Bioactive glass as a nucleic acid carrier with pH-switched controlled release
By developing a pH-switchable bioactive glass composition and combining bioactive glass particles with surface modifiers, the problem of low exogenous nucleic acid delivery efficiency is solved, achieving controlled release of nucleic acids and improving cell efficiency in a specific pH environment. Uptake rate, suitable for gene regulation and therapeutic applications.
Patent Information
- Application Number
- CN202080085508.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-12-09
- Filing Date
- 2020-12-09
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-12-09
AI Technical Summary
Existing technologies have problems of inefficiency when delivering exogenous nucleic acids into cells, especially due to insufficient stability and cellular uptake efficiency of nucleic acids, which limits their application in agriculture and therapeutic fields.
A pH-switchable bioactive glass composition was developed to improve the delivery efficiency of nucleic acids by capturing and controlling the release of nucleic acids in a designated pH environment, using bioactive glass particles combined with surface modifiers. These glass compositions contain components such as SiO2, CaO, P2O5, etc., and their cytophilicity is enhanced by surface modifiers such as polycationic compounds.
It achieves controlled release of nucleic acids within a specific pH range and increases the cellular uptake rate, enhances the delivery efficiency of nucleic acids, solves the problem of low delivery efficiency, and is suitable for the fields of gene regulation and therapy.
Smart Images

Figure CN114829313B_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority under 35 U.S.C. §119 to U.S. Provisional Application Serial No. 62 / 945,779, filed on December 9, 2019, which is hereby based upon and incorporated herein by reference in its entirety. Technical Field
[0003] The present disclosure relates to glass compositions for delivering nucleic acids into cells or microorganisms. In particular, the present disclosure relates to bioactive glass compositions capable of capturing and controlling the release of nucleic acids in a specified pH environment. Background Art
[0004] The use or transfer of exogenous nucleic acids for gene regulation or regulatory applications is an emerging market, especially in the agricultural and therapeutic fields. The ability of small interfering RNA (siRNA) to regulate gene expression has potential therapeutic applications, but its use is limited by inefficient delivery. Specifically, due to the stability of nucleic acids and cellular uptake efficiency, the delivery of exogenous nucleic acids into target organisms or cells remains challenging. Therefore, there is a strong need to develop new glass compositions with improved surface properties that can act as nucleic acid carriers to enhance cellular uptake rates. Summary of the invention
[0005] According to a first aspect, a pH-switchable carrier composition comprises a plurality of bioactive glass particles, wherein each bioactive glass particle is optionally at least partially coated with a surface modifier. In certain embodiments, the bioactive glass particles (with or without a surface modifier) can bind to a nucleic acid compound upon contact within a pH range of about 7 to about 11, and exhibit controlled release of the nucleic acid compound within a pH range of about 5 to about 6. In certain embodiments, the bioactive glass particles comprise, by weight percent of oxides, about 30% to about 75% SiO2, about 2% to about 40% CaO, and about 3% to about 15% P2O5. In certain embodiments, the bioactive glass particles comprising about 75% SiO2, about 2% to about 40% CaO, and about 3% to about 15% P2O5, further comprise, by weight % of oxides: about 0% to about 5% B2O3; about 0% to about 5% Al2O3; about 0% to about 20% MgO; about 0% to about 10% ZrO2; about 0% to about 5% F; and about 0% to about 30% R2O, wherein the R2O comprises about 0% to about 10% K2O and about 0% to about 30% Na2O.
[0006] In certain embodiments, the bioactive glass particles consist essentially of, by weight percent of oxides: about 30% to about 70% B2O3, about 5% to about 25% CaO, and about 1% to about 10% P2O5. In certain embodiments, the bioactive glass particles comprising about 30% to about 70% B2O3, about 5% to about 25% CaO, and about 1% to about 10% P2O5, by weight percent of oxides, further comprise: about 0% to about 5% SiO2; about 0% to about 15% Al2O3; about 0% to about 10% MgO; about 0% to about 10% ZrO2; about 0% to about 5% F; and about 0% to about 20% R2O, wherein R2O comprises about 0% to about 20% K2O and about 0% to about 10% Na2O.
[0007] In some embodiments, the bioactive glass particles include calcium phosphate glass. In some embodiments, the bioactive glass particles are at least partially coated with a surface modifier, and the surface modifier includes a polycationic compound. In some embodiments, the polycationic compound is selected from the group consisting of polyamines, polylysine, polyarginine, polyornithine, polyalkylenimine, chitosan, polyalkylaminoalkyl methacrylate, and derivatives thereof, or any combination thereof. In some embodiments, the polycationic compound is selected from the group consisting of polyethyleneimine, shrimp chitosan, low molecular weight chitosan, and derivatives thereof. In some embodiments, the molecular weight of the low molecular weight chitosan or derivative is from about 50 kDa to about 375 kDa.
[0008] In certain embodiments, wherein the nucleic acid compound is selected from the group consisting of a ribonucleic acid compound, a deoxyribonucleic acid compound, or a derivative thereof. In certain embodiments, the particle size of the bioactive glass particles is about 1 μm to about 10 μm. In certain embodiments, the particle size of the bioactive glass particles is about 1 μm to about 5 μm. In certain embodiments, under neutral conditions, the zeta potential of the unmodified bioactive glass particles is about -10 mV to about -40 mV. In certain embodiments, under neutral conditions, the zeta potential of the surface-modified bioactive glass particles is about 0 mV to about -20 mV. In certain embodiments, the concentration range of the nucleic acid is about 5 ng / mg to about 10 μg / mg of the total weight of the carrier composition.
[0009] According to a second aspect, bioactive glass particles are optionally at least partially coated with a surface modifier; wherein the bioactive glass particles (with or without the surface modifier) can bind to a nucleic acid compound upon contact within a pH range of about 7 to about 11 and exhibit controlled release of the nucleic acid compound within a pH range of about 5 to about 6; and wherein, based on weight percent of oxides, the bioactive glass particles consist essentially of: (a) about 30% to about 75% SiO2, about 2% to about 40% CaO, and about 3% to about 15% P2O5, or (b) about 30% to about 70% B2O3, about 5% to about 25% CaO, and about 1% to about 10% P2O5.
[0010] According to a third aspect, a method for making a bioactive glass carrier comprises: processing bioactive glass into fine particles; mixing the fine particles of bioactive glass with a liquid medium to form a solution; optionally modifying the surface of the bioactive glass particles by a surface modifier in the solution, contacting the bioactive glass particles with a nucleic acid compound in the liquid medium to form an admixture; and culturing the admixture under conditions where the nucleic acid compound is non-covalently bound to the bioactive glass particles. In certain embodiments, the method comprises modifying the surface of the bioactive glass particles by culturing the bioactive glass particles with a surface modifier. In certain embodiments, the surface modifier comprises a polycationic compound. In certain embodiments, the culturing of the bioactive glass particles with the surface modifier is performed at a temperature of about ambient temperature to about 65° C. In certain embodiments, the culturing of the bioactive glass particles with the surface modifier lasts for a period of about 8 to 24 hours.
[0011] In certain embodiments of the third aspect, the method further comprises: contacting the surface-modified bioactive glass particles with the nucleic acid compound in a liquid medium to form a mixture; and incubating the mixture under conditions where the nucleic acid compound is non-covalently bound to the surface-modified bioactive glass particles. In certain embodiments, the incubation of the surface-modified bioactive glass particles with the nucleic acid is performed at room temperature. In certain embodiments, the incubation of the surface-modified bioactive glass particles with the nucleic acid is performed for a period of about 15 minutes to 2 hours. In certain embodiments of the method, the liquid medium is selected from the group consisting of water, an alcohol, or a hydrocarbon.
[0012] In certain embodiments of the method of the third aspect, the bioactive glass particles consist essentially of, by weight percent of oxides: about 30% to about 75% SiO2, about 2% to about 40% CaO, and about 3% to about 15% P2O5. In certain embodiments, the bioactive glass particles comprising about 75% SiO2, about 2% to about 40% CaO, and about 3% to about 15% P2O5, by weight percent of oxides, further comprise: about 0% to about 5% B2O3; about 0% to about 5% Al2O3; about 0% to about 20% MgO; about 0% to about 10% ZrO2; about 0% to about 5% F; and about 0% to about 30% R2O, wherein the R2O comprises about 0% to about 10% K2O and about 0% to about 30% Na2O.
[0013] In certain embodiments of the method of the third aspect, the bioactive glass particles consist essentially of, by weight percent of oxides: about 30% to about 70% B2O3, about 5% to about 25% CaO, and about 1% to about 10% P2O5. In certain embodiments, the bioactive glass particles comprising about 30% to about 70% B2O3, about 5% to about 25% CaO, and about 1% to about 10% P2O5, by weight percent of oxides, further comprise: about 0% to about 5% SiO2; about 0% to about 15% Al2O3; about 0% to about 10% MgO; about 0% to about 10% ZrO2; about 0% to about 5% F; and about 0% to about 20% R2O, wherein the R2O comprises about 0% to about 20% K2O and about 0% to about 10% Na2O.
