with the composite silicone rubber substrate in clean water for 24 h, remove the glass plate, and obtain a composite silicone rubber substrate;

[0054] 4) pre-stretching the composite silicone rubber substrate to a stretching length of about 30% of the original length, spraying a silver nanowire (Ag NWs) solution on the laser-induced graphene electrode in the pre-stretched state, forming a silver nanowire film on the laser-induced graphene electrode, and then forming an Ag NWs / LIG composite electrode with a three-dimensional multilayer film structure on the composite silicone rubber substrate, and then removing the pre-stretching force;

[0055] The concentration of the silver nanowire solution was 5 mg / ml, the solvent was anhydrous ethanol, and the spraying volume was 0.2 ml;

[0056] Spraying a layer of silver nanowire solution on the LIG electrode can significantly reduce the resistance of the electrode, thereby reducing the internal resistance of the triboelectric nanogenerator; In addition, spraying Ag NWs on the LIG electrode in a pre-stretched state is because the fracture gap of the LIG electrode will be further enlarged in the stretched state, allowing the silver nanowires to better combine with the LIG electrode, so that the silver nanowire conductive path is distributed in the fracture gap, thereby avoiding the adverse effects of stretching on the LIG electrode during use;

[0057] 5) Spin coating 2 ml of the polydimethylsiloxane solution from which bubbles were removed on a 4×4 cm glass plate at a spin coating speed of 250 rpm for 60 s; after spin coating, heat at 90° C. for 1 h to cure the polydimethylsiloxane solution to obtain a pure PDMS film, remove the pure PDMS film from the glass plate, and adhere the pure PDMS film as a negative triboelectric layer to the AgNWs / LIG composite electrode;

[0058] 6) Place the cut nylon fabric in a sample bottle containing anhydrous ethanol solution and ultrasonically treat it for 15 minutes. The ultrasonic treatment is used to sterilize and remove impurities. After the treatment, take out the nylon fabric and dry it in an oven to remove excess anhydrous ethanol solution. The drying temperature is 60°C and the drying time is 20 minutes. The dried nylon fabric is used as a positive triboelectric layer, facing the negative triboelectric layer, and the distance between the two is about 5 mm.

[0059] At this point, the preparation of the friction nanogenerator based on the three-dimensional multilayer film structure composite electrode has been completed.

[0060] Example 2

[0061] In this embodiment, a PDMS / Ecoflex film is used as a negative triboelectric layer to prepare a triboelectric nanogenerator based on a three-dimensional multilayer film structure composite electrode, including the following steps:

[0062] 1) A 60 μm thick polyimide film is pasted onto a glass plate using a hydrosol, and a CO2 laser is used to etch the polyimide film to obtain a laser-induced graphene electrode with a size of 2×2 cm;

[0063] 2) The polydimethylsiloxane base solution and the curing agent were magnetically stirred at a speed of 2000 r / min for 2 minutes in a volume ratio of 10:1 to prepare 1.5 ml of polydimethylsiloxane solution; the A solution and the B solution were magnetically stirred at a speed of 2000 r / min for 2 minutes in a volume ratio of 1:1 to prepare 1.5 ml of Ecolflex solution; 1.5 ml of polydimethylsiloxane solution and 1.5 ml of Ecolflex solution were magnetically stirred at a speed of 2000 r / min for 2 minutes to obtain 3 ml of mixed silicone rubber solution, and the mixed silicone rubber solution was placed in a vacuum box for evacuation for 15 minutes to remove bubbles in the solution;

[0064] 3) taking 1 ml of the mixed silicone rubber solution from which bubbles have been removed and applying it to the laser-induced graphene electrode of the polyimide film by scraping, vacuum treating it in a vacuum drying oven for 30 min, so that the mixed silicone rubber solution fills the porous structure of the laser-induced graphene electrode and removes excess air, and then drying it at 80° C. for 2 h, curing the mixed silicone rubber solution to form a composite silicone rubber substrate on a glass plate, and then transferring the laser-induced graphene electrode to the composite silicone rubber substrate; soaking the glass plate with the composite silicone rubber substrate in clean water for 24 h, removing the glass plate, and obtaining a composite silicone rubber substrate;

[0065] 4) pre-stretching the composite silicone rubber substrate to a stretching length of about 30% of the original length, spraying 0.2 ml of a silver nanowire (Ag NWs) solution with a concentration of 5 mg / ml on the laser-induced graphene electrode in the pre-stretched state, forming a silver nanowire film on the laser-induced graphene electrode, and then forming an AgNWs / LIG composite electrode with a three-dimensional multilayer film structure on the composite silicone rubber substrate, and then removing the pre-stretching force;