[0014] According to a fourth aspect, a carrier comprises a pH-switchable carrier composition according to the first aspect. In certain embodiments, the composition comprises a plurality of bioactive glass particles, wherein each bioactive glass particle is optionally at least partially coated with a surface modifier. In certain embodiments, the bioactive glass particles (with or without a surface modifier) can be bonded to a nucleic acid compound after contact in a pH range of about 7 to about 11, and exhibit controlled release of the nucleic acid compound in a pH range of about 5 to about 6. In certain embodiments, the carrier comprises: a drug delivery carrier, a gene delivery carrier, a tissue regeneration carrier, a crop treatment or crop protection, an immunomodulatory carrier, or a gene editing composite carrier. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 Shown is an X-ray diffraction (XRD) pattern of bioactive glass particles according to one or more embodiments shown and described herein.
[0016] Figure 2 Shown is a graph of particle size distribution of an exemplary bioactive glass composition according to one or more embodiments presented and described herein.
[0017] Figure 3 Shown are SEM images of carrier compositions and surface-modified bioactive glass particles according to one or more embodiments shown and described herein.
[0018] Figure 4 The bar graph of shows the DLS particle size distribution of bioactive glass particles according to one or more embodiments shown and described herein.
[0019] Figure 5A and 5B The net surface charge characteristics of bioactive glass in aqueous solution over a pH range of 4 to 12 are shown according to one or more embodiments shown and described herein.
[0020] Figure 6 DNA loading and elution rates are shown for various bioactive glass compositions according to one or more embodiments shown and described herein.
[0021] Figures 7A-7D Various bioactive glass compositions according to one or more embodiments shown and described herein are shown by using improved The lysis kinetics were obtained from the cumulative calcium concentration measured by the calcium cell assay. DETAILED DESCRIPTION
[0022] Reference will now be made in detail to various embodiments, which are illustrated in the accompanying drawings. Whenever possible, the same reference numerals are used in the drawings to represent the same or similar parts. The components in the drawings are not necessarily to scale, but rather, emphasis is placed on illustrating the principles of the exemplary embodiments.
[0023] As discussed above, the present technology generally relates to glass compositions and methods for delivering desired materials (e.g., nucleic acids) into cells and tissues. In various embodiments, the compositions and systems provided herein include bioactive glass particles and methods of making and using the same that can be used to deliver therapeutic agents to cells or tissues of plants, animals, and insects.
[0024] The following provides definitions of certain terms used in this specification. Unless otherwise defined, all technical and scientific terms used herein generally have the meaning commonly understood by one of ordinary skill in the art to which this technology belongs.
[0025] As used in the specification and claims, the singular forms "a", "an", and "the" include plural referents unless the context clearly dictates otherwise. Thus, for example, reference to "a" component includes aspects having two or more such components unless the context clearly dictates otherwise. For example, reference to "a cell" includes combinations of two or more cells, and so forth. In addition, use of the word "or" when not preceded by the antecedent "either" (or when other similar terms indicating "or" are explicitly exclusive, e.g., only one of x or y) should be read as inclusive (e.g., "x or y" means one or both of x or y). In general, the nomenclature used herein and the cell culture, molecular genetics, organic chemistry, analytical chemistry, and nucleic acid chemistry described below are those well known and commonly used in the art.
[0026] The term "and / or" should also be interpreted as inclusive (e.g., "x and / or y" means one or both of x or y). Where "and / or" or "or" is used in connection with a group of three or more items, the group should be understood to include only one item, all items together, or any combination or number of items. In addition, terms such as: having, having, including, and including used in the specification and claims should be interpreted as having the same meaning as the terms including and comprising. With the "and / or" clause, other elements may optionally be present in addition to the specifically specified elements, whether or not they are related or unrelated to those specifically specified elements. As non-limiting examples, reference to "X and / or Y" may refer to only X (optionally including elements other than Y) in one embodiment; may refer to only Y (optionally including elements other than X) in some embodiments; and may refer to both X and Y (optionally including other elements) in some embodiments.
[0027] Unless otherwise indicated or the context warrants otherwise, as used herein, the term "about" in reference to a number is generally considered to include numbers within 1%, 5% or 10% in either direction (greater or less than) of that number (excluding the possibility that such a number would be less than 0% or greater than 100%).
[0028] Unless otherwise indicated, as used herein, the term "particle size" refers to the diameter of the particle. Particle size is expressed, for example, as peak particle size, which represents the hydrodynamic diameter of the particles obtained by dynamic light scattering (DLS) techniques, or as median or average particle size.
[0029] As used herein, the term "bioactive glass (BAG)" or "bioactive glass" refers to an inorganic glass material having silicon oxide or boron oxide as its main component and which is capable of bonding with desired biological materials (e.g., nucleic acids, cells and tissues).
[0030] As used herein, the term "adjustable" or "switchable" refers to a bioactive glass support that changes its behavior in response to an environmental stimulus. For example, a pH-switchable support would demonstrate switchable behavior based on pH, wherein the support is able to bind nucleic acids at a specific pH and elute the nucleic acids at another pH.
[0031] As used herein, the term "controlled release" refers to the release of nucleic acids from nanoparticles according to a predetermined profile. In some aspects, the selected controlled release may include the release of nucleic acid compounds within a specific pH range.
[0032] composition
[0033] Various aspects and / or embodiments of the present disclosure relate to compositions comprising bioactive glass. In various embodiments, provided herein are pH switchable carrier compositions comprising bioactive glass particles, wherein the carrier can demonstrate switchable behavior based on pH. The carrier can bind to nucleic acids at a specific pH and elute the nucleic acids at another pH. The compositions disclosed herein exhibit excellent biocompatibility. The bioactive properties of glass arise from a series of complex physicochemical reactions on the glass surface under physiological conditions. For example, when glass is exposed to body fluids in animals or insects, cation exchange may occur, whereby cations from the glass surface are replaced by protons from the solution. The interfacial pH becomes more alkaline and due to the network dissolution occurring on the glass surface accompanied by Ca 2+ and PO4 3- Ions are released into solution. This promotes the formation of brushite (CaHPO4·2H2O), a known bioactive ceramic, or hydroxyapatite (HCA), which can bind to interfacial metabolites, collagen and glycoproteins. As a result, bioactive glasses have found medical applications, such as in orthopedics and dentistry. The present technology aims to provide bioactive glasses with enhanced bioactivity.
[0034] In one aspect, provided herein are pH-switchable carrier compositions comprising bioactive glass particles, wherein the bioactive glass particles are optionally at least partially coated with a surface modifier, and wherein the bioactive glass particles (with or without the surface modifier) can bind to a nucleic acid compound upon contact within a pH range of about 7 to about 11, and exhibit controlled release of the nucleic acid compound within a pH range of about 5 to about 6.
[0035] The bioactive glass of the carrier composition can be formed from a precursor glass composition from the silicate and borate families, which exhibits excellent nucleic acid capture / release efficiency under different pH environments. Suitable glass precursor materials for this technology include, but are not limited to, the following oxides: silicon, boron, phosphorus, potassium, sodium, calcium, lithium, aluminum, magnesium, zirconium, rubidium, cesium, strontium, barium, chromium, titanium, tungsten, iron and zinc. The glass may additionally contain halides (e.g., fluorides). The biocompatibility and decomposition of the composition are affected by the composition of the bioactive glass. In various embodiments, the bioactive glass particles may include calcium phosphate glass.
[0036] In various embodiments, the precursor glass composition for bioactive glass includes SiO2. When the content of SiO2 is too low, the glass may have poor chemical durability and mechanical durability. On the other hand, when the content of SiO2 is too high, the melting ability of the glass decreases because the melting temperature of pure SiO2 is too high. As the SiO2 content increases, the bioactivity of the glass decreases. In certain embodiments, the precursor glass composition for bioactive glass may include silicate glass, which includes SiO2 as the main oxide forming glass. In various embodiments of silicate glass, the amount of SiO2 present in the precursor glass composition is about 30% by weight to about 75% by weight, such as about 35% by weight to about 70% by weight of the total weight of the precursor glass composition, about 40% by weight to about 65% by weight, about 45% by weight to about 60% by weight, about 50% by weight to about 55% by weight, or any range including any two of these values and / or any two of these values.
[0037] In certain embodiments, the silicate glass composition comprises from about 0 wt. % B2O3 to about 5 wt. % B2O3, such as from about 0.2 wt. % to about 4.5 wt. %, from about 0.5 wt. % to about 4 wt. %, from about 1 wt. % to about 3.5 wt. %, from about 1.5 wt. % to about 3 wt. %, or from about 2 wt. % to about 2.5 wt. % B2O3, based on the total weight of the precursor glass composition, or including any two of these values and / or any range between any two of these values.
[0038] In certain embodiments, a precursor glass composition for a bioactive glass may include a borate glass comprising B2O3 as the primary glass-forming oxide. Borate glass is far less durable than silicate glass, which makes it attractive for rapid degradation. In various embodiments of the borate glass, the amount of B2O3 present in the precursor glass composition is from about 30 wt % to about 70 wt %, such as from about 35 wt % to about 65 wt %, from about 40 wt % to about 60 wt %, from about 45 wt % to about 55 wt %, from about 50 wt % to about 55 wt %, or any range including any two of these values and / or any range between any two of these values.
[0039] In certain embodiments, the borate glass composition comprises from about 0 wt % SiO2 to about 5 wt % SiO2, e.g., from about 0.2 wt % to about 4.5 wt %, from about 0.5 wt % to about 4 wt %, from about 1 wt % to about 3.5 wt %, from about 1.5 wt % to about 3 wt %, or from about 2 wt % to about 2.5 wt % SiO2, based on the total weight of the precursor glass composition, or including any two of these values and / or any range between any two of these values.
[0040] In another aspect, bioactive glass particles are provided, optionally at least partially coated with a surface modifier; wherein the bioactive glass particles (with or without the surface modifier) can bind to a nucleic acid compound upon contact within a pH range of about 7 to about 11, and exhibit controlled release of the nucleic acid compound within a pH range of about 5 to about 6; and wherein, based on weight percent of oxides, the bioactive glass particles consist essentially of: (a) about 30% to about 75% SiO2, about 2% to about 40% CaO, and about 3% to about 15% P2O5, or (b) about 30% to about 70% B2O3, about 5% to about 25% CaO, and about 1% to about 10% P2O5.
[0041] In another aspect, bioactive glass particles are provided, optionally at least partially coated with a surface modifier; wherein the bioactive glass particles (with or without the surface modifier) can bind to a nucleic acid compound upon contact within a pH range of about 7 to about 11, and exhibit controlled release of the nucleic acid compound within a pH range of about 5 to about 6; and wherein, based on weight percent of oxides, the bioactive glass particles consist essentially of: (a) about 30% to about 75% SiO2, about 2% to about 40% CaO, and about 3% to about 15% P2O5, or (b) about 30% to about 70% B2O3, about 5% to about 25% CaO, and about 1% to about 10% P2O5.
[0042] Precursor glass compositions for bioactive glass may also include P2O5, which acts as a network former. In addition, phosphate ions are released to the surface of the bioactive glass to contribute to the formation of Ca-P compounds (e.g., brushite or apatite). Providing phosphate ions by bioactive glass increases the rate of mineral formation and the binding capacity of bone tissue. In addition, P2O5 increases the viscosity of the glass, which in turn expands the operating temperature range, and is therefore advantageous for manufacturing and forming glass. In various embodiments, the amount of P2O5 present in the precursor glass composition is about 0% by weight to about 20% by weight of the gross weight of the precursor glass composition, including about 1% by weight to about 10% by weight and about 3% by weight to about 15% by weight of P2O5, based on the gross weight of the precursor glass composition. In certain embodiments, the silicate glass composition comprises from about 3 wt % to about 15 wt % P2O5, such as from about 4 wt % to about 14 wt %, from about 5 wt % to about 13 wt %, from about 6 wt % to about 12 wt %, from about 7 wt % to about 11 wt %, or from about 8 wt % to about 10 wt % P2O5, or any two of these values and / or any range between any two of these values, based on the total weight of the precursor glass composition. In certain embodiments, the borate glass composition comprises from about 1 wt % to about 10 wt %, such as from about 2 wt % to about 9 wt %, from about 3 wt % to about 8 wt %, from about 4 wt % to about 7 wt %, or from about 5 wt % to about 6 wt % P2O5, or any two of these values and / or any range between any two of these values, based on the total weight of the precursor glass composition.
[0043] The precursor glass composition for the bioactive glass may also include Al2O3 and ZrO2, which help improve chemical durability in the borate glass without toxicity issues. In various embodiments, the amount of Al2O3 present in the precursor glass composition for the bioactive glass is about 0 wt% to about 20 wt% of the total weight of the precursor glass composition, including about 0 wt% to about 5 wt% and about 0.1 wt% to about 15 wt% Al2O3, based on the total weight of the precursor glass composition. In certain embodiments, the silicate glass composition includes about 0 wt% Al2O3 to about 5 wt% Al2O3, such as about 0.2 wt% to about 4.5 wt%, about 0.5 wt% to about 4 wt%, about 1 wt% to about 3.5 wt%, about 1.5 wt% to about 3 wt%, or about 2 wt% to about 2.5 wt% Al2O3, or any two of these values and / or any range between any two of these values. In certain embodiments, the borate glass composition comprises about 0.1 wt % to about 15 wt % Al2O3, such as about 0.5 wt % to about 12 wt %, about 1 wt % to about 10 wt %, about 3 wt % to about 8 wt %, or about 5 wt % to about 7 wt % Al2O3, based on the total weight of the precursor glass composition, or including any two of these values and / or any range between any two of these values.
[0044] In various embodiments, the amount of ZrO2 present in the precursor glass composition (both silicate and borate cases) is from about 0 wt% ZrO2 to about 10 wt% ZrO2 (based on the total weight of the precursor glass composition), such as from about 2 wt% to about 9 wt%, from about 3 wt% to about 8 wt%, from about 4 wt% to about 7 wt%, or from about 5 wt% to about 6 wt% ZrO2, based on the total weight of the precursor glass composition, or any range including any two of these values and / or between any two of these values.
[0045] Precursor glass compositions for bioactive glasses may also include alkaline oxides (Li2O, Na2O, K2O, Rb2O, and Cs2O), which act as additives for achieving low melting temperatures and low liquidus temperatures and improve bioactivity. In various embodiments, the amount of Na2O present in the precursor glass composition for bioactive glass is from about 0 wt% to about 35 wt% of the total weight of the precursor glass composition, including from about 0 wt% to about 30 wt% Na2O and from about 0 wt% to about 10 wt% Na2O, based on the total weight of the precursor glass composition. In certain embodiments, the silicate glass composition includes from about 0 wt% Na2O to about 30 wt% Na2O, such as from about 2 wt% to about 25 wt%, from about 5 wt% to about 20 wt%, from about 7 wt% to about 15 wt%, from about 8 wt% to about 12 wt%, or from about 9 wt% to about 10 wt% Na2O, of the total weight of the precursor glass composition, or including any two of these values and / or any range between any two of these values. In certain embodiments, the borate glass composition includes about 0 wt % Na2O to about 10 wt % Na2O, such as about 0.5 wt % to about 9 wt %, about 1 wt % to about 8 wt %, about 2 wt % to about 7 wt %, or about 5 wt % to about 6 wt % Na2O, based on the total weight of the precursor glass composition, or including any two of these values and / or any range between any two of these values.
[0046] In various embodiments, the amount of K2O present in the precursor glass composition for the bioactive glass is from about 0 wt% to about 25 wt% of the total weight of the precursor glass composition, including from about 0 wt% to about 10 wt% K2O and from about 0 wt% to about 20 wt% K2O, based on the total weight of the precursor glass composition. In certain embodiments, the silicate glass composition comprises from about 0 wt% to about 10 wt% K2O, such as from about 0.5 wt% to about 9 wt%, from about 1 wt% to about 8 wt%, from about 2 wt% to about 7 wt%, or from about 5 wt% to about 6 wt% K2O, based on the total weight of the precursor glass composition, or including any two of these values and / or any range between any two of these values. In certain embodiments, the borate glass composition comprises 0 wt % K2O to about 20 wt % K2O, e.g., about 2 wt % to about 18 wt %, about 5 wt % to about 15 wt %, about 6 wt % to about 12 wt %, or about 8 wt % to about 10 wt % K2O, based on the total weight of the precursor glass composition, or including any two of these values and / or any range between any two of these values.
[0047] In various embodiments, the precursor glass composition for bioactive glass can include divalent cation oxides (e.g., alkaline earth oxides), which improve the melting behavior and bioactivity of the glass. It was found that CaO can react with P2O5 to form apatite when immersed in simulated body fluid (SBF) or in vivo. The Ca released from the glass surface 2+ The ions contribute to the formation of a layer enriched with calcium phosphate. In various embodiments, the amount of CaO present in the precursor glass composition for the bioactive glass is from about 0 wt % to about 50 wt %, including from about 2 wt % to about 40 wt % and from about 5 wt % to about 25 wt % CaO, based on the total weight of the precursor glass composition. In certain embodiments, the silicate glass composition comprises from about 2 wt % CaO to about 40 wt % CaO, such as from about 5 wt % to about 35 wt %, from about 10 wt % to about 30 wt %, from about 15 wt % to about 25 wt %, or from about 18 wt % to about 22 wt % CaO, or any two of these values and / or any range between any two of these values. In certain embodiments, the borate glass composition includes 5 wt % CaO to about 25 wt % CaO, such as about 7 wt % to about 22 wt %, about 10 wt % to about 20 wt %, about 12 wt % to about 18 wt %, or about 15 wt % to about 18 wt % CaO, based on the total weight of the precursor glass composition, or including any two of these values and / or any range between any two of these values.