[0066] 5) Spin-coat the remaining 2 ml of the mixed silicone rubber solution on a 4×4 cm glass plate at a spin-coating speed of 250 rpm for 60 s; after spin-coating, heat at 90° C. for 1 h to solidify to obtain a PDMS / Ecoflex film, remove the PDMS / Ecoflex film from the glass plate, and adhere the PDMS / Ecoflex film as a negative triboelectric layer to the Ag NWs / LIG composite electrode;

[0067] 6) placing the cut nylon fabric into a sample bottle containing anhydrous ethanol solution and ultrasonically treating it for 15 minutes, taking out the nylon fabric after ultrasonic treatment, and drying it in an oven at a temperature of 60° C. for 20 minutes; using the dried nylon fabric as a positive triboelectric layer, facing the negative triboelectric layer, with a distance of about 5 mm between the two;

[0068] At this point, the preparation of the friction nanogenerator based on the three-dimensional multilayer film structure composite electrode has been completed.

[0069] Example 3

[0070] In this embodiment, a MXene / Silicone film is used as a negative triboelectric layer to prepare a triboelectric nanogenerator with a stretchable electrode, including the following steps:

[0071] 1) A 60 μm thick polyimide film is pasted onto a glass plate using a hydrosol, and a CO2 laser is used to etch the polyimide film to obtain a laser-induced graphene electrode with a size of 2×2 cm;

[0072] 2) The polydimethylsiloxane base solution and the curing agent were magnetically stirred at a speed of 2000 r / min for 2 minutes in a volume ratio of 10:1 to prepare 1.3 ml of polydimethylsiloxane; the A solution and the B solution were magnetically stirred at a speed of 2000 r / min for 2 minutes in a volume ratio of 1:1 to prepare 1.3 ml of Ecolflex solution; 1.3 ml of polydimethylsiloxane solution and 1.3 ml of Ecolflex solution were magnetically stirred at a speed of 2000 r / min for 2 minutes to obtain 2.6 ml of mixed silicone rubber solution, and the mixed silicone rubber solution was placed in a vacuum box for evacuation for 15 minutes to remove bubbles in the solution;

[0073] 3) taking 1 ml of the mixed silicone rubber solution from which bubbles have been removed and applying it to the laser-induced graphene electrode of the polyimide film by scraping, vacuum treating in a vacuum drying oven for 30 min, so that the mixed silicone rubber solution fills the porous structure of the laser-induced graphene electrode and removes excess air, and then drying at 80° C. for 2 h, curing the mixed silicone rubber solution to form a composite silicone rubber substrate on a glass plate, and then transferring the laser-induced graphene electrode to the composite silicone rubber substrate; soaking the glass plate with the composite silicone rubber substrate in clean water for 24 h, removing the glass plate, and obtaining a composite silicone rubber substrate;

[0074] 4) pre-stretching the composite silicone rubber substrate to a stretching length of about 30% of the original length, spraying 0.2 ml of a silver nanowire (Ag NWs) solution with a concentration of 5 mg / ml on the laser-induced graphene electrode in the pre-stretched state, forming a silver nanowire film on the laser-induced graphene electrode, and then forming an AgNWs / LIG composite electrode with a three-dimensional multilayer film structure on the composite silicone rubber substrate, and then removing the pre-stretching force;

[0075] 5) Take the remaining 1.6 ml of the mixed silicone rubber solution and 0.4 ml of the MXene solution with a concentration of 5 mg / ml, mix them and magnetically stir them at a speed of 1300 rpm for 30 min to obtain 2 ml of MXene / silicone rubber mixed solution; spin-coat 2 ml of the MXene / silicone rubber mixed solution on a glass plate with a size of 4×4 cm at a spin-coating speed of 250 rpm for 60 s; after spin-coating, heat at 90°C for 1 h to solidify to obtain a MXene / silicone rubber composite film, remove the MXene / silicone rubber composite film from the glass plate, and paste the MXene / silicone rubber composite film as a negative triboelectric layer onto the Ag NWs / LIG composite electrode;

[0076] 6) placing the cut nylon fabric into a sample bottle containing anhydrous ethanol solution and ultrasonically treating it for 15 minutes, taking out the nylon fabric after ultrasonic treatment, and drying it in an oven at a temperature of 60° C. for 20 minutes; using the dried nylon fabric as a positive triboelectric layer, facing the negative triboelectric layer, with a distance of about 5 mm between the two;

[0077] At this point, the preparation of the friction nanogenerator based on the three-dimensional multilayer film structure composite electrode has been completed.

[0078] Figure 3 (a) and (b) are SEM images of LIG electrode and Ag NWs / LIG composite electrode, respectively. It can be seen from the figures that laser-induced graphene is porous and the Ag NWs / LIG composite electrode is a three-dimensional multilayer film structure formed on the basis of silver nanowire layer and laser-induced graphene layer.