[0048] In various embodiments, the amount of MgO present in the precursor glass composition is from about 0 wt % to about 25 wt %, including from about 0 wt % to about 20 wt % and from about 0 wt % to about 10 wt % MgO, based on the total weight of the precursor glass composition. In certain embodiments, the silicate glass composition includes from about 0 wt % MgO to about 10 wt % MgO, such as from about 0.5 wt % to about 9 wt %, from about 1 wt % to about 8 wt %, from about 2 wt % to about 7 wt %, from about 3 wt % to about 6 wt %, or from about 4 wt % to about 5 wt % MgO, based on the total weight of the precursor glass composition, or including any two of these values and / or any range between any two of these values. In certain embodiments, the borate glass composition includes 0 wt % MgO to about 20 wt % MgO, such as about 0.5 wt % to about 18 wt %, about 1 wt % to about 15 wt %, about 3 wt % to about 10 wt %, or about 5 wt % to about 8 wt % MgO, based on the total weight of the precursor glass composition, or including any two of these values and / or any range between any two of these values.
[0049] The glass composition may also optionally include a small amount of fluoride. In certain embodiments, the precursor glass composition (both silicate and borate) includes from about 0 wt % F to about 5 wt % F, such as from about 0.2 wt % F to about 4.5 wt % F, from about 0.5 wt % F to about 4 wt % F, from about 1 wt % F to about 3.5 wt % F, from about 1.5 wt % F to about 3 wt % F, or from about 2 wt % F to about 2.5 wt % F, or any two of these values and / or any range between any two of these values, based on the total weight of the precursor glass composition.
[0050] In various embodiments, the bioactive glass particles primarily comprise, by weight percent of oxides: about 30% to about 75% SiO2, about 2% to about 40% CaO, and about 3% to about 15% P2O5. In such embodiments, the bioactive glass particles further comprise, by weight percent of oxides: about 0% to about 5% B2O3; about 0% to about 5% Al2O3; about 0% to about 20% MgO; about 0% to about 10% ZrO2; about 0% to about 5% F; and about 0% to about 30% R2O, wherein R2O comprises about 0% to about 10% K2O and about 0% to about 30% Na2O.
[0051] In various embodiments, the bioactive glass particles primarily comprise, by weight percent of oxides: about 30% to about 70% B2O3, about 5% to about 25% CaO, and about 1% to about 10% P2O5. In such embodiments, the bioactive glass particles further comprise, by weight percent of oxides: about 0% to about 5% SiO2; about 0% to about 15% Al2O3; about 0% to about 10% MgO; about 0% to about 10% ZrO2; about 0% to about 5% F; and about 0% to about 20% R2O, wherein R2O comprises about 0% to about 20% K2O and about 0% to about 10% Na2O.
[0052] In weight percent, an exemplary silicate glass composition may include:
[0053] 30 to 75% SiO2,
[0054] 3 to 15% P2O5,
[0055] 0 to 5% B2O3,
[0056] 0 to 5% Al2O3,
[0057] 0 to 30% Na2O,
[0058] 0 to 10% K2O,
[0059] 0-20% MgO,
[0060] 2-40% CaO,
[0061] 0-10% ZrO2,
[0062] 0-5%F.
[0063] In weight percent, an exemplary borate glass composition may include:
[0064] 0 to 5% SiO2,
[0065] 30 to 70% B2O3,
[0066] 1 to 10% P2O5,
[0067] 0.1 to 15% Al2O3,
[0068] 0 to 10% Na2O,
[0069] 0 to 20% K2O,
[0070] 0-10% MgO,
[0071] 5-25% CaO,
[0072] 0-10% ZrO2,
[0073] 0-5%F.
[0074] In some embodiments, the bioactive glass can be ground into fine particles of 1-10 μm by air jet milling. Using friction grinding or ball milling of glass frit, the particle size will vary in the range of 1-100 μm. In addition, these glasses can be subsequently processed to submicron level by different methods (e.g., planetary ball milling or wet milling). Complex compositions are possible, but are not easily achieved by bottom-up processes (e.g., sol-gel forming). Another effective method for producing bioactive glass particles with precise size control is to use a microreactor, such as Corning Advanced Flow Reactor. For industrial scale, glass particles of desired size can be produced by top-down melting scheme after milling or grinding, which provides flexibility in composition design and low-cost manufacturing. In some embodiments, bioactive glass can be ground into fine particles by air jet, ball milling or grinding. Glass particles of desired size can be used as is or can be integrated into a polymer matrix, depending on the target application.
[0075] Bioactive glass particles can be bonded to nucleic acid compounds under various pH conditions. Nucleic acids can be coated on or located on the surface of bioactive glass particles. Suitable nucleic acids include any ribonucleic acid (RNA) or deoxyribonucleic acid (DNA), which can be modified or unmodified. In various embodiments, nucleic acids include, but are not limited to: single-stranded or double-stranded RNA, single-stranded or double-stranded DNA, RNA with a mixture of single-stranded and double-stranded regions, DNA with a mixture of single-stranded and double-stranded regions, mixed molecules containing DNA and RNA (which can be single-stranded, or more generally double-stranded, or a mixture of single-stranded and double-stranded regions). In addition, nucleic acids involve triple-stranded regions containing RNA or DNA or both, DNA or RNA containing one or more modified bases, and DNA or RNA with modified backbones for stability or other reasons. In some embodiments, nucleic acids include ribonucleic acid, deoxyribonucleic acid, or derivatives thereof. In some embodiments, nucleic acids include ribonucleic acid or derivatives thereof. In other embodiments, nucleic acids include deoxyribonucleic acid or derivatives thereof. In some embodiments, nucleic acids include interfering ribonucleic acid molecules.
[0076] In various embodiments, the bioactive glass particles are at least partially coated with a surface modifier. In various embodiments, the surface modifier may include a compound or composition that facilitates delivery of nucleic acids to cells. For example, the surface modifier may include a cationic compound, which is a compound having polar groups that are positively charged at or near physiological pH. Exemplary cationic compounds include, but are not limited to, polycations, cationic lipids, cationic polymers, or mixtures thereof. In various embodiments, the surface modifier includes a polycationic compound. The polycation to be used as a surface modifier may be a synthetic polymer, a naturally occurring polymer, or a chemically modified naturally occurring polymer. The polycation suitably has a plurality of positively charged groups at a pH of 5 to 11. The charged groups may be selected from: alkylamines (including primary amines, secondary amines, tertiary amines, and quaternary ammoniums), imines, guanidines, and aromatic amines. Suitable polycations include, but are not limited to, polyamines, polylysine, polyarginine, polyornithine, polyalkyleneimines, chitosan, oligopeptides, cationized polysaccharides, cationized plant proteins or cationized animal proteins, protamine, activated dendrimers, diethylaminoethyl dextran, polyamidoamines, poly(β-amino esters), aminopolysaccharide polypropyleneimine, polyallylamine, homopolymers or copolymers of polyvinylamine, poly(vinylpyridine), homopolymers or copolymers, homopolymers or copolymers of poly(meth)acrylates, homopolymers or copolymers of poly(meth)acrylamides, and derivatives thereof, cationic compounds including peptides and protein fragments or combinations thereof, or combinations thereof. Examples of preferred n are: polyethyleneimine (PEI), Hexadimethrine bromide (available under the trade name polybrene), polyhexamethyleneguanidine (PHMG), polyhexamethylenebiguanide, polyallylamine, guanidinized poly(allylamine), polyaminopropylmethacrylamide, poly-[N-(3-guanidinyl)methacrylamide], polyaminoethyl(meth)acrylate, polydimethylaminoethylmethacrylate (PDMAEMA). In various embodiments, the polycationic compound is selected from the group consisting of polyamines, polylysine, polyarginine, polyornithine, polyalkylenimine, chitosan, polyalkylaminoalkylmethacrylate, and derivatives thereof, or any combination thereof. Chitosan may include low molecular weight chitosan, high molecular weight chitosan, or chitosan obtained from crustacean shells (e.g., shrimp). In various embodiments, the polycation includes polyethyleneimine (PEI). In various embodiments, the polycation includes low molecular weight chitosan. In various embodiments, the polycation includes shrimp chitosan. In various embodiments, the polycationic compound is selected from the group consisting of polyethyleneimine, shrimp chitosan, low molecular weight chitosan, and derivatives thereof.
[0077] Polycations can be side chains and / or straight chains. For example, in the case of PEI, straight chain polyethyleneimine contains all secondary amines, which is different from side chain PEI containing primary amine, secondary amine and tertiary amino groups. It is speculated that these compounds help to deliver nucleic acids into cells because they can neutralize the charge of nucleic acids. For some applications, net cationic charge is maintained under alkaline conditions. As a result, nucleic acids remain combined with polycations, which provides some protection from nuclease degradation (known polycation / nucleic acid complexes show better stability than uncomplexed forms). Polycations can contain one or more types of amino groups containing different pKa values. Polycations can be homopolymers or copolymers. When the positively charged polymer is a copolymer, the comonomer to be copolymerized with the monomer containing the charged amino group is selected to maintain the sufficient water solubility level of the copolymer. Other water-soluble polycations can be selected from chitosan and derivatives thereof, for example: trimethyl chitosan, guanidated chitosan, cationized polysaccharides (for example DEAE dextran) ethyl cationized plant protein or cationized animal protein.
[0078] In various embodiments, the molecular weight of the low molecular weight chitosan or derivative is from about 50 kDa to about 375 kDa, including but not limited to: from about 75 kDa to about 350 kDa, from about 100 kDa to about 300 kDa, from about 150 kDa to about 250 kDa, or from about 180 kDa to about 220 kDa, or including any two of these values and / or any range between any two of these values.
[0079] The key properties to verify the capacity and ability of nucleic acids loaded onto a carrier are surface charge and surface area. Surface charge can be determined directly by zeta potential measurement. The more positive charges on the carrier surface, the higher the potential for capturing negative charges of nucleic acids. On the other hand, nucleic acid capture and release must be controllable and reversible. The carried nucleic acids should be released while being delivered to the target. The pH inside the cell is slightly acidic compared to body fluids. Therefore, for nucleic acid release, a negative surface charge of the carrier in an acidic solution is required. Changes in the zeta potential of the surface of bioactive glass particles can be used to study the bonding of nucleic acids to the surface or to the surface modifiers on the surface of the bioactive glass particles. Changes in the zeta potential indicate that the ligand is bonded to the surface of the bioactive glass particles or to the surface modifier. The zeta potential is a surface charge measurement on the bioactive glass particles and may have an impact on the stability of the particles under various pH conditions. In various embodiments, the zeta potential of the unmodified bioactive glass particles under neutral conditions is about -10 mV to about -40 mV, including: about -10 mV to about 0 mV, -5 mV to about 0 mV, about 0 mV to about 10 mV, 0 mV to about 20 mV, about 0 mV to about 30 mV, about 0 mV to about 40 mV, about -10 mV to about 10 mV, -10 mV to about 20 mV, about -10 mV to about 30 mV, or including any two of these values and / or any range between any two of these values. In various embodiments, the zeta potential of the surface-modified bioactive glass particles under neutral conditions is about 0 mV to about -20 mV, including: about 0 mV to about -5 mV, 0 mV to about -10 mV, about 0 mV to about -15 mV, about 0 mV to about -18 mV, or including any two of these values and / or any range between any two of these values.
[0080] The surface area of the bioactive glass particles can be varied by changing the particle size. The bioactive glass particles of the composition have a narrow particle size distribution and an optimized hydraulic diameter. A narrow particle size range corresponds to a more uniform particle size distribution. The bioactive glass particles have a particle size of less than about 100 μm, for example, less than about 90 μm, less than about 80 μm, less than about 70 μm, less than about 60 μm, less than about 50 μm, less than about 40 μm, less than about 30 μm, less than about 20 μm, less than about 10 μm, or less than about 5 μm. The particle size of the bioactive glass particles can range from about 1 μm to about 100 μm, for example, from about 5 μm to about 90 μm, from about 10 μm to about 80 μm, from about 20 μm to about 70 μm, from about 30 μm to about 60 μm, or from about 40 μm to about 50 μm, or any range including any two of these values and / or any range between any two of these values. In various embodiments, the bioactive glass particles have a particle size ranging from about 1 μm to about 10 μm. In various embodiments, the bioactive glass particles have a particle size ranging from about 1 μm to about 5 μm.
[0081] Bioactive glass particles (with or without surface modification) exhibit an enhanced capacity for nucleic acid loading onto the particle surface. Thus, the nucleic acid loading is much higher and is compatible with several applications. In various embodiments, the concentration of nucleic acid loaded onto the bioactive glass particles ranges from about 5 ng / mg to about 10 μg / mg of the total weight of the carrier composition, including: about 10 ng / mg to about 5 μg / mg, about 100 ng / mg to about 1 μg / mg, about 1 μg / mg to about 10 μg / mg, about 2 μg / mg to about 9 μg / mg, about 3 μg / mg to about 8 μg / mg, about 4 μg / mg to about 7 μg / mg, or about 5 μg / mg to about 6 μg / mg, about 10 ng / mg to about 1 μg / mg, about 20 ng / mg to about 500 ng / mg, about 30 ng / mg to about 100 ng / mg, about 40 ng / mg to about 80 ng / mg, about 50 ng / mg to about 60 ng / mg, or including any two of these values and / or any range between any two of these values. In certain embodiments, the concentration of nucleic acid ranges from about 5 ng / mg to about 10 μg / mg of the total weight of the carrier composition. In certain embodiments, the concentration of nucleic acid ranges from about 100 ng / mg to about 10 μg / mg of the total weight of the vector composition. In certain embodiments, the concentration of nucleic acid ranges from about 5 ng / mg to about 100 ng / mg of the total weight of the vector composition.
[0082] In various embodiments, the ability to capture and release nucleic acids was demonstrated by artificial DNA surrogates of about 200 bp that mimic the length of a typical RNAi fragment. The loading of glass compositions without modifiers may be sufficient for many applications, but surface modifiers can effectively enhance nucleic acid loading capacity under neutral conditions ( Figure 6 , DNA loading). The captured DNA can be quantitatively released in a slightly acidic buffer system with significantly shorter elution times (e.g., 30 minutes or less). This demonstrates the potential of the composition with or without a modifier for nucleic acid transport and delivery to a target.
[0083] Another advantage of the carrier composition is that the glass particles eventually decompose naturally even without being taken up by cells. The decomposition rate of the carrier particles can be tracked by the Ca ion concentration in the solution (Figure 7, Ca trace), which confirms that the glass particles release Ca ions rapidly in the first 24 hours, followed by a slow but steady decomposition over time. The particles will eventually decompose completely naturally, and all components are non-toxic to the environment.
[0084] Although embodiments are described herein with respect to nucleic acids, the bioactive glass particles can be used as carriers for other suitable therapeutic agents or drugs, which can include any compound or substance used to treat or prevent any particular disease or disorder or to modulate a physiological condition in a human or animal subject. In some embodiments, the therapeutic agent can include: an antibiotic, an antifungal agent, a peptide, a protein, a polymer, or a combination thereof. In some embodiments, the bioactive glass particles can include other therapeutic agents in addition to nucleic acids. Suitable nucleic acids and therapeutic agents can be selected from the group consisting of genes, shRNAs, siRNAs, microRNAs, DNA fragments, RNA fragments, plasmids, and combinations thereof.
[0085] method
[0086] Various methods can be used to produce the bioactive glass particles and carrier compositions described herein. For example, the bioactive glass can be first produced by a method comprising: melting a batch of precursor glass at a suitable temperature for a period of time sufficient to melt the batch of precursor glass in a suitable melting apparatus; annealing the glass at a suitable temperature; pouring the molten glass; and cooling the glass to room temperature. Suitable precursor glasses are disclosed herein.
[0087] Depending on the composition, the precursor glass can be melted in a suitable apparatus (e.g., a platinum-covered crucible) at a temperature range of about 1000 to about 1600°C, preferably a temperature range of about 1100 to about 1500°C, more preferably a temperature range of about 1150°C to about 1450°C, for a time sufficient to melt the glass, such as about 60 minutes to about 24 hours, including: about 90 minutes to about 20 hours, about 2 hours to about 18 hours, about 5 hours to about 16 hours, or about 8 hours to about 12 hours, or any range including any two of these values and / or any two of these values. After melting and clarification, the glass can be poured and annealed at a temperature of about 350°C to about 550°C (e.g., about 400°C to about 500°C). The annealed glass can then be poured into a suitable mold, after which the resulting material is cooled naturally at a furnace rate. The glass material thus formed is sized to a suitable particle size using methods known in the art (e.g., milling and grinding).