[0079] Figure 4 The square resistance of the laser-induced graphene before and after transfer and the Ag NWs / LIG composite electrode before and after pre-stretching is shown in the figure. The square resistance of the LIG electrode increases after transfer. This is because the mixed silicone rubber embedded in the LIG electrode blocks some of the conductive paths of the laser-induced graphene electrode during the transfer of the laser-induced graphene electrode to the composite silicone rubber substrate. Spraying silver nanowires on the LIG electrode in the non-pre-stretched state can greatly reduce the square resistance. This is because the silver nanowire film builds a new conductive path on the LIG electrode, which makes up for the defect of the conductive path being blocked during the transfer process of the LIG electrode. In order to make the composite electrode have good stretchability, the silver nanowires are sprayed on the LIG electrode in the pre-stretched state, and the square resistance is further reduced. This is because the LIG electrode is more tightly combined with the silver nanowires in the pre-stretched state, and a new conductive path will be formed at the junction of the LIG electrode and the silver nanowires, further reducing the square resistance.

[0080] Figures 5(a) to (c) show the open circuit voltage, short circuit current density, and transfer charge density of the friction nanogenerator with pure PDMS film, PDMS / Ecoflex film, and MXene / silicone rubber composite film as the negative friction electric layer, respectively. It can be observed from the figure that after the incorporation of Ecoflex into PDMS, the open circuit voltage, short circuit current density, and transfer charge density of the friction nanogenerator all increase. This is because the incorporation of Ecoflex increases the relative dielectric constant of PDMS. After further incorporation of MXene into the PDMS / Ecoflex solution, the output performance of the friction nanogenerator is further improved. This is because MXene is rich in -F functional groups, which can make the negative friction electric layer accumulate more friction charges, thereby enabling the friction nanogenerator to obtain a higher output.

[0081] Figure 6 The open circuit voltage diagram of the friction nanogenerator obtained with different fabric materials as the positive friction electric layer; it can be seen from the figure that when the positive friction electric layer is made of nylon fabric, the friction nanogenerator has the best open circuit voltage, that is, the open circuit voltage is the largest. On the one hand, this can be attributed to the fact that the positive friction electric layer is close to the positive end in the known friction electric series, which also determines that the positive friction electric layer is more likely to lose electrons when in contact with the negative friction electric material, which helps to improve the output performance of the friction nanogenerator. On the other hand, the microstructure of the nylon fabric increases the effective contact area when the positive friction electric layer contacts the negative friction electric material, which helps to accumulate friction charges and further improves the output performance of the generator.

[0082] Figure 7(a) shows the resistance change rate of the LIG electrode and the Ag NWs / LIG composite electrode under different tensile strains, and Figure 7(b) shows the resistance change rate of the Ag NWs / LIG composite electrode under different pre-stretching conditions; As can be seen from Figure 7(a), with the increase of tensile strain, the resistance change rate of the Ag NWs / LIG composite electrode is smaller than that of the LIG electrode, which is due to the formation of a silver nanowire film on the laser-induced graphene electrode after spraying the silver nanowires, making the Ag NWs / LIG composite electrode present a three-dimensional multilayer film structure. As can be seen from Figure 7(b), with the increase of tensile strain, the resistance change rate of the Ag NWs / LIG composite electrode becomes smaller and smaller, which is because the three-dimensional multilayer film structure of the Ag NWs and LIG electrodes becomes more complete with the increase of tensile strain.

[0083] Figure 8 This is the open circuit voltage of the friction nanogenerator prepared in Example 3 under different tensile strains. As the tensile strain increases, the open circuit voltage decays less and the generator can still maintain a stable output. Therefore, stretching has little effect on the output performance of the friction nanogenerator.

[0084] Fig. 9This is the open circuit voltage of the friction nanogenerator prepared in Example 3 after 10,000 working cycles. After the friction nanogenerator has worked for 10,000 times, it can still maintain a stable output.

[0085] Figure 10(a) shows the load current density and load voltage of the triboelectric nanogenerator prepared in Example 3 under different load resistances, and Figure 10(b) shows the power density of the triboelectric nanogenerator prepared in Example 3 under different load resistances. When the load resistance is 10 7 When Ω, the generator has the maximum power density.

[0086] Any matters not described in the present invention are applicable to the prior art.