[0088] Aspects of the technology herein relate to methods for making bioactive glass carriers. In various embodiments, the methods include: processing bioactive glass into fine particles; mixing the fine particles of bioactive glass with a liquid medium to form a solution; optionally modifying the surface of the bioactive glass particles by a surface modifier in the solution, contacting the bioactive glass particles with a nucleic acid compound in the liquid medium to form a mixture; and culturing the mixture under conditions where the nucleic acid compound is non-covalently bound to the bioactive glass particles.
[0089] In certain embodiments, the surface of the bioactive glass particles can be modified by incubating the bioactive glass particles with a surface modifier. For example, the surface modification on the glass particles can be performed by mixing the surface modifier (e.g., a polycationic polymer (e.g., chitosan or polyethyleneimine)) with the glass particles. The admixed compound can then be incubated at an elevated temperature with gentle shaking for a period of time to form a coating. Finally, the coated surface-modified bioactive glass particles are appropriately washed to remove excess polymer and ensure that there is no interference from polymer agglomerated particles. In various embodiments, the bioactive glass particles are incubated with the surface modifier at a temperature of about ambient temperature to about 65°C, including but not limited to: about 20°C to 65°C, about 30°C to 65°C, about 35°C to 65°C, about 40°C to 65°C, or about 50°C to 65°C, or any two of these values and / or any range between any two of these values. In various embodiments, the bioactive glass particles are cultured with the surface modifying agent for a period of about 8 to 24 hours, including but not limited to about 9 hours to about 22 hours, about 10 hours to about 20 hours, about 12 hours to about 18 hours, or about 15 hours to about 16 hours, or any two of these values and / or any range between any two of these values.
[0090] In various embodiments, the method further comprises: contacting the surface-modified bioactive glass particles with the nucleic acid compound in a liquid medium to form a mixture; and incubating the mixture under conditions where the nucleic acid compound is non-covalently bonded to the surface-modified bioactive glass particles. In various embodiments, the incubation of the surface-modified bioactive glass particles with the nucleic acid is performed at room temperature. In various embodiments, the incubation of the bioactive glass particles with the nucleic acid is performed for a period of about 15 minutes to 2 hours, including but not limited to: about 20 minutes to about 100 minutes, about 30 minutes to about 80 minutes, about 40 minutes to about 60 minutes, or about 45 minutes to about 55 minutes, or any two of these values and / or any range between any two of these values. In various embodiments, the coating of the nucleic acid onto the surface of the bioactive glass particles can be performed in a suitable liquid medium (e.g., water, alcohols, or hydrocarbons).
[0091] Another aspect of the present technology relates to a carrier comprising a pH switchable carrier composition described herein. The carrier may include: a drug delivery carrier, a gene delivery carrier, a tissue regeneration carrier, a crop treatment or crop protection, an immunomodulatory carrier, or a gene editing composite carrier. The carrier can be used to deliver the bioactive glass particles and carrier compounds described herein to various types of cells. According to the present technology, any type of cell type that is easy to transfer nucleic acids can be used as a target for transmission. Examples include, but are not limited to: insect cells, animal cells and embryos, fungi, fish, yeast, and plant cells. Stable aqueous suspensions can be used as part of a plant quarantine composition for controlling pests. For example, a stable suspension can be used to protect crops from insects, in which case the nucleic acid is an insecticidal double-stranded RNA. Using interfering ribonucleic acid (RNA) molecules, compositions and suspensions can be used to prevent and / or control insect pest infestations in plants. Compositions and combinations containing interfering RNA molecules for topical application of the present technology, such as in the form of insecticides.
[0092] For delivery to animal cells, the vector composition can be delivered by intravenous, intramuscular or intraperitoneal injection to provide systemic (and possibly local in the case of intramuscular or intraperitoneal injection) anti-inflammatory effects. These effects can be therapeutic and / or preventive. In one embodiment, the particles are locally delivered, for example by inhalation, by spraying (in the form of an aerosol) or by mixing the particles with a gel (e.g., a biocompatible hydrogel), a cream or other aqueous or non-aqueous carrier, and the composition is subcutaneously applied or injected at a later site where surgery is to be performed. The composition may advantageously include other carriers and additives. For delivery to plant cells, the vector composition may be delivered by various methods known in the art, for example by spraying, drip irrigation or irrigation. Aspects of the present invention relate to methods for protecting crops from insect pests, the method comprising delivering a vector composition comprising bioactive glass particles described herein to the crop. In various embodiments, the method comprises protecting the crop from the effects of Hemiptera, Coleoptera, Siphonaptera, Diptera, Lepidoptera, Orthoptera and Diptera. In such methods, the nucleic acid in the composition may include insecticidal double-stranded ribonucleic acid. Another aspect of the technology herein relates to a method for down-regulating the expression of a target gene in a pest species to prevent and / or control pest infestation, comprising contacting the pest species with an effective amount of a vector composition as described herein, the vector composition comprising at least one interfering ribonucleic acid (RNA). Suitable interfering RNAs are known in the art.
[0093] It will be apparent to those skilled in the art that various modifications and variations may be made without departing from the spirit or scope of the claimed subject matter. Therefore, the claimed subject matter is not to be restricted except by the appended claims and their equivalents.
[0094] Example
[0095] Various embodiments will be further illustrated by the following examples, which are not intended to limit the present disclosure in any way.
[0096] Example 1: Preparation of Bioactive Glass Composition
[0097] Exemplary bioactive glasses described herein are silicate or borate glasses comprising a base composition comprising the constituent components listed in Table 1, in weight percent of oxides.
[0098] Table 1
[0099]
[0100] Glass was made in a platinum crucible using the raw material batches listed in Table 1. Each crucible containing the formulated raw material batch was placed in a preheated furnace and melted at 1100-1500° C. for 16 hours. The glass was clarified to produce a molten precursor glass, which was then cast into 7×11 inch block precursor glasses and annealed at a temperature range of 400-500° C., as recorded in the table. The glass was crushed using air jets and ball milling. Figure 2 Particle size distribution of BAG#8 (876EKH) after air jet and ball milling is shown. Additional ball milling can reduce the D50 from 2.6 μm (after air jet milling) to 0.9 μm.
[0101] The characteristics of the crystalline phases and / or the crystal size of the crystalline phases of the crystalline phase ensemble are determined by X-ray diffraction (XRD) analysis techniques known to those skilled in the art, using such commercially available instruments as a Bruker D4 Endeavor diffractometer manufactured by Bruker Corporation, Massachusetts, United States. The spectrum is typically obtained from 10 to 40 degrees 2θ. The glasses were subjected to XRD analysis, and Table 2 shows the results obtained. Figure 1 XRD patterns of glass powders after immersion in 0.02M KH2PO4 solution for 14 days are shown. The formation of brushite (CaHPO4·2H2O) indicates the excellent biocompatibility of these glass compositions. Higher crystallinity was observed in UV and UY (BAG#5 and BAG#6) samples compared to HFK or EKH (BAG#7 and BAG#8), indicating better bioactivity of the formers.
[0102] Table 2
[0103] atom% BAG only PEI Chitosan, shrimp shell Chitosan, low MW Si 19.55 11.51 10.86 6.02 P 3.04 1.94 – – Na 0.48 – – 0.25 K 0.71 – 0.29 – Ca 6.41 4.20 1.07 0.67 O 69.80 45.69 48.43 35.62 C – 36.66 39.35 57.45
[0104] Example 2: Surface modification and characterization of bioactive glass compositions
[0105] 100 mg of bioactive glass (BAG) prepared according to the process of Example 1 was added to a 1.5 mL microtube, and 1 mL of water and the mixture were vortexed and aliquoted. Three sets of PEI (polyethyleneimine, AL-408727-100ML, branched, ~MW 25,000) solutions were prepared. 100 mg of each PEI solution was transferred to a 1.5 mL microtube, to which 0.8 mL of water was added. The resulting solution was warmed in a 65°C dry bath for 10 minutes. Similarly, three sets of low MW chitosan (AL-448869-50G, low MW, alkaline deacetylation pretreatment) solutions were prepared. 10 mg of each chitosan powder was transferred to a 1.5 mL microtube, to which 0.8 mL of 0.3% acetic acid (30 μL HOAc / 10 mL water) was added. The solution was vortexed for 1 minute. Finally, three shrimp shell chitosan (AL-417963-25G, from shrimp shell, alkali deacetylation pretreatment) solutions were prepared, 10 mg of each chitosan particle was transferred to a 1.5 mL microtube, to which 0.8 mL of 0.3% acetic acid (30 μL HOAc / 10 mL water) was added. The solution was vortexed for 1 minute.
[0106] 200 μL of BAG well-suspended solution was combined with 800 μL of water, prepared PEI and prepared low MW and shrimp chitosan solution and cultured on a 65°C dry bath for 20 hours. The mixture was purified by ultracentrifugation at 15000 rpm for 5 minutes. The supernatant was discarded, and the residue was washed with 400 μL of water and centrifuged at 15000 rpm for 5 minutes. The purification step was repeated twice.
[0107] The surface modified BAG particle solution was resuspended in 800 μL of water. Two aliquots were collected, one for analysis and one for DNA binding assessment. The analysis set was maintained at room temperature without solution until analysis.
[0108] The chemical composition, approximate particle size and morphology of the bioactive glasses with / without modifiers were examined by scanning electron microscopy (SEM, JEOL JSM-6500F, EDS detector). Figure 3 SEM images are shown. Particle size measurements were also checked by dynamic light scattering based on Brownian motion (Malvern Zetasizer Nano ZS) and by estimation of Z-average particle size ( Figure 4 ). It was observed that the size of the surface-modified glass particles was slightly larger than that of the original particles, and the modifiers on the surface of the glass particles were verified by semi-quantitative analysis using SEM-EDX.
[0109] Surface charge measurements were checked by measuring zeta potential (Malvern Zetasizer Nano ZS) at various pH values. pH solutions were prepared using 0.01M KCl adjusted to pH levels with dilute HCl or KOH. Samples were ultrasonically mixed, and then 35 μL of sample was added to 950mL of pH solution and mixed. It was put into a Malvern disposable folding capillary unit for testing. The RI value was 1.540. Fig. 5 shows the surface charge of the zeta potential of bioactive glass at pH 4, pH 8, and pH 12 (unmodified (5A) and coated with chitosan (5B) in H2O). In the accompanying drawings, RT represents pre-soaking in water at room temperature, and SS represents chitosan derived from shrimp shells. It was observed that for unmodified BAG samples, for BAG#7, zeta potential increased with increasing pH, while for all other tested BAG samples, it decreased. For BAG samples modified with shrimp shell chitosan, similar trends were observed, but the changes were not as obvious as for unmodified particles. The observation of surface charge by zeta potential can partially answer the binding-release mechanism of nucleic acids from the BAG surface. Exposed cations from bioactive glass particles also contribute to the nucleic acid binding-release phenomenon, especially when the change charge presents a negative charge and the carrier composition is still able to capture the negative charge of the nucleic acid.
[0110] Example 3: DNA Modification of Bioactive Glass Compositions
[0111] The BAG concentration of the aliquot before surface modification was 20 mg / 300 μL H 2 O. The BAG concentration after surface modification was 10 mg / 300 μL, and for each preparation below, the DNA concentration was 100 ng / 10 μL.
[0112] DNA solution is added to each BAG solution and vortexed to mix well, then cultured for 30 minutes at room temperature in a microtube equipped with a gentle oscillator (300rpm). Samples were centrifuged at 14000rpm for 5 minutes to obtain 10 μL supernatant samples for DNA quantitative analysis in Qubit-HS-dsDNA assay. If the Qubit readings indicate that the BAG surface is not saturated with DNA, 100 ng / 10 μL DNA is added again, and the solution is vortexed and cultured again for 30 minutes. This DNA addition and quantitative analysis process is repeated several times to evaluate DNA loading.
[0113] Example 4: DNA Elution from Bioactive Glass Compositions
[0114] Surface modified or unmodified BAGs were centrifuged to remove all supernatants and leave DNA quantitative analysis. 300 μL of 50 mM phosphate buffer (170 mM ionic strength) at pH 5.4 was added to the BAG solution for elution. The solution was resuspended by vortex stirring and incubated at room temperature for 30 minutes using a gentle shaker (300 rpm). The solution was centrifuged at 14000 rpm for 5 minutes to remove all supernatants and used for DNA quantitative analysis (10 μL sample was tested) in the Qubit-HS-dsDNA test.
[0115] DNA modification and DNA elution results are shown in Figure 6 As shown, it confirms the potential of BAG compositions (with or without surface modifiers) for nucleic acid delivery and delivery to targets. Specifically, it was observed that surface modifiers can enhance the ability of nucleic acid loading efficiency under neutral conditions, and the captured DNA can be quantitatively released in a slightly acidic buffer system within an elution time of 30 minutes or less.
[0116] Example 5: Solubility Test Process
[0117] 20mg BAG (#5, #6#7 and #8) and 0.2mL water or 0.2mL phosphate buffer were added to 1.5mL microtubes and vortexed to mix. The mixture was heated on a 35°C dry bath for time tracking. The solution was vortexed to mix before centrifugation. The mixture was centrifuged at 14000rpm for 5 minutes. After centrifugation, the supernatant was removed from one group and replaced with fresh water or buffer after inspection. For another group, 15μL was sampled for pH testing and refilled with 15μL of fresh water or buffer after inspection.
[0118] Example 6: Calcium Unit Test
[0119] By Merck Calcium unit test, calcium concentration was quantified by UV detection at different time points. 400 μL of buffer solution was equally divided from the unit into 10 microtubes, and 100 μL of reagent Ca-1K and 100 μL of BAG sample were added to each microtube. The pH value was about 7 for standards and samples. After waiting for 3 minutes, 50 μL of reagent Ca-2K was added to each microtube. The change in calcium concentration within 1 hour was measured using a NanoDrop Microvolume spectrophotometer (2 μL sample). The results are shown in Figure 7, which confirms that the glass particles release Ca ions rapidly in the first 24 hours, and then slowly but steadily decompose over time.
[0120] Example 7: RNA Modification of Bioactive Glass Compositions
[0121] The procedure of Example 3 was repeated except that RNA was used instead of DNA. RNA was loaded onto unmodified and surface modified BAG particles and the RNA modification and RNA elution results were studied.
[0122] All of the above examples were performed using RNA instead of DNA.
[0123] Unless otherwise expressly stated, any method described herein should not be construed as requiring that its steps be performed in a specific order, or requiring that any device have a particular orientation. Therefore, if a method claim does not actually recite the order in which its steps are to be followed, or if any device claim does not actually recite the order or orientation of the components, or if there is no other specific statement in the claims or specification that the steps are limited to a specific order, or if a specific order or orientation of the device components is not recited, then no order or orientation should be inferred in any respect. The same applies to any possible non-expressly stated basis for interpretation, including: logic regarding the setting of steps, operational flow, component order, or component orientation; general meaning derived from grammatical structure or punctuation; and the number or type of embodiments described in the specification.
[0124] All disclosed ranges are understood to include and provide support for claims stating any and all subranges or any and all individual values contained by each range. For example, the stated range of 1 to 10 should be considered to include and provide support for any and all subranges or individual values between and / or including a minimum value of 1 and a maximum value of 10; that is, all subranges start at a minimum value of 1 or greater and end at a maximum value of 10 or less (e.g., 5.5 to 10, 2.34 to 3.56, etc.), or any value from 1 to 10 (e.g., 3, 5.8, 9.9994, etc.). Any listed range can be easily identified as fully describing and allowing the same range to be decomposed into at least half, one-third, one-quarter, one-fifth, one-tenth, etc. As a non-limiting example, each range discussed herein can be easily decomposed into a lower third, a middle third, and an upper third, etc. It will also be understood by those skilled in the art that all languages, such as "up to", "at least", "greater than", "less than", etc., include the stated numbers and relate to ranges that can be subsequently decomposed into subranges discussed above. Finally, as will be understood by those skilled in the art, a range includes each individual member. Thus, for example, a group having 1-3 layers refers to groups having 1, 2, or 3 layers. Similarly, a group having 1-5 layers refers to groups having 1, 2, 3, 4, or 5 layers, and so on.
[0125] The drawings should be interpreted as showing one or more embodiments drawn to scale and / or one or more embodiments not drawn to scale. This means that the drawings may be interpreted, for example, as showing the following: (a) everything is drawn to scale; (b) nothing is drawn to scale; or (c) one or more features are drawn to scale and one or more features are not drawn to scale. Thus, the drawings may be used to provide support for the size, proportions, and / or other dimensions of any illustrated feature described individually or relative to each other. Furthermore, all such sizes, proportions, and / or other dimensions are understood to vary from 0-100% in either direction, thereby providing support for claims stating such values or any and all ranges or sub-ranges that may be formed from such values.
[0126] Terms stated in the claims should be determined by reference to relevant entries in widely used general dictionaries and / or dictionaries of relevant technology, meanings commonly understood by persons skilled in the art, etc., and it is understood that the terms of the claims have the broadest meaning given by any one or combination of these sources (e.g., two or more relevant dictionary entries should be combined to provide the broadest meaning of the combination of the entries, etc.), subject only to the following exceptions: (a) if a term is used in a manner broader than its ordinary and customary meaning, the term should be given its ordinary and customary meaning plus an additional extended meaning, or (b) if a term has been expressly defined to have a different meaning by stating that the term is as used in this document, or similar language (e.g., "this term means," "this term is defined as," "for the purposes of this disclosure, this term should mean," etc.). Reference to specific examples, use of "i.e.," use of the phrase "the present technology," etc. is not intended to refer to exception (b) or otherwise limit the scope of the claim terms. Except where exception (b) applies, nothing contained in this document shall be construed as a waiver of a claim or a denial of the scope of a claim.