Claims

1. A method for preparing a triboelectric nanogenerator based on a three-dimensional multilayer film structure composite electrode, wherein the triboelectric nanogenerator prepared by the method comprises a positive triboelectric layer, a negative triboelectric layer, an Ag NWs / LIG composite electrode and a composite silicone rubber substrate from top to bottom; characterized in that: The method comprises the following steps: 1) Laser etching the polyimide film to obtain a laser-induced graphene electrode; 2) Mixing a polydimethylsiloxane base solution and a curing agent in a volume ratio of 10:1 and performing magnetic stirring to prepare a polydimethylsiloxane solution; mixing solution A and solution B in a volume ratio of 1:1 and performing magnetic stirring to prepare an Ecolflex solution; mixing a polydimethylsiloxane solution and an Ecolflex solution in a volume ratio of 1:1 and performing magnetic stirring to obtain a mixed silicone rubber solution, and vacuuming the mixed silicone rubber solution to remove bubbles; wherein the Ecolflex solution is an aromatic random copolyester solution; 3) The mixed silicone rubber solution from which bubbles are removed is evenly scraped onto the laser-induced graphene electrode of the polyimide film, and then vacuum-treated in a vacuum drying oven, dried, and cured to obtain a composite silicone rubber substrate, at which point the laser-induced graphene electrode is transferred to the composite silicone rubber substrate; 4) pre-stretching the composite silicone rubber substrate, uniformly spraying a silver nanowire solution on the laser-induced graphene electrode in the pre-stretched state, forming a silver nanowire film on the laser-induced graphene electrode, and then forming a Ag NWs / LIG composite electrode with a three-dimensional multilayer film structure on the composite silicone rubber substrate, and then removing the pre-stretching force; 5) evenly spin coating a solution for preparing a negative triboelectric layer on a glass plate, and heating and curing the solution to obtain a negative triboelectric layer film; removing the negative triboelectric layer film from the glass plate and pasting it onto the Ag NWs / LIG composite electrode; 6) placing the cut fabric in an anhydrous ethanol solution for ultrasonic treatment, and drying the fabric after the ultrasonic treatment; placing the dried fabric as a positive triboelectric layer directly opposite to the negative triboelectric layer; In step 5), the negative triboelectric layer film is a pure PDMS film, a PDMS / Ecoflex film or a MXene / silicone rubber composite film. When the MXene / silicone rubber composite film is used as the negative triboelectric layer, the output performance of the friction nanogenerator is optimal.

2. The method for preparing a triboelectric nanogenerator based on a three-dimensional multilayer film structure composite electrode according to claim 1, characterized in that: In step 1), the etching power is 6.5-7.1 W, the etching speed is 348-372 mm / s, the density is 250-750 PPI, and the vertical distance between the etched grating and the polyimide film is 1.1-1.3 mm.

3. The method for preparing a triboelectric nanogenerator based on a three-dimensional multilayer film structure composite electrode according to claim 1, characterized in that: In step 5), 2 ml of the solution for preparing the negative triboelectric layer is spin-coated on a 4×4 cm glass plate at a spin-coating speed of 250 rpm for 60 s; after spin-coating, it is heated at 90° C. for 1 h to solidify to obtain a negative triboelectric layer film.

4. The method for preparing a triboelectric nanogenerator based on a three-dimensional multilayer film structure composite electrode according to claim 1, characterized in that: In step 5), the process of preparing the MXene / silicone rubber composite film is as follows: The mixed silicone rubber solution and the MXene solution were mixed in a volume ratio of 4:1 and magnetically stirred to obtain a MXene / silicone rubber mixed solution; the MXene / silicone rubber mixed solution was evenly spin-coated on a glass plate and heated and cured to obtain a MXene / silicone rubber composite film; the concentration of the MXene solution was 5 mg / ml, and the speed and time of the magnetic stirring were 1300 rpm and 30 min, respectively.

5. The method for preparing a triboelectric nanogenerator based on a three-dimensional multilayer film structure composite electrode according to claim 1, characterized in that: In step 6), the fabric is one of serge, corduroy, damask polyester cloth, polyester canvas, cotton and linen, nylon fabric, simulated silk or wool fabric; when nylon fabric is used as the positive friction electric layer, the open circuit voltage of the friction nanogenerator is the largest.

6. The method for preparing a triboelectric nanogenerator based on a three-dimensional multilayer film structure composite electrode according to claim 1, characterized in that: In step 2), the speed of magnetic stirring was 2000 r / min and the duration was 2 min.

7. The method for preparing a triboelectric nanogenerator based on a three-dimensional multilayer film structure composite electrode according to claim 1, characterized in that: In step 4), the concentration of the silver nanowire solution is 5 mg / ml, the solvent is anhydrous ethanol, and the spraying volume is 0.2 ml.

8. The method for preparing a triboelectric nanogenerator based on a three-dimensional multilayer film structure composite electrode according to claim 1, characterized in that: In step 5), the thickness of the negative triboelectric layer film is 1.5 to 2.5 mm.

Citation Information

Patent Citations

  • Stretchable friction nanogenerator in single electrode mode and preparation method thereof

    CN109889081A

  • Stretchable friction nano-power generator and preparation method thereof

    CN112260573A

  • Contact-friction-type nano-generator

    CN105099257A

  • Porous graphene / silver composite film for friction nano generator and preparation method thereof