[0127] Unless otherwise defined, all terms used herein (including technical terms and scientific terms) have the same meanings as commonly understood by those of ordinary skill in the art to which the present technology belongs. It will also be understood that terms (such as those defined in commonly used dictionaries) should be understood to be consistent with their definitions in the present application and related fields, and unless otherwise defined herein, should not be understood as idealized or fully formalized meanings. Although not clearly defined below, such terms should be interpreted according to their common meanings.
[0128] In addition, where features or aspects of the disclosure are described in terms of Markush groups, those skilled in the art will recognize that the disclosure is also thereby described in terms of any individual member or subgroup of members of the Markush group.
[0129] Unless the context clearly states otherwise, it is intended that the various features of the present technology described herein can be used in any combination. In addition, in some embodiments, the present disclosure also contemplates that any feature or combination of features described herein can be excluded or omitted. Explanatory note, if the specification states that a consortium includes components A, B, and C, it is specifically intended that any or any combination of A, B, or C can be omitted or abandoned individually or in any combination thereof.
[0130] Unless expressly stated otherwise, all specific embodiments, features and terms are intended to include both the stated embodiment, feature or term and its biological equivalents.
[0131] All patents, patent applications, provisional applications, and publications referred to or cited herein are hereby incorporated by reference in their entirety, including all figures and tables, to the extent they are not inconsistent with the teachings of this specification.
Claims
1. A pH switchable carrier composition comprising: A plurality of bioactive glass particles, wherein Each bioactive glass particle is at least partially coated with a surface modifier, the surface modifier comprising a polycationic compound selected from the group consisting of polyethyleneimine, shrimp chitosan, low molecular weight chitosan, and derivatives thereof; Among them, the bioactive glass particles with or without surface modifiers are capable of binding to nucleic acid compounds upon contact within a pH range of about 7 to about 11, and exhibit controlled release of the nucleic acid compounds within a pH range of about 5 to about 6.
2. The pH switchable carrier composition according to claim 1, wherein The bioactive glass particles primarily comprise, in weight percent of oxides, about 30% to about 75% SiO2, about 2% to about 40% CaO, and about 3% to about 15% P2O5.
3. The pH switchable carrier composition according to claim 1, wherein The bioactive glass particles primarily comprise, in weight percent of oxides, about 30% to about 70% B2O3, about 5% to about 25% CaO, and about 1% to about 10% P2O5.
4. The pH switchable carrier composition according to claim 2, wherein The bioactive glass particles further comprise, in weight percent of oxides: about 0% to about 5% B2O3; about 0% to about 5% Al2O3; about 0% to about 20% MgO; about 0% to about 10% ZrO2; about 0% to about 5% F; and From about 0% to about 30% R2O, wherein the R2O includes from about 0% to about 10% K2O and from about 0% to about 30% Na2O.
5. The pH switchable carrier composition according to claim 3, wherein The bioactive glass particles further comprise, in weight percent of oxides: about 0% to about 5% SiO2; about 0% to about 15% Al2O3; about 0% to about 10% MgO; about 0% to about 10% ZrO2; about 0% to about 5% F; and From about 0% to about 20% R2O, wherein the R2O includes from about 0% to about 20% K2O and from about 0% to about 10% Na2O.
6. The pH switchable carrier composition according to any one of claims 1 to 5, wherein The bioactive glass particles include calcium phosphate glass.
7. The pH switchable carrier composition according to claim 1, wherein The molecular weight of low molecular weight chitosan or derivative is about 50 kDa to about 375 kDa.
8. The pH switchable carrier composition according to any one of claims 1 to 5, wherein The nucleic acid compound is selected from the group consisting of a ribonucleic acid compound, a deoxyribonucleic acid compound, or a derivative thereof.
9. The pH switchable carrier compound according to any one of claims 1 to 5, wherein The bioactive glass particles have a particle size of about 1 μm to about 10 μm.
10. The pH switchable carrier compound according to claim 9, wherein The bioactive glass particles have a particle size of about 1 μm to about 5 μm.
11. The pH switchable carrier compound according to any one of claims 1 to 5, wherein The zeta potential of unmodified bioactive glass particles under neutral conditions is about -10 mV to about -40 mV.
12. The pH switchable carrier compound according to any one of claims 1 to 5, wherein The zeta potential of the surface modified bioactive glass particles under neutral conditions is from about 0 mV to about -20 mV.
13. The pH switchable carrier compound according to any one of claims 1 to 5, wherein The concentration of nucleic acid ranges from about 5 ng / mg to about 10 μg / mg of the total weight of the vector composition.
14. A bioactive glass particle at least partially coated with a surface modifier, the surface modifier comprising a polycationic compound selected from the group consisting of polyethyleneimine, shrimp chitosan, low molecular weight chitosan, and derivatives thereof; in, The bioactive glass particles having a surface modifier are capable of binding to a nucleic acid compound upon contact within a pH range of about 7 to about 11 and exhibiting controlled release of the nucleic acid compound within a pH range of about 5 to about 6; and Wherein, in terms of weight % of oxides, the bioactive glass particles mainly comprise: (a) from about 30% to about 75% SiO2, from about 2% to about 40% CaO, and from about 3% to about 15% P2O5; or (b) about 30% to about 70% B2O3, about 5% to about 25% CaO, and about 1% to about 10% P2O5.
15. A method for manufacturing a bioactive glass carrier, comprising: Processing bioactive glass into fine particles; Fine particles of bioactive glass are mixed with a liquid medium to form a solution; The surface of the bioactive glass particles is modified in a solution with a surface modifier, wherein the surface modifier comprises a polycationic compound selected from the group consisting of polyethyleneimine, shrimp chitosan, low molecular weight chitosan, and derivatives thereof, contacting the bioactive glass particles with the nucleic acid compound in a liquid medium to form a mixture; and The mixture is incubated under conditions where the nucleic acid compound is non-covalently bound to the bioactive glass particles.
16. The method of claim 15, comprising modifying the surface of the bioactive glass particles by culturing the bioactive glass particles with a surface modifying agent.
17. The method according to claim 15 or 16, wherein: Surface modifiers include polycationic compounds.
18. The method according to claim 15 or 16, wherein: Incubation of the bioactive glass particles with the surface modifying agent is performed at a temperature between about ambient temperature and about 65°C.
19. The method according to claim 15 or 16, wherein: The bioactive glass particles are incubated with the surface modifying agent for a period of about 8 to 24 hours.
20. The method of claim 15, further comprising: contacting the surface-modified bioactive glass particles with a nucleic acid compound in a liquid medium to form a mixture; as well as The mixture is incubated under conditions where the nucleic acid compound non-covalently binds to the surface-modified bioactive glass particles.
21. The method of claim 20, wherein: Incubation of the surface-modified bioactive glass particles with nucleic acids was performed at room temperature.
22. The method of claim 20 or 21, wherein: The surface modified bioactive glass particles are incubated with the nucleic acid for a period of about 15 minutes to 2 hours.
23. The method of claim 15 or 16, wherein: The liquid medium is selected from the group consisting of water, alcohols or hydrocarbons.
24. The method of claim 15 or 16, wherein: The bioactive glass particles primarily comprise, in weight percent of oxides, about 30% to about 75% SiO2, about 2% to about 40% CaO, and about 3% to about 15% P2O5.
25. The method of claim 15 or 16, wherein: The bioactive glass particles primarily comprise, in weight percent of oxides, about 30% to about 70% B2O3, about 5% to about 25% CaO, and about 1% to about 10% P2O5.
26. The method of claim 24, wherein the bioactive glass particles further comprise, in weight percent of oxides: about 0% to about 5% B2O3; about 0% to about 5% Al2O3; about 0% to about 20% MgO; about 0% to about 10% ZrO2; about 0% to about 5% F; and From about 0% to about 30% R2O, wherein R2O includes about 0% to about 10% K2O and about 0% to about 30% Na2O.
27. The method of claim 25, wherein the bioactive glass particles further comprise, in weight percent of oxides: about 0% to about 5% SiO2; about 0% to about 15% Al2O3; about 0% to about 10% MgO; about 0% to about 10% ZrO2; about 0% to about 5% F; and From about 0% to about 20% R2O, wherein R2O includes about 0% to about 20% K2O and about 0% to about 10% Na2O.
28. A carrier comprising the pH-switchable carrier composition according to any one of claims 1-5.
29. The carrier of claim 28, wherein The carriers include: drug delivery carriers, gene delivery carriers, tissue regeneration carriers, crop treatment or crop protection, immunomodulatory carriers or gene editing complex carriers.